A negative electrode sheet with coating, preparation method thereof and lithium ion battery
By applying a porous coating to the negative electrode sheet of a lithium-ion battery and using a composite material of polymer and inorganic ceramic particles, the problem of capacity fading caused by expansion and contraction of the negative electrode material is solved, and the cycle performance and energy density of the battery are improved.
Patent Information
- Application Number
- CN202211398093.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-11-09
AI Technical Summary
The irreversible capacity attenuation of the silicon-carbon anode material in lithium-ion batteries due to expansion and contraction during the cycle affects the energy density and life of the battery.
A negative electrode sheet with a porous coating is used. The coating is composed of a polymer and inorganic ceramic particle composite material. Through a combination of pore control solution and solvents with different boiling points, a porous structure is formed to restrain the expansion and contraction of the negative electrode material and improve Liquid retention capacity.
It effectively prevents the negative electrode material from falling off due to expansion and contraction, improves battery cycle performance, and enhances battery energy density and lifespan.
Smart Images

Figure BDA0003934515260000121 
Figure HDA0003934515270000011
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a negative electrode plate with a coating, a preparation method thereof, and a lithium ion battery. Background Art
[0002] In recent years, national policies have strongly encouraged the development of the new energy industry, and the capital market has shown unprecedented enthusiasm for investment in the new energy industry. In addition, the traditional automobile industry has been undergoing transformation, leading to intensified competition in the industry. Whoever can occupy the technological commanding heights can occupy the market.
[0003] Battery safety issues caused by the pursuit of high energy density and long life of electric vehicles are becoming more and more frequent, and improving battery safety is an urgent problem to be solved. In the pursuit of high energy density, a large number of silicon-carbon negative electrode materials are being developed and used. However, Si materials have defects such as very large volume changes (300%), mechanical degradation (crushing) and chemical aging during the cycle, resulting in insufficient number of charge / discharge cycles that can be achieved by the battery, which is still an obstacle to the use of Si / C materials. Summary of the invention
[0004] In view of this, the technical problem to be solved by the present invention is to provide a negative electrode plate with a coating, a preparation method thereof, and a lithium-ion battery. The negative electrode plate with a coating provided by the present invention can exert a certain restraint on the expansion and contraction of the negative electrode material, thereby preventing the material from falling off the plate due to expansion and contraction, resulting in irreversible capacity decay.
[0005] The present invention provides a negative electrode plate with a coating, comprising a current collector, a negative electrode active material layer and a porous coating which are compounded in sequence, wherein the porous coating comprises a composite material of a high molecular polymer and inorganic ceramic particles.
[0006] Preferably, the high molecular polymer is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, polypyrrole, polythiophene, polyethylene, polypropylene, polystyrene, polyacrylamide, ethylene-propylene-diene copolymer resin, styrene-butadiene rubber, polybutadiene, fluororubber, polyethylene oxide, polyvinyl pyrrolidone, acrylic resin, epoxy resin, polyvinyl alcohol, carboxypropyl cellulose, ethyl cellulose, sodium carboxymethyl cellulose, styrene-butadiene latex and other high molecular materials.
[0007] Preferably, the inorganic ceramic particles are selected from one or more of aluminum oxide, silicon dioxide, boehmite, titanium dioxide, silicon dioxide, zirconium oxide, barium titanate, lithium niobate, yttrium-doped zirconium oxide, gadolinium-doped cerium oxide, montmorillonite, aluminosilicate, lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium lanthanum zirconium niobium oxide, lithium aluminum titanium phosphate, lithium germanium titanium phosphate, and lithium lanthanum titanate;
[0008] The particle size of the inorganic ceramic particles is 100 nm to 20 μm, preferably 200 nm to 2.5 μm.
[0009] Preferably, the mass ratio of the porous coating polymer to the inorganic ceramic particles is 1:(0-50).
[0010] Preferably, the porosity of the porous coating is 20% to 70%;
[0011] The total volume of the porous coating is no more than 80% of the total volume of the negative electrode sheet based on the total volume of the negative electrode sheet;
[0012] The thickness of the negative electrode active material layer is greater than or equal to the thickness of the porous coating layer;
[0013] The thickness of the porous coating is 2 to 50 μm, and more preferably the thickness of the coating is 8 to 12 μm;
[0014] The thickness of the negative electrode plate is 20 μm to 300 μm.
[0015] The present invention also provides a method for preparing the above-mentioned negative electrode sheet, comprising the following steps:
[0016] A) coating the negative electrode slurry on the surface of the current collector to obtain a negative electrode active material layer;
[0017] B) dispersing the high molecular polymer and the inorganic ceramic particles in a pore control solution to obtain a coating slurry; the porosity control solution is a mixed solution composed of two or more solvents with different boiling points;
[0018] C) coating the coating slurry on the surface of the negative electrode active material layer to obtain a negative electrode sheet.
[0019] Preferably, the porosity controlling solution is selected from a mixed solution of deionized water and acetone, a mixed solution of acetone and dimethyl carbonate, a mixed solution of N,N-dimethylformamide and dimethyl carbonate, or a mixed solution of N,N-dimethylacetamide and dimethyl carbonate, and the volume ratio is: (1-10):1.
[0020] Preferably, the coating slurry has a solid content of 7 wt% to 50 wt%.
[0021] The present invention also provides a lithium-ion battery, comprising the above-mentioned negative electrode plate.
[0022] Compared with the prior art, the present invention provides a negative electrode plate with a coating, comprising a current collector, a negative electrode active material layer and a porous coating which are compounded in sequence, wherein the porous coating comprises a composite material of a high molecular polymer and inorganic ceramic particles. The coating constructed by the negative electrode plate provided by the present invention has a porous structure, which, on the one hand, has a certain restraint on the expansion and contraction of the negative electrode material, preventing the material from falling off the plate due to expansion and contraction, resulting in irreversible capacity decay; on the other hand, it makes the negative electrode surface more capable of retaining liquid, improves the phenomenon of increased DC internal resistance caused by adding the coating, and effectively improves the cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of the cross-sectional structure of a negative electrode plate with a coating provided by the present invention. DETAILED DESCRIPTION
[0024] The present invention provides a negative electrode plate with a coating, comprising a current collector, a negative electrode active material layer and a porous coating which are compounded in sequence, wherein the porous coating comprises a composite material of a high molecular polymer and inorganic ceramic particles.
[0025] See also Figure 1 , Figure 1 A schematic diagram of the cross-sectional structure of a negative electrode plate with a coating provided by the present invention. Figure 1 In the figure, 1 is a current collector, 2 is a negative electrode active material layer, and 3 is a porous coating. The negative electrode active material layer and the porous coating are arranged on both sides of the current collector and are arranged symmetrically. The porous coating is arranged on the negative electrode active material layer away from the current collector.
[0026] Specifically, the negative electrode plate with coating provided by the present invention includes a current collector, and the present invention has no special restrictions on the specific type of the current collector, and any type of current collector known to those skilled in the art can be used. In the present invention, the current collector is selected from copper foil or composite copper foil.
[0027] The negative electrode plate with coating provided by the present invention also includes a negative electrode active material layer, wherein the negative electrode active material in the negative electrode active material layer is selected from one or more of silicon-carbon negative electrode, graphite negative electrode, metal oxide negative electrode and hard carbon.
[0028] The negative electrode plate with coating provided by the present invention further comprises a porous coating, wherein the porous coating comprises a composite material of a high molecular polymer and inorganic ceramic particles.
[0029] The high molecular polymer is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, polypyrrole, polythiophene, polyethylene, polypropylene, polystyrene, polyacrylamide, ethylene-propylene-diene copolymer resin, styrene-butadiene rubber, polybutadiene, fluororubber, polyethylene oxide, polyvinyl pyrrolidone, acrylic resin, epoxy resin, polyvinyl alcohol, carboxypropyl cellulose, ethyl cellulose, sodium carboxymethyl cellulose, styrene-butadiene latex and other high molecular materials.
[0030] The inorganic ceramic particles are selected from one or more of aluminum oxide, silicon dioxide, boehmite, titanium dioxide, silicon dioxide, zirconium oxide, barium titanate, lithium niobate, yttrium-doped zirconium oxide, gadolinium-doped cerium oxide, montmorillonite, aluminosilicate, lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium lanthanum zirconium niobium oxide, lithium aluminum titanium phosphate, lithium germanium titanium phosphate, and lithium lanthanum titanate;
[0031] The particle size of the inorganic ceramic particles is 100 nm to 20 μm, preferably 100 nm, 500 nm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, or any value between 100 nm and 20 μm, and more preferably any value between 200 nm and 2.5 μm.
[0032] In the present invention, the mass ratio of the porous coating polymer to the inorganic ceramic particles is 1:(0-50), preferably 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45, 1:50, or any value between 1:(0-50).
[0033] The porosity of the porous coating is 20% to 70%, preferably 20%, 30%, 40%, 50%, 60%, 70%, or any value between 20% and 70%;
[0034] The total volume of the porous coating is no more than 80% of the total volume of the negative electrode sheet based on the total volume of the negative electrode sheet;
[0035] The thickness of the negative electrode active material layer is greater than or equal to the thickness of the porous coating layer;
[0036] The thickness of the porous coating is 2 to 50 μm, preferably 2, 5, 10, 20, 30, 40, 50, or any value between 2 and 50 μm, and more preferably the thickness of the coating is any value between 8 and 12 μm;
[0037] The thickness of the negative electrode plate is 20 μm to 300 μm, preferably 20, 50, 100, 150, 200, 250, 300, or any value between 20 μm and 300 μm.
[0038] The present invention also provides a method for preparing the above-mentioned negative electrode sheet, comprising the following steps:
[0039] A) coating the negative electrode slurry on the surface of the current collector to obtain a negative electrode active material layer;
[0040] B) dispersing the high molecular polymer and the inorganic ceramic particles in a pore control solution to obtain a coating slurry; the porosity control solution is a mixed solution composed of two or more solvents with different boiling points;
[0041] C) coating the coating slurry on the surface of the negative electrode active material layer to obtain a negative electrode sheet.
[0042] The present invention first prepares negative electrode slurry. Specifically, the negative electrode slurry is prepared from negative electrode active material, a binder and a conductive agent.
[0043] Wherein, the negative electrode active material is preferably a silicon-carbon material;
[0044] The binder is preferably CMC and SBR;
[0045] The conductive agent is preferably SP;
[0046] The mass ratio of the negative electrode active material, the binder and the conductive agent is 96.5:2.5:1.
[0047] The present invention has no particular limitation on the specific method for preparing the negative electrode active material layer, and any method known to those skilled in the art may be used.
[0048] Specifically, the negative electrode active material, the binder and the conductive agent are dispersed in a solvent to obtain a negative electrode slurry, and then the negative electrode slurry is coated on the surface of the current collector and dried to obtain a negative electrode active material layer. The solvent is selected from water.
[0049] Then, the high molecular polymer and the inorganic ceramic particles are dispersed in the pore control solution to obtain a coating slurry.
[0050] Wherein, the porosity controlling solution is selected from a mixed solution of deionized water and acetone, a mixed solution of acetone and dimethyl carbonate, a mixed solution of N,N-dimethylformamide and dimethyl carbonate, or a mixed solution of N,N-dimethylacetamide and dimethyl carbonate.
[0051] In some specific embodiments of the present invention, the porosity controlling solution is a mixed solution of N,N-dimethylformamide and acetone, wherein the volume ratio of N,N-dimethylformamide to acetone is 2-5:5-8, preferably 2:8, 5:5, or any value between 2-5:5-8.
[0052] The high molecular polymer and the inorganic ceramic particles are dispersed in the pore control solution, and the high molecular polymer is fully dissolved and mixed uniformly to form a coating slurry, wherein the coating slurry has a solid content of 22 wt%.
[0053] Next, the coating slurry is applied to the surface of the negative electrode active material layer and dried to obtain a porous coating layer.
[0054] Finally, trimming, cutting and stripping are performed to obtain the negative electrode sheet with coating.
[0055] The porous coating is constructed by adjusting the porosity of the coating by a pore control solution or adjusting the ratio of the polymer and the inorganic ceramic particles or adjusting the particle size of the inorganic ceramic particles. The present invention selects solvents with different boiling points and utilizes the different volatilization temperatures and volatilization rates of the two solvents during the drying process to leave pore channels inside the coating to form pores. In addition, the size of the inorganic ceramic particles determines the size of the internal pores during the stacking process. Large particles stacking result in large pores, while small particles stacking result in small pores.
[0056] The present invention also provides a lithium-ion battery, comprising the above-mentioned porous negative electrode sheet. Specifically, the lithium-ion battery provided by the present invention comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The present invention has no special restrictions on the selection of specific types of positive electrode sheets, separators and electrolytes and the preparation methods, and the types and methods known to those skilled in the art can be used.
[0057] The coating constructed on the negative electrode plate provided by the present invention has a porous structure. On the one hand, it has a certain restraint on the expansion and contraction of the negative electrode material, preventing the material from falling off the plate due to expansion and contraction and causing irreversible capacity decay; on the other hand, it makes the negative electrode surface more capable of retaining liquid, improves the phenomenon of increased DC internal resistance caused by adding the coating, and effectively improves the cycle performance of the battery.
[0058] In order to further understand the present invention, the negative electrode plate with coating, the preparation method thereof and the lithium ion battery provided by the present invention are described below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0059] The silicon-carbon negative electrode material is obtained by physically mixing nano-silicon and graphite carbon material in a mass ratio of 3:7.
[0060] Embodiment 1:
[0061] A lithium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator spaced between the positive electrode sheet and the negative electrode sheet, and an electrolyte; wherein a porous coating is coated on the negative electrode sheet.
[0062] (1) Preparation of positive electrode
[0063] The positive electrode slurry is prepared by uniformly mixing NCM811 positive electrode active material, conductive agent superconducting carbon and carbon tube, and binder polyvinylidene fluoride in a mass ratio of 96:2:0.5:1.5, coating the positive electrode slurry on one surface of the current collector aluminum foil, drying and rolling at 120°C, and then coating and drying the positive electrode slurry on the other side of the aluminum foil according to the above method, and then cold pressing the prepared aluminum foil with the positive electrode active material layer on both sides; trimming, cutting, and striping are performed, and after stripping, a lithium-ion battery positive electrode sheet is prepared.
[0064] (2) Preparation of negative electrode sheet
[0065] Preparation of negative electrode active material layer: silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber are prepared into negative electrode slurry in a mass ratio of 96:1.5:1.0:1.5, coated on the current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with negative electrode active material layer on both sides is cold pressed;
[0066] Preparation of porous coating:
[0067] Add polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 200 nm in a mass ratio of 2:3 to N,N-dimethylformamide and acetone in an organic solvent volume ratio of 2:8, and wait until the polyvinylidene fluoride is fully dissolved and mixed evenly to form a coating slurry with a solid content of 25%. The coating slurry is coated on the surface of the prepared negative electrode sheet, and dried at 100° C. with forced air to obtain a functional coating with a thickness of 12 μm;
[0068] The negative electrode sheets for lithium-ion batteries are cut into pieces, sliced and stripped to form negative electrode sheets with a total thickness of 124 μm.
[0069] (3) Diaphragm: A polyethylene porous film with a thickness of 9 μm was selected as the diaphragm.
[0070] (4) Preparation of electrolyte:
[0071] Lithium hexafluorophosphate is dissolved in a mixed solvent of ethylene carbonate, ethyl methyl carbonate and diethyl carbonate (the mass ratio of the three is 3:5:2) to obtain an electrolyte.
[0072] (5) Preparation of batteries:
[0073] The positive electrode sheet, separator and negative electrode sheet are wound into a battery cell with a capacity of about 5Ah. The separator is located between the adjacent positive and negative electrode sheets, the positive electrode is spot welded out with an aluminum tab, and the negative electrode is spot welded out with a nickel tab; the battery cell is then placed in an aluminum-plastic packaging bag, baked, and injected with the above electrolyte, and finally made into a polymer lithium-ion battery through packaging, formation, capacity division and other processes.
[0074] Example 2
[0075] The difference from Example 1 is the preparation of the negative electrode sheet.
[0076] Preparation of negative electrode:
[0077] Preparation of negative electrode active material layer: silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber are prepared into negative electrode slurry in a mass ratio of 96:1.5:1.0:1.5, coated on the current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with negative electrode active material layer on both sides is cold pressed;
[0078] Preparation of porous coating:
[0079] Polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 200 nm are dissolved in an organic solvent of N,N-dimethylformamide and acetone with a volume ratio of 5:5 at a mass ratio of 2:3, and mixed evenly to form a coating slurry with a solid content of 25%. The coating slurry is coated on the surface of the negative electrode sheet and dried at 100° C. with forced air to obtain a functional coating with a thickness of 12 μm.
[0080] The negative electrode sheet of a lithium-ion battery with a total thickness of 124 μm is manufactured by trimming, cutting and stripping.
[0081] Example 3
[0082] The difference from Example 1 is the preparation of the negative electrode sheet.
[0083] Preparation of negative electrode:
[0084] Preparation of negative electrode active material layer: silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber are prepared into negative electrode slurry in a mass ratio of 96:1.5:1.0:1.5, coated on the current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with negative electrode active material layer on both sides is cold pressed;
[0085] Preparation of porous coating:
[0086] Polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 200 nm are dissolved in an organic solvent of N,N-dimethylformamide and acetone with a volume ratio of 5:5 at a mass ratio of 2:8, and mixed evenly to form a coating slurry with a solid content of 25%. The coating slurry is coated on the surface of the negative electrode sheet and dried at 100° C. with forced air to obtain a functional coating with a thickness of 12 μm.
[0087] The negative electrode sheet of a lithium-ion battery with a total thickness of 124 μm is manufactured by trimming, cutting and stripping.
[0088] Example 4
[0089] The difference from Example 1 is the preparation of the negative electrode sheet.
[0090] Preparation of negative electrode:
[0091] Preparation of negative electrode active material layer: silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber are prepared into negative electrode slurry in a mass ratio of 96:1.5:1.0:1.5, coated on the current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with negative electrode active material layer on both sides is cold pressed;
[0092] Preparation of porous coating:
[0093] Dissolve polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 2.5 μm in a mass ratio of 2:8 in an organic solvent of N,N-dimethylformamide and acetone with a volume ratio of 5:5, mix them evenly to form a coating slurry with a solid content of 25%, apply the coating slurry on the surface of the negative electrode sheet, and dry it at 100° C. with forced air to obtain a functional coating with a thickness of 12 μm;
[0094] The negative electrode sheet of a lithium-ion battery with a total thickness of 124 μm is manufactured by trimming, cutting and stripping.
[0095] Example 5
[0096] The difference from Example 1 is the preparation of the negative electrode sheet.
[0097] Preparation of negative electrode:
[0098] A negative electrode slurry is prepared by mixing silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber in a mass ratio of 96:1.5:1.0:1.5, and coated on a current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with a negative electrode active material layer on both sides is cold pressed;
[0099] Preparation of porous coating:
[0100] Polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 200 nm are dissolved in an organic solvent of N,N-dimethylformamide and acetone with a volume ratio of 2:3 at a mass ratio of 2:3, and mixed evenly to form a coating slurry with a solid content of 25%. The coating slurry is coated on the surface of the negative electrode sheet and dried at 100° C. with forced air to obtain a functional coating with a thickness of 8 μm.
[0101] Example 6
[0102] The difference from Example 1 is the preparation of the negative electrode sheet.
[0103] Preparation of negative electrode:
[0104] A negative electrode slurry is prepared by mixing silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber in a mass ratio of 96:1.5:1.0:1.5, and coated on a current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with a negative electrode active material layer on both sides is cold pressed;
[0105] Preparation of porous coating:
[0106] Polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 200 nm are dissolved in an organic solvent of N,N-dimethylformamide and acetone with a volume ratio of 5:5 at a mass ratio of 2:3, and mixed evenly to form a coating slurry with a solid content of 25%. The coating slurry is applied on the surface of the negative electrode sheet and dried at 100° C. with forced air to obtain a functional coating with a thickness of 8 μm.
[0107] The negative electrode sheet for lithium-ion batteries is manufactured by trimming, cutting and slitting. The negative electrode sheet for lithium-ion batteries is 116 μm in total thickness.
[0108] Example 7
[0109] The difference from Example 1 is the preparation of the negative electrode sheet.
[0110] Preparation of negative electrode:
[0111] A negative electrode slurry is prepared by mixing silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber in a mass ratio of 96:1.5:1.0:1.5, and coated on a current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with a negative electrode active material layer on both sides is cold pressed;
[0112] Preparation of porous coating:
[0113] Polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 200 nm are dissolved in an organic solvent of N,N-dimethylformamide and acetone with a volume ratio of 5:5 at a mass ratio of 2:8, and mixed evenly to form a coating slurry with a solid content of 25%. The coating slurry is coated on the surface of the negative electrode sheet and dried at 100° C. with forced air to obtain a functional coating with a thickness of 8 μm.
[0114] The negative electrode sheet for lithium-ion batteries is manufactured by trimming, cutting and slitting. The negative electrode sheet for lithium-ion batteries is 116 μm in total thickness.
[0115] Example 8
[0116] The difference from Example 1 is the preparation of the negative electrode sheet.
[0117] Preparation of negative electrode:
[0118] A negative electrode slurry is prepared by mixing silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber in a mass ratio of 96:1.5:1.0:1.5, and coated on a current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with a negative electrode active material layer on both sides is cold pressed;
[0119] Preparation of porous coating:
[0120] Polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 2.5 μm are dissolved in an organic solvent of N,N-dimethylformamide and acetone with a volume ratio of 5:5 at a mass ratio of 2:8, and mixed evenly to form a coating slurry with a solid content of 25%. The coating slurry is applied on the surface of the negative electrode sheet, and air-dried at 100° C. to obtain a functional coating with a thickness of 8 μm; trimming, cutting, and striping are performed, and the negative electrode sheet of a lithium-ion battery is prepared after stripping.
[0121] Example 9
[0122] The difference from Example 1 is the preparation of the negative electrode sheet.
[0123] Preparation of negative electrode:
[0124] Preparation of negative electrode active material layer: silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber are prepared into negative electrode slurry in a mass ratio of 96:1.5:1.0:1.5, coated on the current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with negative electrode active material layer on both sides is cold pressed;
[0125] Preparation of porous coating:
[0126] Polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 200 nm are dissolved in a mass ratio of 2:8 in dimethylformamide and acetone with a volume ratio of 5:5 as an organic solvent, and mixed evenly to form a coating slurry with a solid content of 25%. The coating slurry is applied on the surface of the negative electrode sheet and dried at 100° C. with forced air to obtain a functional coating with a thickness of 12 μm.
[0127] The negative electrode sheet of a lithium-ion battery with a total thickness of 124 μm is manufactured by trimming, cutting and stripping.
[0128] Comparative Example 1
[0129] A lithium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator spaced between the positive electrode sheet and the negative electrode sheet, and an electrolyte; wherein a porous coating is coated on the negative electrode sheet.
[0130] (1) Preparation of positive electrode
[0131] The positive electrode slurry is prepared by uniformly mixing NCM811 positive electrode active material, conductive agent superconducting carbon and carbon tube, and binder polyvinylidene fluoride in a mass ratio of 96:2:0.5:1.5, coating the positive electrode slurry on one surface of the current collector aluminum foil, drying and rolling at 120°C, and then coating and drying the positive electrode slurry on the other side of the aluminum foil according to the above method, and then cold pressing the prepared aluminum foil with the positive electrode active material layer on both sides; trimming, cutting, and striping are performed, and after stripping, a lithium-ion battery positive electrode sheet is prepared.
[0132] (2) Preparation of negative electrode sheet
[0133] Preparation of negative electrode active material layer: silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber are prepared into negative electrode slurry in a mass ratio of 96:1.5:1.0:1.5, coated on the current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with negative electrode active material layer on both sides is cold pressed;
[0134] The negative electrode sheets of lithium-ion batteries with a total thickness of 100 μm are manufactured by trimming, cutting and stripping.
[0135] (3) Diaphragm: A polyethylene porous film with a thickness of 9 μm was selected as the diaphragm.
[0136] (4) Preparation of electrolyte:
[0137] Lithium hexafluorophosphate is dissolved in a mixed solvent of ethylene carbonate, ethyl methyl carbonate and diethyl carbonate (the mass ratio of the three is 3:5:2) to obtain an electrolyte.
[0138] (5) Preparation of batteries:
[0139] The positive electrode sheet, separator and negative electrode sheet are wound into a battery cell with a capacity of about 5Ah. The separator is located between the adjacent positive and negative electrode sheets, the positive electrode is spot welded out with an aluminum tab, and the negative electrode is spot welded out with a nickel tab; the battery cell is then placed in an aluminum-plastic packaging bag, baked, and injected with the above electrolyte, and finally made into a polymer lithium-ion battery through packaging, formation, capacity division and other processes.
[0140] Comparative Example 2
[0141] The difference from Comparative Example 1 is the preparation of the negative electrode sheet.
[0142] Preparation of negative electrode:
[0143] Preparation of negative electrode active material layer: silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber are prepared into negative electrode slurry in a mass ratio of 96:1.5:1.0:1.5, coated on the current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with negative electrode active material layer on both sides is cold pressed;
[0144] Preparation of porous coating:
[0145] Dissolve polyvinylidene fluoride in N,N-dimethylformamide and acetone in an organic solvent with a volume ratio of 5:5, mix them evenly to form a coating slurry with a solid content of 15%, apply the coating slurry on the surface of the negative electrode sheet, and dry it at 100° C. with forced air to obtain a functional coating with a thickness of 12 μm;
[0146] The negative electrode sheet of a lithium-ion battery with a total thickness of 124 μm is manufactured by trimming, cutting and stripping.
[0147] Comparative Example 3
[0148] The difference from Comparative Example 1 is the preparation of the negative electrode sheet.
[0149] Preparation of negative electrode:
[0150] Preparation of negative electrode active material layer: silicon-carbon negative electrode active material, conductive agent superconducting carbon, thickener sodium carboxymethyl cellulose, and binder styrene-butadiene rubber are prepared into negative electrode slurry in a mass ratio of 96:1.5:1.0:1.5, coated on the current collector copper foil and dried and rolled at 105°C, and then the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method, and then the prepared copper foil with negative electrode active material layer on both sides is cold pressed;
[0151] Preparation of porous coating:
[0152] Dissolve polyvinylidene fluoride and lithium lanthanum zirconium oxide with a D50 of 200 nm in an organic solvent N,N-dimethylformamide at a mass ratio of 2:8, mix them evenly to form a coating slurry with a solid content of 15%, apply the coating slurry on the surface of the negative electrode sheet, and dry it at 100° C. with forced air to obtain a functional coating with a thickness of 12 μm;
[0153] The negative electrode sheet of a lithium-ion battery with a total thickness of 124 μm is manufactured by trimming, cutting and stripping.
[0154] The negative electrode sheets and batteries prepared in the above examples and comparative examples were tested. The results are shown in Table 1.
[0155] Table 1
[0156]
[0157] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A negative electrode plate with a coating, characterized in that: The invention comprises a current collector, a negative electrode active material layer and a porous coating layer which are composited in sequence, wherein the porous coating layer comprises a composite material of a high molecular polymer and inorganic ceramic particles; the porosity of the porous coating layer is 20% to 70%; the inorganic ceramic particles are selected from one or more of yttrium-doped zirconium oxide, gadolinium-doped cerium oxide, lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium lanthanum zirconium niobium oxide and lithium lanthanum titanate; The negative electrode active material in the negative electrode active material layer includes a silicon-carbon negative electrode material; The method for preparing the negative electrode sheet comprises the following steps: A) coating the negative electrode slurry on the surface of the current collector to obtain a negative electrode active material layer; B) dispersing a high molecular polymer and inorganic ceramic particles in a pore control solution to obtain a coating slurry; the porosity control solution is a mixed solution composed of two or more solvents with different boiling points; C) coating the coating slurry on the surface of the negative electrode active material layer to obtain a negative electrode sheet.
2. The negative electrode sheet according to claim 1, characterized in that: The high molecular polymer is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, polypyrrole, polythiophene, polyethylene, polypropylene, polystyrene, polyacrylamide, ethylene-propylene-diene copolymer resin, styrene-butadiene rubber, polybutadiene, fluororubber, polyethylene oxide, polyvinyl pyrrolidone, acrylic resin, epoxy resin, polyvinyl alcohol, carboxypropyl cellulose, ethyl cellulose, sodium carboxymethyl cellulose, styrene-butadiene latex and high molecular materials.
3. The negative electrode sheet according to claim 1, characterized in that: The particle size of the inorganic ceramic particles is 100 nm to 20 μm.
4. The negative electrode sheet according to claim 1, characterized in that: The particle size of the inorganic ceramic particles is 200nm~2.5μm.
5. The negative electrode sheet according to claim 1, characterized in that: The mass ratio of the porous coating polymer to the inorganic ceramic particles is 2:3-1:
50.
6. The negative electrode sheet according to claim 1, characterized in that: Based on the total volume of the negative electrode sheet, the total volume of the porous coating layer is no more than 80% of the total volume of the negative electrode sheet.
7. The negative electrode sheet according to claim 1, characterized in that: The thickness of the negative electrode active material layer is greater than or equal to the thickness of the porous coating layer; The thickness of the porous coating is 2-50 μm; The thickness of the negative electrode plate is 20 μm to 300 μm.
8. The negative electrode sheet according to claim 1, characterized in that: The thickness of the porous coating layer is 8-12 μm.
9. A method for preparing a negative electrode sheet according to any one of claims 1 to 8, characterized in that: The following steps are involved: A) coating the negative electrode slurry on the surface of the current collector to obtain a negative electrode active material layer; B) dispersing a high molecular polymer and inorganic ceramic particles in a pore control solution to obtain a coating slurry; the porosity control solution is a mixed solution composed of two or more solvents with different boiling points; C) coating the coating slurry on the surface of the negative electrode active material layer to obtain a negative electrode sheet.
10. The preparation method according to claim 9, characterized in that: The porosity controlling solution is selected from a mixed solution of deionized water and acetone, a mixed solution of acetone and dimethyl carbonate, a mixed solution of N,N-dimethylformamide and dimethyl carbonate, or a mixed solution of N,N-dimethylacetamide and dimethyl carbonate, and the volume ratio is: (1-10):
1.
11. The preparation method according to claim 9, characterized in that: The coating slurry has a solid content of 7wt% to 50wt%.
12. A lithium ion battery, characterized in that: Comprising the negative electrode sheet as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Electrode material, electrode and electrode material manufacturing method
CN103828102A
Negative electrode for secondary batteries and method for producing same
CN104303340A
Lithium-ion battery negative pole piece, and preparation method and application thereof
CN105070882A
Safety coating, electrode plate, preparation method of electrode plate and lithium ion battery
CN113488609A