Electrolyte and battery
By using disodium ethylenediaminetetraacetate and tetrasodium ethylenediaminetetraacetate as additives in the sodium-ion battery electrolyte, the problem of long infiltration time of the sodium-ion battery electrolyte is solved and higher capacity development and cycle performance are achieved. , improving battery production efficiency and safety.
Patent Information
- Application Number
- CN202211347351.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-10-31
AI Technical Summary
The existing sodium-ion battery electrolyte requires a long time in the positive electrode, negative electrode and separator infiltration process, which limits the production capacity of the battery production line.
Disodium ethylenediaminetetraacetate and tetrasodium ethylenediaminetetraacetate are used as additives to increase the concentration of sodium ions in the electrolyte, reduce the surface tension of the positive electrode, negative electrode and separator, improve wettability, and form a stable SEI film on the surface of the negative electrode , enhance the cycle performance of sodium-ion batteries.
It shortens the infiltration time of the electrolyte, improves the capacity and cycle performance of the sodium-ion battery, increases the production capacity of the production line, and enhances the safety performance of the battery.
Smart Images

Figure BDA0003918733010000053 
Figure BDA0003918733010000061 
Figure BDA0003918733010000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of sodium ion batteries, in particular to an electrolyte and a battery. Background Art
[0002] At present, lithium resources are extremely scarce, and the price of ternary materials has risen sharply, resulting in a substantial increase in the cost of lithium-ion batteries. In comparison, low-cost sodium-ion batteries appear to have more advantages.
[0003] The structure and working principle of sodium-ion batteries are similar to those of lithium batteries. Compared with lithium batteries, sodium-ion batteries have wide resources, low costs and small fluctuations. Considering the comprehensive energy density and cycle life, sodium batteries are expected to first replace lead-acid and lithium iron phosphate batteries in the start-stop, low-speed electric vehicles, energy storage and other markets.
[0004] The electrolyte is the carrier of ion transmission in the battery, and plays the role of ion conduction between the positive and negative electrodes. It is generally composed of high-purity organic solvents, electrolyte salts, and other necessary additives in a certain proportion. It is the guarantee for the battery to obtain advantages such as high voltage and high specific energy. In order to ensure stable operation and excellent performance of the battery, the electrolyte is generally required to completely infiltrate the electrode and reach a balanced state, so a longer infiltration time is required, which limits the production capacity of the battery production line. Summary of the invention
[0005] In view of this, the technical problem to be solved by the present invention is to provide an electrolyte and a battery. The electrolyte provided by the present invention can shorten the time of the wetting process of the positive electrode, the negative electrode and the separator without reducing the battery capacity and the capacity retention rate.
[0006] The present invention provides an electrolyte, comprising: sodium salt, additives, solvent and auxiliary agent; the auxiliary agent is at least one of disodium ethylenediaminetetraacetate and tetrasodium ethylenediaminetetraacetate. Specifically, the electrolyte of the present invention is a sodium ion battery electrolyte.
[0007] The auxiliary agent of the present invention is sodium salt of ethylenediaminetetraacetic acid. In certain embodiments of the present invention, the auxiliary agent is disodium ethylenediaminetetraacetic acid and tetrasodium ethylenediaminetetraacetic acid, and the mass ratio of disodium ethylenediaminetetraacetic acid and tetrasodium ethylenediaminetetraacetic acid is 1-10:1-10. In certain embodiments of the present invention, the mass percentage of the auxiliary agent in the electrolyte is 0.1%-0.5%.
[0008] The present invention uses at least one of tetrasodium ethylenediaminetetraacetate (EDTA-4Na) and disodium ethylenediaminetetraacetate (EDTA-2Na) as an auxiliary agent for the sodium ion battery electrolyte, which has the following effects: first, it plays a role in appropriately increasing the sodium ion concentration in the electrolyte, and appropriately improves the capacity of the sodium ion battery. Second, it significantly reduces the surface tension of the contact interface between the positive electrode, the negative electrode and the diaphragm and the electrolyte before formation, thereby improving the wettability of the positive electrode, the negative electrode and the diaphragm in the electrolyte, so that the electrolyte can fully infiltrate the positive electrode, the negative electrode and the diaphragm before formation, shortening the time of the infiltration process, and making a significant contribution to the production capacity improvement of the production line; at the same time, after the contact area between the positive electrode, the negative electrode and the diaphragm and the electrolyte is improved, the transmission resistance of sodium ions at the electrode interface becomes smaller, which is helpful for the deintercalation of sodium ions on the electrode surface, thereby improving the capacity of the sodium ion battery. Third, during the formation, EDTA-4Na and EDTA-2Na help to form a dense, uniform and stable SEI film on the negative electrode surface. The SEI film is not easy to decompose, which improves the cycle performance of the sodium ion battery and reduces the generation of gas in the later use process. 2- EDTA 4- It can complex with heavy metal ions precipitated from the positive electrode material, preventing the heavy metal ions from migrating to the negative electrode during charging or reacting and precipitating on the negative electrode surface, thereby improving the safety performance of sodium ion batteries.
[0009] In certain embodiments of the present invention, the sodium salt is selected from at least one of sodium hexafluorophosphate, sodium perchlorate, sodium difluorophosphate, sodium bisoxalatoborate, sodium difluorooxalatoborate, sodium bistrifluoromethylsulfonyl imide and sodium bisfluorosulfonyl imide. In one embodiment, the sodium salt is selected from sodium hexafluorophosphate. In certain embodiments of the present invention, the mass percentage of the sodium salt in the electrolyte is 8% to 20%.
[0010] The solvent of the present invention is an organic solvent. In certain embodiments of the present invention, the solvent is selected from at least one of ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, and ethyl acetate. In one embodiment, the solvent is selected from ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a mass ratio of 2:2:1. In certain embodiments of the present invention, the mass percentage of the solvent in the electrolyte is 60% to 80%.
[0011] The additive of the present invention is an additive suitable for the field of batteries. In certain embodiments of the present invention, the additive is selected from vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, diethyl pyrocarbonate, 1,3-propane sultone, vinyl sulfate, 1,3-propylene glycol cyclic sulfate, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, 4,4'-linked-1,3-dioxolane-2,2'-dione, 3,3-disulfate vinyl ester, triallyl phosphate, tripropargyl phosphate. In one embodiment, the additive is selected from vinylene carbonate, vinyl ethylene carbonate and vinyl sulfate in a mass ratio of 1:1:1. In certain embodiments of the present invention, the mass percentage of the additive in the electrolyte is 2% to 10.5%.
[0012] The present invention provides a method for preparing the above-mentioned electrolyte, comprising: mixing a solvent, an additive, an auxiliary agent and a sodium salt to obtain the above-mentioned electrolyte. Specifically, a solvent, an additive and an auxiliary agent are mixed to obtain a mixed solution, and sodium salt is added to the mixed solution to obtain the above-mentioned electrolyte. In certain embodiments of the present invention, under a protective gas atmosphere, an additive is added to a solvent, and then an auxiliary agent is added, and a mixed solution is obtained after mixing, and sodium salt is added to the mixed solution, and the above-mentioned electrolyte is obtained after mixing. In one embodiment, the protective gas is selected from at least one of nitrogen, helium or argon. In one embodiment, the O2 content in the protective gas is less than 1ppm; the H2O content in the protective gas is less than 1ppm. The solvent, additive, auxiliary agent and sodium salt are the same as above and will not be repeated.
[0013] The present invention also provides a battery, comprising a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and the above electrolyte. Specifically, the battery of the present invention is a sodium ion battery.
[0014] The battery of the present invention includes a positive electrode. In some embodiments of the present invention, the positive electrode includes a positive electrode active material, a positive electrode conductive agent, a positive electrode binder and an aluminum foil current collector; wherein the positive electrode active material is selected from at least one of transition metal oxides, polyanionic compounds, Prussian blue and its analogs and organic compounds; the positive electrode conductive additive is selected from at least one of Super P conductive agent, carbon nanotubes, acetylene black, Ketjen black, conductive graphite, carbon fiber, and graphene; the positive electrode binder is selected from at least one of fluorine-containing resin, polyether resin, cellulose-type binder, polyacrylate-type binder, and polyimide.
[0015] The battery of the present invention includes a negative electrode. In some embodiments of the present invention, the negative electrode includes a negative electrode active material, a negative electrode conductive additive, a negative electrode binder, and a negative electrode aluminum foil current collector; wherein the negative electrode active material is hard carbon; the negative electrode conductive additive includes at least one of Super P conductive agent, carbon nanotubes, acetylene black, Ketjen black, conductive graphite, carbon fiber, and graphene; the negative electrode binder includes but is not limited to at least one of fluorine-containing resin, polyether resin, cellulose-type binder, polyacrylate-type binder, and polyimide.
[0016] The present invention includes a separator disposed between the positive electrode and the negative electrode. In certain embodiments of the present invention, the separator is at least one of polypropylene, polyethylene, and glass fiber. The present invention also includes an electrolyte, which is the same as the above and will not be described in detail.
[0017] The present invention provides an electrolyte, comprising: a sodium salt, an additive, a solvent and an auxiliary agent; the auxiliary agent is at least one of disodium ethylenediaminetetraacetate and tetrasodium ethylenediaminetetraacetate. Specifically, the electrolyte of the present invention is a sodium ion battery electrolyte. The electrolyte provided by the present invention can shorten the time of the wetting process of the positive electrode, the negative electrode and the diaphragm without reducing the battery capacity and the capacity retention rate. Experiments show that compared with the case where the electrolyte of the present invention is not added with the auxiliary agent of the present invention, the 0.2C capacity and the 0.5C / 1C cycle 400 capacity retention rate of the electrolyte of the present invention are higher, and the infiltration time is significantly shortened. DETAILED DESCRIPTION
[0018] The present invention discloses an electrolyte and a battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0019] The present invention prepares the electrolytes of Examples 1 to 6 and Comparative Example 1 according to the electrolyte formula shown in Table 1; wherein EC is ethylene carbonate; DMC is dimethyl carbonate; EMC is ethyl methyl carbonate; VC is vinylene carbonate; DTD is vinyl sulfate; EDTA-2Na is disodium ethylenediaminetetraacetate, and its structural formula is Its CAS No. is 139-33-3; EDTA-4Na is tetrasodium ethylenediaminetetraacetate, and its structural formula is Its CAS No. is 13235-36-4.
[0020] Table 1
[0021]
[0022]
[0023] The present invention will be further described below in conjunction with embodiments:
[0024] Example 1
[0025] In a glove box filled with nitrogen (O2 <1ppm, H2O <1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) were mixed uniformly in a mass ratio of 2:2:1 to obtain 79g of an organic solvent, and then 2g of vinylene carbonate (VC), 2g of vinyl ethylene carbonate (VEC) and 2g of vinyl sulfate (DTD) were added to the organic solvent as additives, and then 0.3g of disodium ethylenediaminetetraacetate (EDTA-2Na) was added as an auxiliary agent to obtain a mixed solution. Finally, 14.7g of sodium hexafluorophosphate was slowly added to the mixed solution, and the electrolyte was prepared after mixing uniformly.
[0026] Example 2
[0027] The difference from Example 1 is that 0.3 g of tetrasodium ethylenediaminetetraacetate (EDTA-4Na) is used as an auxiliary agent.
[0028] Example 3
[0029] The difference from Example 1 is that 0.5 g of disodium ethylenediaminetetraacetate (EDTA-2Na) is used as an auxiliary agent.
[0030] Example 4
[0031] The difference from Example 1 is that 0.5 g of tetrasodium ethylenediaminetetraacetate (EDTA-4Na) is used as an auxiliary agent.
[0032] Example 5
[0033] The difference from Example 1 is that 0.3 g of disodium ethylenediaminetetraacetate (EDTA-2Na) and tetrasodium ethylenediaminetetraacetate (EDTA-4Na) in a mass ratio of 1:2 is used as an auxiliary agent.
[0034] Example 6
[0035] The difference from Example 1 is that 0.5 g of disodium ethylenediaminetetraacetate (EDTA-2Na) and tetrasodium ethylenediaminetetraacetate (EDTA-4Na) in a mass ratio of 1:2 is used as an auxiliary agent.
[0036] Example 7
[0037] The difference from Example 1 is that 0.3 g of disodium ethylenediaminetetraacetate (EDTA-2Na) and tetrasodium ethylenediaminetetraacetate (EDTA-4Na) in a mass ratio of 1:1 is used as an auxiliary agent.
[0038] Example 8
[0039] The difference from Example 1 is that 0.5 g of disodium ethylenediaminetetraacetate (EDTA-2Na) and tetrasodium ethylenediaminetetraacetate (EDTA-4Na) in a mass ratio of 1:1 is used as an auxiliary agent.
[0040] Comparative Example 1
[0041] In a glove box filled with nitrogen (O2 < 1ppm, H2O < 1ppm), ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) were mixed uniformly in a mass ratio of 2:2:1 to obtain 79.3g of an organic solvent, and then 2g of vinylene carbonate (VC), 2g of vinyl ethylene carbonate (VEC) and 2g of vinyl sulfate (DTD) were added to the organic solvent as additives to obtain a mixed solution. Finally, 14.7g of sodium hexafluorophosphate was slowly added to the mixed solution, and the electrolyte was obtained after mixing uniformly.
[0042] Performance Testing
[0043] Sodium vanadium fluorophosphate (NaVPO4F) positive electrode material, hard carbon negative electrode material, polypropylene diaphragm and the electrolyte described in Examples 1 to 6 and Comparative Example 1 are respectively made into 18650 cylindrical sodium ion batteries, and the time required for the pole piece and diaphragm to be completely wetted is evaluated after injection; after formation and high temperature aging, the normal temperature capacity test and cycle test are carried out in sequence. Among them, the method of the normal temperature capacity test is: charge and discharge at 0.2C, repeat 3 times, record the capacity of 3 divided capacities and take the average value, and the average capacity is the capacity of the sodium ion battery. The method of the normal temperature cycle test is: at an ambient temperature of 25°C, charge to 4.2V at 0.5C constant current and constant voltage, the cut-off current is 0.02C, and then discharge to 2.75V at 1C current constant current, cycle several times, record the discharge capacity of the first circle and the discharge capacity of the last circle, calculate the capacity retention rate, and the calculation formula of the capacity retention rate is: capacity retention rate = the last discharge capacity / the first discharge capacity × 100%. The results of the above room temperature capacity test and cycle test are shown in Table 2.
[0044] Table 2
[0045]
[0046]
[0047] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An electrolyte for improving battery wettability, characterized in that: include: Sodium salt, additives, solvents and auxiliary agents; the electrolyte is an electrolyte for sodium ion batteries; The auxiliary agent is disodium ethylenediaminetetraacetate and tetrasodium ethylenediaminetetraacetate, and the mass ratio of disodium ethylenediaminetetraacetate to tetrasodium ethylenediaminetetraacetate is 1:(1~2); The mass percentage of the auxiliary agent in the electrolyte is 0.1% to 0.5%; The sodium salt is selected from at least one of sodium hexafluorophosphate, sodium perchlorate, sodium difluorophosphate, sodium bisoxalatoborate, sodium difluorooxalatoborate, sodium bistrifluoromethylsulfonyl imide and sodium bisfluorosulfonyl imide.
2. The electrolyte according to claim 1, characterized in that The solvent is selected from at least one of ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate and ethyl acetate.
3. The electrolyte according to claim 1, characterized in that The additive is selected from at least one of vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, diethyl pyrocarbonate, 1,3-propane sultone, vinyl sulfate, 1,3-propylene glycol cyclic sulfate, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, 4,4'-di-1,3-dioxolane-2,2'-dione, 3,3-ethylene disulfate, triallyl phosphate, and tripropargyl phosphate.
4. The electrolyte according to claim 1, characterized in that The mass percentage of the sodium salt in the electrolyte is 8% to 20%.
5. The electrolyte according to claim 1, characterized in that The mass percentage of the solvent in the electrolyte is 60% to 80%.
6. The electrolyte according to claim 1, characterized in that The mass percentage of the additive in the electrolyte is 2% to 10.5%.