Composite current collector and preparation method thereof, electrode sheet, and battery
By using a composite current collector composed of a polymer substrate and multi-layer conductive layers in a lithium-ion battery, the problem of insufficient toughness after thinning of the current collector is solved, and the high cycle life and energy density of the battery are achieved, which is maintained through slow-release functional additives. The stability of the SEI film improves the overall performance of the battery.
Patent Information
- Application Number
- CN202110712587.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-06-25
AI Technical Summary
The current collector in the existing lithium-ion battery has insufficient toughness after thinning, is easily broken, and has a single function, which cannot improve the electrochemical performance of the battery.
A composite current collector is used, which is composed of a polymer substrate and a multi-layer conductive layer. The polymer substrate has good toughness and contains functional additives in the electrolyte, which can slow down and participate in the formation of a stable solid electrolyte interface film (SEI). , improve the cycle performance of the battery.
It improves the cycle life and energy density of the battery, enhances the mechanical and electrochemical properties of the battery, avoids breakage of the current collector during mechanical deformation, and maintains the stability of the SEI film through slow-release functional additives.
Smart Images

Figure CN115528250B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a composite current collector and a preparation method thereof, an electrode sheet and a battery. Background Art
[0002] The common current collector in lithium-ion batteries is generally metal foil, such as aluminum foil on the positive electrode side and copper foil on the negative electrode side. However, since metal foil is an inactive component in the battery, thinning the metal foil is beneficial to improving the energy density of the battery. However, when the thickness of the metal foil is too thin, its toughness is low. It is easy to break during battery manufacturing processes such as coating and winding, and in special scenarios where the battery is in a bent state, affecting the battery preparation yield and the reliability of battery use. In addition, the current battery current collector has a single function, which only plays the role of collecting current and cannot take into account the role of improving other electrochemical properties of the battery. Summary of the invention
[0003] In view of this, the present application provides a composite current collector with a novel structure, which has good flexibility and light weight, and contains functional additives that can be slowly released into the battery electrolyte, so that the composite current collector can also play a role in improving the electrochemical performance of the battery.
[0004] In the first aspect, an embodiment of the present application provides a composite current collector, comprising a polymer substrate, a first conductive layer arranged on a first surface of the polymer substrate and a second conductive layer arranged on a second surface, the first surface and the second surface being arranged relative to each other, wherein the polymer substrate contains a polymer and a functional additive, the functional additive is soluble in a battery electrolyte and can participate in the formation of a SEI film (solid electrolyte interface); along a first direction perpendicular to the thickness of the composite current collector, the thickness of the polymer substrate gradually increases from the middle to both sides.
[0005] In the composite current collector provided in the first aspect of the embodiment of the present application, the polymer substrate is located in the middle, which will not affect the electronic conduction function of the conductive layer, and the polymer substrate has good toughness, so that the composite current collector can withstand a certain degree of mechanical deformation such as stretching, winding, bending, etc. without breaking. The special structure of the polymer substrate, which is thin in the middle and thick on both sides, can provide sustained-release conditions for functional additives that are soluble in the electrolyte and pre-stored therein, so that they can be gradually released into the battery electrolyte when needed and participate in the formation of a stable SEI film, thereby improving the battery's cycle performance.
[0006] In the embodiment of the present application, the surfaces of the first conductive layer and the second conductive layer facing away from the polymer substrate are both flat.
[0007] In some embodiments of the present application, the thickness of one of the first conductive layer and the second conductive layer gradually decreases from the middle to both sides, and the thickness of the other one remains unchanged from the middle to both sides.
[0008] In some other embodiments of the present application, the distances between the cross section of the thinnest part of the polymer substrate and the first surface and the second surface gradually increase from the middle of the polymer substrate to both sides.
[0009] Optionally, the thickness of the first conductive layer and the second conductive layer gradually decreases from the middle to both sides.
[0010] Optionally, the middle thickness of the first conductive layer and the second conductive layer are both within the range of 0.05 μm-3.95 μm, and the thickness on both sides are both within the range of 5 nm-3.5 μm.
[0011] Optionally, the polymer substrate has a middle thickness of 0.1 μm-7.9 μm and a thickness on both sides of 1 μm-7.99 μm.
[0012] In the embodiment of the present application, the thickness of the composite current collector does not exceed 8 μm.
[0013] In an embodiment of the present application, the functional additive includes one or more of lithium nitrate, magnesium nitrate, silver nitrate, lithium bis(oxalatoborate), and lithium difluorooxalatoborate.
[0014] In the embodiment of the present application, the functional additive accounts for 5%-40% by mass in the polymer substrate.
[0015] In the embodiment of the present application, the polymer substrate has a porous structure.
[0016] In some embodiments of the present application, the polymer substrate further contains a conductive additive.
[0017] In some embodiments of the present application, the first conductive layer and the second conductive layer have a porous structure.
[0018] In a second aspect, the present application also provides an electrode sheet, which includes the composite current collector described in the first aspect of the present application, and an electrode active material layer formed on the first conductive layer and the second conductive layer of the composite current collector. The electrode sheet has a high preparation yield, and using it in a battery can help effectively improve the cycle performance and energy density of the battery.
[0019] In a third aspect, an embodiment of the present application further provides a battery, the battery comprising a positive electrode sheet, a negative electrode sheet, and a separator and an electrolyte located between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet and / or the negative electrode sheet comprises the electrode sheet as described in the second aspect of the embodiment of the present application. The battery provided by the present application may have a long cycle life and a high energy density.
[0020] In some embodiments of the present application, the negative electrode plate is the electrode plate described in the second aspect of the embodiment of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1a A schematic diagram of the structure of a composite current collector provided in an embodiment of the present application;
[0022] Figure 1b Another schematic diagram of the structure of the composite current collector provided in the embodiment of the present application;
[0023] Figure 2a Provided for the embodiments of this application Figure 1a A flow chart of a preparation method of the composite current collector shown;
[0024] Figure 2b Provided for the embodiments of this application Figure 1a Another preparation method flow chart of the composite current collector shown;
[0025] Figure 2c Provided for the embodiments of this application Figure 1b A flow chart of a preparation method of the composite current collector shown;
[0026] Figure 3 The embodiment of the present application provides Figure 1a A schematic diagram of the structure of the negative electrode sheet of the composite current collector;
[0027] Figure 4 The embodiment of the present application provides Figure 3 A schematic diagram of the structure of a lithium-ion battery with a negative electrode in the middle. DETAILED DESCRIPTION
[0028] The embodiments of the present application are described in detail below in conjunction with the drawings in the embodiments of the present application.
[0029] Figure 1a , Figure 1bTwo representative structural schematic diagrams of the composite current collector provided in the embodiments of the present application are shown respectively. The composite current collector 100 includes a polymer substrate 10, the polymer substrate 10 has a first surface 10A and a second surface 10B arranged opposite to each other, a first conductive layer 20 is arranged on the first surface 10A of the polymer substrate 10, and a second conductive layer 20' is arranged on the second surface 10B, wherein, along the first direction perpendicular to the thickness of the composite current collector 10, the thickness of the polymer substrate 10 gradually increases from the middle to both sides; the polymer substrate 10 contains a polymer and a functional additive 103, the functional additive 103 is soluble in the battery electrolyte and can participate in the formation of the SEI film. Among them, the first conductive layer 20 can partially cover or completely cover the first surface 10A of the polymer substrate 10, and the second conductive layer 20' can partially cover or completely cover the second surface 10B of the polymer substrate 10. Subsequently, the electrode active material can be deposited or coated on the two conductive layers to obtain an electrode plate.
[0030] In the composite current collector 100 provided in the embodiment of the present application, the polymer substrate 10 is located in the middle, and the conductive layer 20 is provided on both sides thereof. The conductive layer 20 can play the role of electron conduction and current collection. The polymer substrate 10 is used to carry the conductive layer 20, and supports and protects the conductive layer 20. The polymer substrate 10 has good toughness, which can ensure that the conductive layer 20 thereon is not easy to crack or break under a certain degree of mechanical deformation such as stretching, winding, bending, etc., and can still withstand large tensile and compressive deformation after loading the electrode active material layer, thereby improving the battery preparation yield and meeting special use scenarios such as battery extrusion and bending. In addition, since the density of the polymer substrate 10 is usually smaller than that of metal, the above-mentioned composite current collector 100 is lighter than the density of conventional battery current collectors such as aluminum foil and copper foil, and the battery made therefrom is also lighter in weight, which is conducive to improving the energy density of the battery.
[0031] In addition, the battery electrolyte usually contains organic solvents, electrolyte lithium salts and additives, etc. The original amount of additives added to the electrolyte is generally saturated, and the content is generally small due to its low solubility. The additives have a significant positive effect on the battery performance, but they will be consumed as the battery cycle progresses to form a SEI film, and when the content of the additives is too low or is completely consumed, it is not conducive to the stability of the SEI film. The above-mentioned polymer substrate 10, which is thin in the middle and thick on both sides, can provide a sustained release condition for the functional additives 103 that can be dissolved in the electrolyte pre-stored therein, so that it can be dissolved from both sides of the polymer substrate 10 when needed, and timely added to the electrolyte and participate in the formation of the SEI film, so as to supplement the consumption of the SEI film-forming agent with low solubility in the electrolyte during the operation of the battery, which helps to ensure that the SEI film on the surface of the electrode plate remains stable and complete, and improves the long cycle capacity of the battery.
[0032] Therefore, the composite current collector provided in the embodiment of the present application has good toughness and light weight, and can also slowly release functional additives to improve the cycle performance of the battery, and has other functionalities besides electronic conductivity.
[0033] Figure 1a In the figure, not only does the thickness of the polymer substrate 10 gradually increase from the middle to the sides, but also the distance from the cross section 10C (horizontal direction, parallel to each conductive layer) at the thinnest part of the polymer substrate 10 to the first surface 10A and the second surface 10B gradually increases along the middle of the polymer substrate 10 to the sides. At this time, the shape of the polymer substrate 10 can be called a "double trumpet type" or a "slender waist type". Among them, the first surface 10A and the second surface 10B can be planes or curved surfaces. The above-mentioned "first direction" can be the length direction or width direction of the composite current collector 100, that is, the horizontal direction. For example, when the first direction is the length direction, the shape of the longitudinal section of the polymer substrate 10 along the length direction (Z direction, parallel to the thickness direction) is as follows: Figure 1a As shown, there are two trapezoids lying horizontally with the same short side; the shape of the longitudinal section of the polymer substrate 10 along the width direction (Z direction, parallel to the thickness direction) is a rectangle.
[0034] Accordingly, Figure 1a In the embodiment, along the first direction, the thickness of the first conductive layer 20 and the second conductive layer 20' gradually decreases from the middle to the two sides. At this time, the thickness of the conductive layer is thick in the middle and thin on both sides, so that it is not easy to be damaged under high mechanical deformation, and it is also convenient to ensure that the outer surface of the composite current collector 100 formed by the above-mentioned polymer substrate 10 and the two conductive layers 20 is basically flat. Optionally, the surfaces of the first conductive layer 20 and the second conductive layer 20' facing away from the polymer substrate 10 are both flat. This makes it easy to form an electrode active material layer with uniform and controllable thickness on the conductive layer later.
[0035] In some embodiments of the present application, the polymer substrate 10 is an axisymmetric structure, wherein the middle cross section (horizontal direction) of the thinnest part of the polymer substrate 10 is the symmetry plane of the polymer substrate 10. In this case, it is beneficial to form two conductive layers with the same morphology and size characteristics on the opposite sides of the polymer substrate 10. Optionally, the conductive layers 20 and 20' are symmetrically distributed on both sides of the polymer substrate 10.
[0036] Figure 1aIn the embodiment, the middle thickness of the polymer substrate 10 can be 0.1 μm-7.9 μm, and the thickness on both sides can be 1 μm-7.99 μm. In other words, the thickness of the polymer substrate 10 gradually increases from 0.1 μm-7.9 μm to 1 μm-7.99 μm from the middle to the two sides, and the thickness on both sides is 1 μm-7.99 μm. The "middle" and "both sides" of the above-mentioned polymer substrate are both for the above-mentioned first direction. The middle thickness refers to the thickness of the thinnest part of the polymer substrate, and the thickness on both sides refers to the thickness of the outermost side of the polymer substrate along the first direction (or called "edge thickness"), that is, the thickness of the thickest part. A polymer substrate with suitable thickness can avoid fracture during the processing of the pole piece and avoid negative impact on the volume energy density of the battery. Among them, the middle thickness of the polymer substrate 10 can be 0.1, 0.5, 1, 2, 3, 4, 5, 6 or 7.5 μm, etc., and the thickness on both sides can be 1, 2, 3, 4, 5, 6, 7 or 7.5 μm, etc. For example, the polymer substrate 10 has a thickness of 1 μm in the middle and 4 μm on both sides. At this time, the average thickness of the polymer substrate 10 is 2.5 μm. The average thickness refers to the average value of the thickness at the thickest part of the polymer substrate 10 and the thickness at the thinnest part.
[0037] Figure 1a In the embodiment, the middle thickness of the conductive layer 20 and 20' can be independently in the range of 0.05μm-3.95μm, and the thickness on both sides can be independently in the range of 5nm-3.5μm. A conductive layer of suitable thickness is conducive to ensuring the lighter density of the composite current collector 100, as well as effective electron conduction under high mechanical deformation, and ensuring a longer cycle life of the electrode plate as a whole. Among them, the middle thickness of each conductive layer can be 0.05, 0.06, 0.08, 0.1, 0.2, 0.5, 1, 2, 3 or 3.5μm, etc., and the thickness on both sides can be 10nm, 20nm, 50nm, 100nm, 120nm, 200nm, 500nm, 1μm, 2μm or 3μm, etc. Exemplarily, the middle thickness of the first conductive layer 20 and the second conductive layer 20' can both be 0.5μm, and the thickness on both sides can both be 2μm. At this time, the average thickness of the first conductive layer 20 and the second conductive layer 20' is 1.25μm. It should be noted that the setting Figure 1a The thickness characteristics of the two conductive layers on the opposite sides of the polymer substrate 10 may be the same or different.
[0038] With the above Figure 1a Different in Figure 1bIn the embodiment, the distance between the cross section 10C at the thinnest part of the polymer substrate 10 and the first surface 10A gradually increases along the first direction from the middle of the polymer substrate 10 to both sides, while the distance between the cross section 10C at the thinnest part of the polymer substrate 10 and the second surface 10B remains substantially unchanged. In this case, the shape of the polymer substrate 10 can be called a "single trumpet type". In this case, Figure 1b In the embodiment, the thickness of the first conductive layer 20 gradually decreases from the middle to the sides, and the thickness of the second conductive layer 20' remains unchanged from the middle to the sides. The surfaces of the first conductive layer 20 and the second conductive layer 20' facing away from the polymer substrate 10 are also flat, which is conducive to forming electrode active material layers with uniform and controllable thickness thereon.
[0039] Similarly, Figure 1b The first conductive layer 20 may have a thickness in the middle of 0.05 μm to 3.95 μm and a thickness on both sides of 5 nm to 3.5 μm; the second conductive layer 20' may have a thickness of 0.1 μm to 7.9 μm. The polymer substrate 10 may have a thickness in the middle of 0.05 μm to 3.95 μm and a thickness on both sides of 0.5 μm to 4 μm.
[0040] In the embodiment of the present application, the functional additive 103 in the polymer substrate 10 may include one or more of lithium nitrate (LiNO3), magnesium nitrate (Mg(NO3)2), silver nitrate (AgNO3), lithium bis(oxalatoborate) (LiBOB), lithium difluoro(oxalatoborate) (LiDFOB), etc. Among them, these functional additives can all participate in the formation of SEI film, and lithium nitrate, LiBOB, and LiDFOB are lithium-containing compounds, which can also supplement the concentration of lithium in the lithium deposition area, shorten the transmission path of lithium ions, and help improve the rate performance of the battery. Magnesium nitrate and silver nitrate do not contain lithium elements. After forming an SEI film at the negative electrode, they can also serve as sites for guiding lithium ion deposition, control the uniform deposition of lithium ions on the surface of the negative electrode sheet, effectively inhibit the growth of lithium dendrites on the surface of the negative electrode, and improve the safety performance of the battery. In addition, the above-mentioned functional additives will generate a pore structure in situ after dissolving into the electrolyte, so that the functional additives located on both sides of the thicker polymer substrate will generate a pore structure after dissolving into the electrolyte, which is conducive to the dissolution of the functional additives in the thinner polymer substrate.
[0041] Optionally, the mass proportion of the functional additive 103 in the polymer substrate 10 may be 5%-40%. The functional additive is added at this mass ratio, which substantially does not affect the mechanical properties of the polymer substrate 10. Among them, the first additive 103 may be uniformly distributed relative to the polymer constituting the polymer substrate 10. However, overall, the mass proportion of the first additive 103 in the middle of the composite current collector is less than its mass proportion on both sides of the composite current collector.
[0042] In the embodiment of the present application, the polymer constituting the polymer substrate 10 may include one or more of polyimide, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyethylene terephthalate, polybutylene terephthalate, perfluorosulfonic acid polymer, styrene-butadiene rubber, etc., but is not limited thereto. Among them, the density of the polymer substrate 10 is less than the density of the conductive layer 20. In this way, the surface density of the composite current collector 100 provided in the embodiment of the present application is lower than that of the pure metal foil, which is conducive to improving the weight energy density of the battery.
[0043] In the embodiment of the present application, the polymer substrate 10 has a porous structure. The porous structure of the polymer substrate 10 can facilitate the release of the functional additive 103, especially the dissolution of the functional additive 103 located at the edge of the polymer substrate 10, and can also further reduce the surface density of the composite current collector 100, which is more conducive to improving the energy density of the battery. In the slurry for preparing the polymer substrate, due to the presence of the above-mentioned functional additives, based on the interaction between the functional additives and the solvent, after the solvent evaporates, the formed polymer substrate 10 has a certain porous structure. Of course, a pore-forming agent that is susceptible to thermal decomposition can also be added to the slurry for preparing the polymer substrate so that the polymer substrate 10 has a porous structure. Specifically, the porosity of the polymer substrate 10 is 1%-20%, and the pore size is 10nm-10μm. Appropriate porosity can prevent the polymer substrate 10 from having holes due to excessively high porosity, affecting its toughness.
[0044] In some embodiments of the present application, the polymer substrate 10 also contains a conductive additive. That is, the constituent materials of the polymer substrate 10 include the aforementioned polymer, functional additives and conductive additives. An appropriate amount of conductive additives can enhance the conductivity of the polymer substrate 301, which is beneficial to reduce the surface resistance of the composite current collector 100. In addition, the conductive additive is insoluble in the electrolyte and is hardly released from the polymer substrate 10. Optionally, in an embodiment of the present application, the mass proportion of the conductive additive in the polymer substrate 10 does not exceed 5%, for example, 1%-4%. Optionally, the conductive additive includes one or more carbon-based conductive materials such as carbon nanotubes, carbon fibers, graphene, graphite, acetylene black, amorphous carbon, etc.
[0045] In the embodiment of the present application, the constituent materials of the first conductive layer 20 and the second conductive layer 20' are independently selected from at least one of a metal conductive material and a carbon-based conductive material. Among them, the metal conductive material includes one or more of copper, aluminum, nickel, titanium, silver and their alloys (such as nickel-copper alloy, aluminum-zirconium alloy, etc.); the carbon-based conductive material includes one or more of carbon nanotubes, graphene, graphite, acetylene black, amorphous carbon, etc. When the composite current collector of the embodiment of the present application is used in a lithium-ion battery, the composite current collector whose conductive layer contains copper, nickel, titanium, and carbon can be used for the negative electrode of the battery; the composite current collector whose conductive layer contains aluminum or its alloy, silver or carbon can be used for the positive electrode of the battery.
[0046] In some embodiments, the first conductive layer 20 and the second conductive layer 20' may have a porous structure. The porous structure may be achieved by laser etching the conductive layer. The conductive layer having a porous structure may further reduce the weight of the current collector to increase the weight energy density of the battery, and the presence of pores in the conductive layer may also facilitate the penetration of the electrolyte into the electrode active material layer, thereby improving the wettability of the negative electrode. Exemplarily, the pores in the first conductive layer 20 may have a pore size of 1-50 μm, and the area of the pores in the first conductive layer 20 may account for 5%-50% of the total area of the first conductive layer 20.
[0047] In the embodiment of the present application, the thickness of the composite current collector 100 does not exceed 8 μm, for example, 4 μm-6 μm. Compared with pure metal foil, the composite current collector is thinner, which is more conducive to reducing the energy density of the battery and performing effective and stable electron conduction under high mechanical deformation.
[0048] In the embodiment of the present application, the surface density of the composite current collector 100 is 0.1 g / cm 2 -0.85g / cm 2 At this time, the surface density of the composite current collector is low, which helps to improve the energy density of the battery, and the mechanical properties of the composite current collector are also excellent.
[0049] In the embodiment of the present application, the tensile strength of the composite current collector 100 is greater than 300 MPa. In some embodiments, the tensile strength is greater than or equal to 340 MPa, for example, 340-380 MPa. The tensile strength of the composite current collector is higher than that of pure metal foil, and it can withstand a certain degree of tensile deformation without breaking. In addition, the tensile elongation of the composite current collector 100 can be 5%-10%.
[0050] In the embodiment of the present application, the sheet resistance of the composite current collector 100 is 1.0 mΩ / sq-3.5 mΩ / sq.
[0051] Accordingly, the present application also provides Figure 1a The preparation method corresponding to the composite current collector shown.
[0052] Reference Figure 2a The preparation method of the composite current collector comprises the following steps:
[0053] S11, coating a polymer slurry containing a polymer and a functional additive on one side surface of the carrier 200, and forming a first polymer layer 101 after drying, wherein the functional additive is soluble in the battery electrolyte and can participate in the formation of the SEI film; the bottom surface of the first polymer layer 101 is flat, and the thickness of the first polymer layer 101 gradually increases from the middle to both sides;
[0054] S12, depositing a first conductive layer 20 on a first surface of the first polymer layer 101 facing away from the carrier 200 (corresponding to the aforementioned surface 10A);
[0055] S13, peeling the first polymer layer 101 deposited with the first conductive layer 20 from the carrier 200, and coating the polymer slurry on the surface of the first polymer layer 101 away from the first conductive layer 20, and forming a second polymer layer 102 after drying, wherein the thickness of the second polymer layer 102 gradually increases from the middle to both sides;
[0056] S14, depositing a second conductive layer 20' on a second surface of the second polymer layer 102 facing away from the first polymer layer 101 (corresponding to the aforementioned surface 10B) to obtain a composite current collector 100; wherein the first polymer layer 101 and the second polymer layer 102 constitute a polymer substrate 10 of the composite current collector.
[0057] In step S11, the coating die used for coating the polymer slurry is a special die, whose liquid outlet side is not a flat surface (its two sides gradually bulge downward toward the middle), but is complementary to the shape of the first surface 10A of the desired polymer substrate 10. In this way, the thickness of the first polymer layer 101 formed on the flat carrier 200 using the special die gradually increases from the middle to the two sides. Similarly, in step S13, the coating die used to form the second polymer layer 102 is complementary to the shape of the second surface 10B of the aforementioned polymer substrate 10. When the polymer substrate 10 is an axisymmetric figure symmetrical about the horizontal plane, step S13 can be the same shape as the coating die used in step S11.
[0058] The carrier 200 may be made of a hard material such as glass, stainless steel, or polyethylene terephthalate (PET).
[0059] Among them, the first conductive layer 20 and the second conductive layer 20' can be independently prepared on the polymer substrate 10 by one or more methods such as liquid coating, vapor deposition, electroplating, and chemical plating. At this time, the conductive layer is deposited in situ on the polymer substrate, and the bonding force between the two is strong, which can ensure that the composite current collector 100 has a high structural stability. Among them, the vapor deposition method and the liquid coating method are particularly suitable for the preparation of the conductive layer made of carbon-based conductive materials; the vapor deposition method, electroplating, and chemical plating are particularly suitable for the preparation of the conductive layer made of metal conductive materials. The vapor deposition method can specifically include atomic layer deposition, physical vapor deposition, and chemical vapor deposition. Among them, the atomic layer deposition method and the physical vapor deposition method are more suitable for the preparation of the metal conductive layer. Specifically, the physical vapor deposition method can include at least one of laser pulse deposition, sputtering, evaporation, etc.; the sputtering method can specifically include magnetron sputtering, radio frequency sputtering, etc.; the evaporation method can specifically include at least one of vacuum evaporation, thermal evaporation, and electron beam evaporation. In some embodiments of the present application, the conductive layer is prepared by magnetron sputtering.
[0060] The present application embodiment also provides a Figure 1a The preparation method of the composite current collector shown in FIG. Figure 2b The preparation method of the composite current collector comprises the following steps:
[0061] S21, forming a mixture containing a polymer and a functional additive into a polymer substrate 10; wherein, along a first direction perpendicular to the thickness of the polymer substrate 10, the thickness of the polymer substrate 10 gradually increases from the middle to both sides, the polymer substrate 10 has a first surface 10A and a second surface 10B that are oppositely arranged, and the distances from the cross section of the thinnest part of the polymer substrate 10 to the first surface 10A and the second surface 10B gradually increase along the middle of the polymer substrate 10 to both sides; the functional additive is soluble in the battery electrolyte and can participate in the formation of the SEI film;
[0062] S22, depositing a first conductive layer 20 on the first surface 10A of the polymer substrate 10;
[0063] S23 , depositing a second conductive layer 20 ′ on a second surface 10B of the polymer substrate 10 facing away from the first conductive layer 20 to obtain a composite current collector 100 .
[0064] In step S21, the polymer substrate 10 can be integrally formed, and its forming method can be a common forming method such as extrusion molding, injection molding, etc. In a specific embodiment, the viscous mixed material of the polymer and the functional additive can be extruded into a molded body with a cross-section similar to the shape of the die through a specially designed extruder die under a pressurized state, and then cooled and shaped. The extruder die has a flow cavity ( Figure 2b (pointed by the arrow in the middle).
[0065] In addition, it should be noted that Figure 2b The preparation method shown is also applicable to the preparation of Figure 1b The composite current collector shown in the figure only needs to be selected with Figure 1b The extruder die can be matched with the shape of the polymer substrate.
[0066] The present application embodiment also provides a Figure 1b The preparation method of the composite current collector shown in FIG. Figure 2c The preparation method of the composite current collector comprises the following steps:
[0067] S31, coating a polymer slurry containing a polymer and a functional additive on one side surface of a carrier 200, and after drying, forming a polymer substrate 10, wherein the functional additive is soluble in a battery electrolyte and can participate in forming a SEI film; the bottom surface of the polymer substrate 10 in contact with the carrier 200 is flat, and the thickness of the polymer substrate 10 gradually increases from the middle to both sides;
[0068] S32, forming a first conductive layer 20 by deposition on a first surface of the polymer substrate 10 facing away from the carrier 200;
[0069] S33, peeling the polymer substrate 10 on which the first conductive layer 20 is deposited from the carrier 200, and depositing a second conductive layer 20' on a second surface of the polymer substrate 10 away from the first conductive layer 20 to obtain a composite current collector.
[0070] in, Figure 2c The preparation method shown is Figure 2a They are very similar, except that the shapes of the polymer substrates are different and the number of coatings is different. Figure 2a The polymer substrate is formed by two coating processes. Figure 2c The polymer substrate is formed by one coating. Accordingly, the conductive layers formed in the above two are slightly different.
[0071] The preparation method of the composite current collector provided in the embodiment of the present application has a simple process, and the prepared composite current collector has a stable structure and can effectively play a role in improving the battery cycle performance and energy density.
[0072] The embodiment of the present application also provides an electrode plate using the composite current collector, which can be a positive electrode plate or a negative electrode plate. Figure 3 A schematic diagram of the structure of a negative electrode sheet is shown. The negative electrode sheet 30 includes the aforementioned composite electrode current collector 100 and a negative electrode active material layer 31 disposed on the first conductive layer 20 and the second conductive layer 20 ′ of the composite electrode current collector 100 .
[0073] The negative electrode sheet 30 has a high production yield due to the use of the composite current collector 100. Using it in a battery can help effectively improve the cycle performance and energy density of the battery. Figure 3 The negative electrode sheet shown is only the one using the above Figure 1a The composite current collector shown is an example, but is not limited to only Figure 1a In addition, the positive electrode sheet using the composite current collector is Figure 3 The negative electrode sheet shown is similar, the main difference being that located above the two conductive layers is a layer of positive active material.
[0074] See also Figure 4 , the present application also provides a schematic diagram of the structure of a battery. The battery 400 includes the aforementioned negative electrode sheet 30, the positive electrode sheet 40, and a separator 30 and an electrolyte (not shown) located between the negative electrode sheet 30 and the positive electrode sheet 40. Among them, the positive electrode sheet 40 may include a positive electrode current collector 401 and a positive electrode active material layer 41 disposed on the opposite sides of the positive electrode current collector 401. It should be noted that, Figure 4 In the figure, only the composite current collector 100 is used as the current collector of the negative electrode plate. In other embodiments of the present application, the composite current collector may be used as the positive electrode current collector of the positive electrode plate 40, or both the positive electrode plate and the negative electrode plate may use the composite current collector. Since the battery's electrode plate and / or positive electrode plate include the composite current collector described above, the battery may have a longer cycle life and a higher energy density.
[0075] The battery 400 of the present application may be of a winding type or a laminated type. The battery 400 may be any one of a lithium secondary battery, a sodium secondary battery, a potassium secondary battery, a magnesium secondary battery, a zinc secondary battery, etc. For a lithium-ion battery, its negative electrode active material may include at least one of metallic lithium, graphite, silicon-based materials (including elemental silicon, silicon alloys, silicon oxides, silicon-carbon composite materials), tin-based materials (including elemental tin, tin oxides, tin-based alloys), lithium titanate, etc.; its positive electrode active material may specifically be at least one of lithium iron phosphate (LiFePO4), lithium manganese phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium vanadium phosphate, lithium cobalt acid, lithium manganate, lithium nickel acid, lithium vanadate, lithium manganese nickel acid, lithium manganate, lithium-rich manganese-based materials, lithium nickel cobalt manganate, and lithium nickel cobalt aluminum acid.
[0076] The following further describes the embodiments of the present application in multiple embodiments. The embodiments of the present application are not limited to the following specific embodiments. The embodiments can be appropriately modified without changing the scope of the main rights of the present application.
[0077] Example 1
[0078] A method for preparing a composite current collector, see Figure 2a , including the following steps:
[0079] (1) 45 g of polyimide (Kukdo Chemical, Korea, molecular weight 23800) and 5 g of lithium nitrate were added to 500 mL of N-methylpyrrolidone (NMP), and the mixture was stirred at 60° C. for 24 hours to obtain a polymer slurry;
[0080] (2) The polymer slurry of step (1) is coated with a coating machine with a special die head (made by Fudi Battery Co., Ltd., such as Figure 2a The NMP was coated on a PET carrier base film with a thickness of 10 μm, and then transferred to a continuous oven at 80° C., 90° C., 100° C., 110° C. and 120° C. for drying to dry the NMP to obtain a first polymer layer with a middle thickness of 0.5 μm and an edge thickness of 2 μm;
[0081] (3) The PET carrier film with the first polymer layer was placed in a vacuum magnetron sputtering coating machine (Shenyang Ke Instrument Co., Ltd., model FJL560), and the vacuum degree of the sputtering chamber was evacuated by a vacuum pump to 8×10 -2 Pa, and then a certain amount of high-purity argon gas is introduced to adjust the vacuum degree to 2×10 -1 Pa, then the first polymer layer is cleaned by a surface ion source for 5 minutes, and after the cleaning is completed, the ion source power is turned off; then the copper plating power is started to magnetron sputter plate a metal copper layer on the surface of one side of the first polymer, wherein the sputtering time of the metal copper layer is 10 minutes, and the middle thickness of the obtained copper layer is 2 μm and the edge thickness is 0.5 μm;
[0082] (4) peeling the first polymer layer on which the copper layer is deposited from the PET carrier base film, and placing the first polymer layer upward, coating the polymer slurry on the surface of the first polymer layer away from the copper layer according to the method described in step (2), and forming a second polymer layer after drying, wherein the middle thickness is 0.5 μm and the edge thickness is 2 μm; then forming a copper film with a middle thickness of 2 μm and an edge thickness of 0.5 μm on the second polymer layer according to the method described in step (3), thereby completing the preparation of the composite current collector;
[0083] Wherein, the above steps (1)-(4) are all carried out in a dry environment with a dew point of -50°C.
[0084] The first polymer layer and the second polymer layer constitute the polymer substrate 10 of the composite current collector in Example 1, and the middle thickness of the polymer substrate is 1 μm and the edge thickness is 4 μm. The porosity of the polymer substrate 10 is 10%, and the pore size is 1 μm-10 μm. The total thickness of the composite current collector prepared in Example 1 is 5 μm. The composite current collector is cut into samples with a size of 10 cm*10 cm, and its tensile strength is measured by Junrui's electronic universal testing machine to be 363 MPa.
[0085] Example 2
[0086] A method for preparing a composite current collector, which differs from Example 1 in that the polyimide in step (1) of Example 1 is replaced by polyvinylidene fluoride (PVDF-HFP) of equal mass.
[0087] The composite current collector prepared in Example 2 has a structure as follows: Figure 1a As shown, it includes a polymer substrate and conductive layers arranged on the surfaces of the two opposite sides of the polymer substrate; wherein the polymer substrate contains PVDF-HFP and lithium nitrate, and the mass percentage of lithium nitrate in the polymer substrate is 10wt%; the middle thickness of the polymer substrate is 1μm, and the edge thickness is 4μm; the middle thickness of each conductive layer is 2μm, and the edge thickness is 0.5μm, and all are copper layers.
[0088] The total thickness of the composite current collector prepared in Example 2 is 5 μm. The composite current collector is cut into samples with a size of 10 cm*10 cm, and the tensile strength thereof is measured by an electronic universal testing machine of Junrui Company and is 342 MPa.
[0089] Example 3
[0090] A composite current collector is different from the embodiment 1 in that: the polymer substrate contains silver nitrate instead of lithium nitrate; and the polymer constituting the polymer substrate is not polyimide but PVDF-HFP.
[0091] The composite current collector of Example 3 can be Figure 2b The composite current collector of Example 3 was prepared according to the process flow chart shown in the figure. After testing, the tensile strength of the composite current collector of Example 3 was 340 MPa.
[0092] Example 4
[0093] A composite current collector having a structure as Figure 1aAs shown, it includes a polymer substrate and conductive layers arranged on the opposite side surfaces of the polymer substrate; wherein the polymer substrate contains polyimide and magnesium nitrate [Mg(NO3)2], and the mass percentage of Mg(NO3)2 in the polymer substrate is 10wt%; the middle thickness of the polymer substrate is 2μm, and the edge thickness is 3μm; each conductive layer is a copper layer, the middle thickness is 1.5μm, and the edge thickness is 1μm.
[0094] The total thickness of the composite current collector of Example 4 is about 5 μm. According to the test, the tensile strength of the composite current collector of Example 4 is 355 MPa.
[0095] Example 5
[0096] A composite current collector, which is different from Example 1 in that the mass percentage of lithium nitrate contained in the polymer substrate is 5wt%.
[0097] After testing, the tensile strength of the composite current collector of Example 5 is 365 MPa.
[0098] Example 6
[0099] A composite current collector, which is different from Example 1 in that the mass percentage of lithium nitrate contained in the polymer substrate is 20wt%.
[0100] After testing, the tensile strength of the composite current collector of Example 6 is 347 MPa.
[0101] Example 7
[0102] A composite current collector, which is different from Example 1 in that the mass percentage of lithium nitrate contained in the polymer substrate is 40wt%.
[0103] After testing, the tensile strength of the composite current collector of Example 7 is 345 MPa.
[0104] Example 8
[0105] A composite current collector, the structural schematic diagram of which is shown in Figure 1b As shown, it includes a polymer substrate and a first conductive layer and a second conductive layer arranged on two opposite sides of the polymer substrate; wherein the polymer substrate contains polyimide and lithium nitrate, and the mass percentage of lithium nitrate in the polymer substrate is 10wt%; the middle thickness of the polymer substrate is 0.5μm, and the edge thickness is 2μm; the first conductive layer and the second conductive layer are both copper layers, wherein the middle thickness of the first conductive layer is 2μm, the edge thickness is 0.5μm, and the thickness of the second conductive layer is uniform, which is 2.5μm.
[0106] The composite current collector of Example 8 can be Figure 2cThe composite current collector of Example 8 has a total thickness of about 5 μm. According to the test, the tensile strength of the composite current collector of Example 8 is 356 MPa.
[0107] Example 9
[0108] A composite current collector, which differs from Example 1 in that: the polymer substrate further contains 5 wt% of carbon nanotubes.
[0109] After testing, the tensile strength of the composite current collector of Example 9 is 373 MPa.
[0110] In addition, in order to highlight the beneficial effects of the technical solution of the present application, the following comparative example is set.
[0111] Comparative Example 1
[0112] A method for preparing a composite current collector, which is different from Example 1 in that the polymer slurry in step (1) does not contain lithium nitrate.
[0113] Comparative Example 2
[0114] A method for preparing a composite current collector, which differs from Example 1 in that: in step (2), a conventional die is used to coat the polymer slurry, and the thickness of the obtained polymer substrate is uniform and the thickness is 1.25 μm. Subsequently, copper conductive layers with uniform thickness of 1.25 μm are deposited on the opposite sides of the polymer substrate.
[0115] To further support the beneficial effects of the embodiments of the present application, the composite current collectors of the above embodiments and comparative examples are made into negative electrode sheets and used in lithium-ion full batteries. The following takes the composite current collector of embodiment 1 as an example to introduce a method for preparing a lithium-ion full battery, which specifically includes the following steps:
[0116] (1) Preparation of positive electrode sheets for lithium-ion batteries
[0117] 49.2 g of positive electrode active material (specifically LiFePO4) was mixed with 0.4 g of conductive agent (acetylene black) and 0.4 g of binder (polyvinylidene fluoride, PVDF) in N-methylpyrrolidone (NMP), and stirred at 1000 rpm for 12 h to obtain a uniform positive electrode slurry, which was evenly coated on both sides of the current collector aluminum foil to control the surface density to 214 g / m 2 , and then dried at 80°C, and rolled by a roller press to obtain a positive electrode sheet Z', which was then cut into a positive electrode sheet Z with a size of 21×42mm; and one of the sheets was cut into a 13mm diameter disc to assemble into a button battery for capacity calibration, and the calibrated capacity was 6mAh / cm 2 .
[0118] (2) Preparation of negative electrode sheets for lithium-ion batteries
[0119] The composite current collector of Example 1 was transferred into a thermal evaporator (Shenyang Keyi, China, model DZ270) and the vacuum pump was evacuated until the vacuum degree of the chamber reached 4×10 -1 After Pa, the temperature is raised to 300°C, and metallic lithium is deposited on the surfaces of both sides of the current collector. The deposition time is 10 minutes and the deposition thickness is about 5 μm. After the deposition is completed, the cavity is cooled to 100°C, the vacuum is turned off, and the negative electrode sheet is taken out after cooling to room temperature.
[0120] (3) The positive electrode sheet Z, the separator, the negative electrode sheet and the positive electrode sheet are stacked layer by layer to assemble a laminated cell, and 2.2 mL / Ah of electrolyte is added dropwise, and after packaging, a full battery is obtained. The electrolyte contains lithium nitrate, lithium bis(fluorosulfonyl)imide (LiFSI) and ethylene glycol dimethyl ether (DME), the molar concentration of LiFSI in the electrolyte is 4 mol / L, and the mass fraction of lithium nitrate in the electrolyte is 1 wt%.
[0121] The following electrochemical performances of each full cell were tested.
[0122] 1) Cycle performance test: Take 5 full batteries of each embodiment and comparative example, and perform charge and discharge cycle test at 0.2C on LAND CT 2001C secondary battery performance test device at 25℃. The steps are as follows: leave for 10min; charge at 0.2C constant current to 3.8V, charge at constant voltage to 3.8V / 0.05C and cut off; leave for 10min; discharge at 0.5C to 2.7V, which is 1 cycle. Repeat the charge and discharge cycle steps. When the capacity of the battery is lower than 80% of the initial discharge capacity during the cycle, the cycle is terminated. The number of cycles is the cycle life of the battery. The average value of each group is taken, and it is summarized in the following Table 1 together with the average initial discharge capacity of the battery and the thickness change rate before and after the battery cycle. In addition, an impedance (EIS) test (amplitude 5mV, frequency 1000-0.01Hz) is performed every 5 cycles during the first 40 cycle tests. The experimental results are shown in Table 2.
[0123] 2) Nitrate ion test in the electrolyte during the cycle: 10 full batteries of each embodiment and comparative example were taken, and one battery from each group of full batteries was disassembled after the 1st, 5th, 10th, 15th, 20th, 25th, 30th, 50th, 100th and 150th cycles, and the residual electrolyte was extracted. The nitrate ion content in the residual electrolyte was tested by ultraviolet spectrophotometry (Shanghai Kuncheng Scientific Instrument, UV7504). The test results are summarized in Table 3 below.
[0124] 3) Rate test: ① Take 2 full batteries from each embodiment and comparative example, set aside for 5 minutes; charge at 0.5C constant current to 3.8V, charge at constant voltage to 0.05C and cut off; set aside for 10 minutes; then discharge at 0.5C to 2.7V, which is 1 cycle, repeat this step. When the battery capacity is lower than 80% of the initial discharge capacity during the cycle, the cycle is terminated. The number of cycles is the cycle life of the battery. Take the average value for each group, and this parameter is the data of the average initial discharge capacity of the battery. ② Take another 2 batteries to repeat the above experimental test ①, and change the charge and discharge rate from 0.5C to 1C. ③ Take another 2 batteries to repeat the above experimental test ①, and change the charge and discharge rate from 0.5C to 1.5C. ④ Take another 2 batteries to repeat the above experimental test ①, and change the charge and discharge rate from 0.5C to 2C. ⑤ Take another 2 batteries to repeat the above experimental test ①, and change the charge and discharge rate from 0.5C to 3C. ⑥Take another 2 batteries and repeat the above ① experiment test, changing the charge and discharge rate from 0.5C to 5C. The relevant experimental results are shown in Table 4.
[0125] Table 1 Average first discharge capacity of each full battery and battery thickness change rate before and after cycling
[0126]
[0127] Table 2 Battery impedance data of each full battery after every 5 cycles
[0128]
[0129]
[0130] Table 3 Summary of nitrate content in the electrolyte of each full battery after different cycle times
[0131]
[0132] Table 4 Summary of rate properties of each full battery
[0133]
[0134]
[0135] It can be seen from Table 1 that the full batteries of the embodiments of the present application all show a high cycle life and low volume expansion. It can be seen from Table 2 that the impedance of the full batteries of the embodiments of the present application is low during the cycle, indicating that a relatively stable interface impedance is obtained. It can be seen from Table 3 that as the cycle proceeds, the lithium nitrate in the electrolyte participates in the film-forming reaction, but since a certain nitrate additive is pre-stored in the composite current collector in the embodiments of the present application, it can be added to the electrolyte in time, so the battery of the embodiments of the present application is relatively stable during the cycle. It can be seen from Table 4 that the full batteries of the embodiments of the present application show good rate performance, which is attributed to the good cycle interface stability and low interface impedance brought by the composite current collector of the polymer substrate + conductive layer on the one hand, and on the other hand, based on the special shape of the polymer substrate in the composite current collector, the functional additives pre-stored therein can replenish the concentration of lithium in the lithium deposition area in time, shortening the transmission path of lithium ions, which is conducive to improving the rate performance of the battery.
[0136] The above only expresses several exemplary embodiments of the present application, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present application. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present application, which all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be based on the attached claims.
Claims
1. A composite current collector, characterized in that: It includes a polymer substrate, a first conductive layer arranged on the first surface of the polymer substrate and a second conductive layer on the second surface, the first surface and the second surface are arranged opposite to each other, wherein the polymer substrate contains a polymer and a functional additive, the functional additive is soluble in the battery electrolyte and can participate in the formation of an SEI film; along a first direction perpendicular to the thickness of the composite current collector, the thickness of the polymer substrate gradually increases from the middle to the edge, and the first direction is the length direction or the width direction of the composite current collector.
2. The composite current collector according to claim 1, characterized in that: Along a first direction perpendicular to the thickness of the composite current collector, the thickness of one of the first conductive layer and the second conductive layer gradually decreases from the middle to the edge, and the thickness of the other remains unchanged from the middle to the edge.
3. The composite current collector according to claim 1, characterized in that: The distances of the cross section of the thinnest part of the polymer substrate along the horizontal direction from the first surface and the second surface gradually increase from the middle to the edge of the polymer substrate.
4. The composite current collector according to claim 3, characterized in that: Along the first direction, the thicknesses of the first conductive layer and the second conductive layer gradually decrease from the middle to the edge.
5. The composite current collector according to claim 3, characterized in that: The polymer substrate has a middle thickness of 0.1 μm to 7.9 μm and an edge thickness of 1 μm to 7.99 μm.
6. The composite current collector according to claim 4, characterized in that: The middle thickness of the first conductive layer and the second conductive layer are both within the range of 0.05 μm-3.95 μm, and the edge thickness are both within the range of 5 nm-3.5 μm.
7. The composite current collector according to claim 1 or 3, characterized in that: The thickness of the composite current collector does not exceed 8 μm.
8. The composite current collector according to claim 1, characterized in that: The functional additives include one or more of lithium nitrate, magnesium nitrate, silver nitrate, lithium bis(oxalatoborate), and lithium difluorooxalatoborate.
9. The composite current collector according to claim 8, characterized in that: The functional additive accounts for 5%-40% by weight in the polymer substrate.
10. The composite current collector according to claim 1, characterized in that: The polymer substrate has a porous structure.
11. The composite current collector according to claim 1, characterized in that: The polymer matrix also contains a conductive additive.
12. The composite current collector according to claim 1, characterized in that: The first conductive layer and the second conductive layer have a porous structure.
13. An electrode plate, characterized in that: The electrode plate includes the composite current collector according to any one of claims 1 to 12 and an electrode active material layer formed on the first conductive layer and the second conductive layer.
14. A battery, characterized in that: The battery comprises a positive electrode sheet, a negative electrode sheet, and a separator and an electrolyte located between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet and / or the negative electrode sheet comprises the electrode sheet as claimed in claim 13.
15. A method for preparing a composite current collector, characterized in that: The following steps are involved: A polymer slurry containing a polymer and a functional additive is coated on one side of a carrier, and after drying, a polymer substrate is formed, wherein the functional additive is soluble in a battery electrolyte and can participate in the formation of an SEI film; the bottom surface of the polymer substrate in contact with the carrier is flat, and along the length direction or the width direction of the polymer substrate, the thickness of the polymer substrate gradually increases from the middle to the edge; Depositing a first conductive layer on a first surface of the polymer substrate facing away from the carrier; The polymer substrate on which the first conductive layer is deposited is peeled off from the carrier, and a second conductive layer is deposited on a second surface of the polymer substrate away from the first conductive layer to obtain a composite current collector.
16. A method for preparing a composite current collector, characterized in that: The following steps are involved: A polymer slurry containing a polymer and a functional additive is coated on one side of a carrier, and after drying, a first polymer layer is formed, wherein the functional additive is soluble in a battery electrolyte and can participate in forming a SEI film; the bottom surface of the first polymer layer is flat, and along the length or width direction of the first polymer layer, the thickness of the first polymer layer gradually increases from the middle to the edge; Depositing a first conductive layer on a first surface of the first polymer layer facing away from the carrier; The first polymer layer on which the first conductive layer is deposited is peeled off from the carrier, and the polymer slurry is coated on the surface of the first polymer layer away from the first conductive layer, and a second polymer layer is formed after drying, wherein the thickness of the second polymer layer gradually increases from the middle to the edge along the length or width direction of the second polymer layer; A second conductive layer is deposited on a second surface of the second polymer layer facing away from the first polymer layer to obtain a composite current collector; wherein the first polymer layer and the second polymer layer constitute a polymer substrate of the composite current collector.
17. A method for preparing a composite current collector, characterized in that: The following steps are involved: A mixture containing a polymer and a functional additive is formed into a polymer substrate; wherein, along a first direction perpendicular to the thickness of the polymer substrate, the first direction being the length direction or the width direction of the polymer substrate, the thickness of the polymer substrate gradually increases from the middle to the edge; the functional additive is soluble in the battery electrolyte and can participate in the formation of the SEI film; A first conductive layer and a second conductive layer are deposited on opposite side surfaces of the polymer substrate to obtain a composite current collector.