A method for regulating residual stress in low carbon steel by enhancing Mn partitioning plasticity
Through pre-deformation and Mn distribution stress relief technology, the precipitation of alloy carbides and the accumulation of Mn at the α and θ phase interface are promoted, which solves the problem of insufficient residual stress after tempering of low carbon microalloy steel and achieves efficient stress reduction of low carbon steel. and material performance improvements.
Patent Information
- Application Number
- CN202211086972.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-07
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-09-07
AI Technical Summary
Low carbon microalloy steel has insufficient residual stress relaxation during the tempering process, resulting in the risk of distortion in the material during downstream processing and use, affecting its service performance.
Before tempering, pre-deformation is used to suppress cementite precipitation and promote the formation of alloy carbides. Mn is used to induce plastic strain in three forms during the Mn distribution process. The Mn distribution stress relief stage is set, which is divided into rapid temperature rise, surface and core. During the soaking, slow heating and cooling stages, alloy carbides are induced to precipitate and Mn accumulates at the α and θ phase interface, thereby enhancing the plastic strain relaxation ability.
It effectively reduces the initial stress of low carbon steel by about 80%, significantly improves the service performance of the material, and reduces the risk of distortion in downstream processing.
Smart Images

Figure CN115584378B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of heat treatment of metal materials, and in particular relates to a method for regulating residual stress of low-carbon steel for enhancing Mn partitioning plasticity. Background Art
[0002] High-strength and ultra-high-strength steel plates are key basic materials for the manufacture of large-scale engineering equipment, which directly determine the accuracy and life of the equipment. Driven by the demand for large-scale and lightweight engineering equipment, the strength of steel plates has increased from the traditional 345-700MPa to 1000-2000MPa. Quenching is the most important technical means to improve the strength and hardness of materials. The interaction between temperature stress and organizational transformation during the quenching process introduces high-amplitude residual stress into the material, resulting in material distortion, fatigue damage, stress corrosion and delayed cracking, which seriously restricts the development of advanced basic materials and high-end manufacturing industries. Tempering is the most critical technical means to improve quenching residual stress, but after tempering, the residual stress level of many materials is still very high, and the material is still prone to distortion during the downstream preparation process. The impact of residual stress on the service performance of the material is difficult to fundamentally improve.
[0003] Low-carbon, micro-alloyed high-strength steels with a carbon content of less than 0.08wt% have gradually become the most widely used basic materials in high-strength structural steels due to their low material cost and excellent welding performance. However, it is precisely because of the relatively low content of C and alloying elements such as Ti and Nb that the amount of carbide precipitation during the tempering process of the above-mentioned low-carbon micro-alloyed steel is low, and the plastic strain generated by the precipitation of carbides is correspondingly small, resulting in this type of high-strength structural steel being difficult to relax the residual stress with the help of the plastic strain generated by the precipitation of carbides. After tempering, the residual stress of many low-carbon steels is still as high as 60% of the initial residual stress. After tempering, low-carbon steels still have the risk of distortion during downstream striping, welding, and bending processes, and the degree of improvement of the service performance of low-carbon steels by tempering is limited. Therefore, how to improve the residual stress of low-carbon micro-alloyed steels is a key technical bottleneck that needs to be broken through in both theoretical research and actual production.
[0004] Some studies have suggested that, during the tempering process, the residual stress in the organization can be relaxed by using the plastic strain generated by the Mn partitioning process, which can increase the relaxation of residual stress in the tempering process of low-carbon microalloyed steel from 40% to ≥60%, thereby improving the service performance of low-carbon steel. However, for some products with unsatisfactory residual stress distribution during hot rolling and "N" type distribution of residual stress in the thickness direction of the strip, the plastic strain generated by the Mn partitioning process of low-carbon microalloyed steel is still low, and the relaxation of residual stress is still insufficient, so there is still a risk of distortion during downstream processing and use. Summary of the invention
[0005] Aiming at the problem that the plastic strain generated in the Mn partitioning process of low carbon microalloy steel is still low and the relaxation of residual stress is insufficient, the present invention provides a low carbon steel residual stress control method for enhancing Mn partitioning plasticity, which can reduce the initial stress in the low carbon steel by about 80%.
[0006] The technical solution adopted by the present invention is:
[0007] A method for regulating residual stress of low carbon steel for enhancing Mn partitioning plasticity, wherein for low carbon microalloy steel with low carbon content and weak plastic behavior caused by carbide precipitation, pre-deformation is used to inhibit cementite precipitation before tempering, so as to promote the formation of more alloy carbides in the matrix structure; a Mn partitioning stress relief stage is set before the cooling stage of the tempering process, and the plastic strain generated by the Mn partitioning process is used to relax the residual stress in the structure, and Mn induces plastic strain in three forms, namely, Mn partitioning between alloy carbides and matrix structure, Mn aggregation at the interface between alloy carbides and matrix structure, and Mn inducing C aggregation at the interface between alloy carbides and matrix structure.
[0008] Furthermore, the deformation amount of the pre-deformation is 0.3%-5%.
[0009] Furthermore, pre-deformation is performed by a leveling unit.
[0010] Furthermore, in the Mn partitioning stress relief stage, the hot-rolled strip or steel plate heated to 650°C is kept warm for 2-30 minutes to induce the Mn on the surface and core of the material to simultaneously aggregate at the α and θ phase interfaces, and gradually complete the partitioning of Mn between the α and θ phases, thereby strengthening the plastic strain generated inside the material during the Mn partitioning process and enhancing the ability to relax residual stress during the tempering process.
[0011] Furthermore, the entire tempering process is divided into a rapid heating stage, a surface-core soaking stage, a slow heating stage, a Mn partitioning stress relief stage and a cooling stage in sequence; in the rapid heating stage, the hot-rolled strip or steel plate is rapidly heated at the highest heating rate, thereby inducing the formation of sufficient alloy carbide precipitation sites in the structure; in the surface-core soaking stage, the rapidly heated hot-rolled strip or steel plate is kept warm for a certain period of time, thereby making the surface and core of the material soaked; in the slow heating stage, the hot-rolled strip or steel plate is heated to 650°C at a low heating rate, thereby ensuring that the temperature difference between the surface and the core of the material is below a certain level.
[0012] Furthermore, in the rapid heating stage, the hot-rolled strip or steel plate is rapidly heated to 500°C-550°C at the highest heating rate, and in the surface core equalization stage, the hot-rolled strip or steel plate at 500°C-550°C is kept warm for 2-15 minutes.
[0013] Furthermore, during the slow heating stage, the temperature difference between the material surface and the core is ensured to be less than 50°C.
[0014] The beneficial effects of the present invention are:
[0015] The present invention utilizes pre-deformation to promote the formation of more alloy carbides in the matrix structure, utilizes Mn in three forms to induce plastic strain in the Mn partitioning process to relax the residual stress in the structure, and can reduce the initial stress in the low carbon steel by about 80%. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the effect of no pre-deformation and 3% pre-deformation on Mn distribution in the present invention.
[0017] Figure 2 3 is a comparative diagram of the improvement of residual stress by different tempering methods in Example 1 of the present invention, in which (a), (b), and (c) are the residual stress using this method, the residual stress using Mn partitioning but without pre-deformation, and the initial residual stress, respectively.
[0018] Figure 3 3 is a comparison diagram of the improvement of residual stress by different tempering methods in Example 2 of the present invention, in which (a), (b), and (c) are the residual stress using this method, the residual stress using Mn partitioning but without pre-deformation, and the initial residual stress, respectively. DETAILED DESCRIPTION
[0019] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0020] A method for regulating residual stress of low carbon steel to enhance Mn partitioning plasticity. For low carbon microalloy steel with low carbon content and weak plastic behavior caused by carbide precipitation, pre-deformation is used to inhibit cementite precipitation before tempering to promote the formation of more alloy carbides in the matrix structure, such as Figure 1 As shown in the figure, a Mn distribution stress relief stage is set before the cooling stage of the tempering process, and the plastic strain generated by the Mn distribution process is used to relax the residual stress in the structure. Mn induces plastic strain in three forms, namely, Mn distribution between alloy carbides and matrix structures, Mn aggregation at the interface of alloy carbides and matrix structures, and Mn induces C aggregation at the interface of alloy carbides and matrix structures. The present invention utilizes pre-deformation to promote the formation of more alloy carbides in the matrix structure, and utilizes Mn to induce plastic strain in three forms in the Mn distribution process to relax the residual stress in the structure, which can reduce the initial stress in low-carbon steel by about 80%.
[0021] In the present invention, the pre-deformation amount is 0.3%-5%, and the pre-deformation is performed by a flattening unit.
[0022] In the present invention, during the Mn partitioning stress relief stage, the hot-rolled strip or steel plate heated to 650°C is kept warm for 2-30 minutes to induce the Mn on the surface and core of the material to simultaneously aggregate at the α and θ phase interfaces, and gradually complete the partitioning of Mn between the α and θ phases, thereby strengthening the plastic strain generated inside the material during the Mn partitioning process and enhancing the relaxation ability of the residual stress during the tempering process.
[0023] In the present invention, the entire tempering process is divided into a rapid heating stage, a surface-core soaking stage, a slow heating stage, a Mn partitioning stress relief stage and a cooling stage in sequence; in the rapid heating stage, the hot-rolled strip or steel plate is rapidly heated at the highest heating rate, thereby inducing the formation of sufficient alloy carbide precipitation sites in the structure; in the surface-core soaking stage, the rapidly heated hot-rolled strip or steel plate is kept warm for a certain period of time, thereby making the surface and core of the material soaked; in the slow heating stage, the hot-rolled strip or steel plate is heated to 650°C at a low heating rate, thereby ensuring that the temperature difference between the surface and the core of the material is below a certain level.
[0024] In the present invention, in the rapid heating stage, the hot-rolled strip or steel plate is rapidly heated to 500°C-550°C at the highest heating rate; in the surface core equalization stage, the hot-rolled strip or steel plate at 500°C-550°C is kept warm for 2-15 minutes; in the slow heating stage, the temperature difference between the surface and the core of the material is ensured to be less than 50°C.
[0025] Embodiment 1
[0026] The thickness is 4 mm, the C content is 0.07wt%, and the Mn content is 1.88wt%. Low carbon microalloy steel, such as Figure 2 As shown in (c), the maximum residual stress of the hot-rolled steel plate along the thickness direction is 360MPa.
[0027] When the Mn partitioning method is used without pre-deformation, such as Figure 2 As shown in (b), the maximum residual stress along the thickness direction of the hot-rolled steel plate is 142 MPa, which is 39.4% of the value before tempering. The improvement of residual stress is still insufficient.
[0028] When adopting this method: firstly, the hot-rolled steel plate is subjected to 1% pre-deformation treatment through a flattening unit. Then, the tempering treatment is carried out. In the rapid heating stage and the surface and core equalization stage, the tempering furnace is heated to 550°C, and the hot-rolled steel plate is directly placed in the tempering furnace and kept warm for 2 minutes, so as to induce the formation of sufficient alloy carbide precipitation sites in the organization and make the surface and core of the material equalized; in the slow heating stage, the hot-rolled steel plate is heated from 550°C to 650°C at a heating rate of 1°C / s, and the temperature difference between the surface and the core of the material is ensured to be less than 50°C during the heating process; in the Mn partitioning and stress relief stage, the 650°C hot-rolled steel plate is kept warm for 2 minutes, so as to induce the Mn on the surface and the core of the material to gather synchronously at the interface of α and θ phases, and gradually complete the partitioning of Mn between α and θ phases, strengthen the plastic strain generated inside the material during the Mn partitioning process, and enhance the relaxation ability of the residual stress during the tempering process; in the cooling stage, the hot-rolled steel plate is taken out of the tempering furnace and air-cooled to room temperature.
[0029] After adopting this method, the stress and material properties are measured, such as Figure 2 As shown in (a), the residual stress in the hot-rolled steel sheet is reduced to 78 MPa, which is 21.7% of that before tempering.
[0030] Embodiment 2
[0031] The thickness is 4 mm, the C content is 0.07wt%, and the Mn content is 1.88wt%. Low carbon microalloy steel, such as Figure 3 As shown in (c), the maximum residual stress of the hot-rolled steel plate along the thickness direction is 360MPa.
[0032] When the Mn partitioning method is used without pre-deformation, such as Figure 3 As shown in (b), the maximum residual stress along the thickness direction of the hot-rolled steel plate is 142 MPa, which is 39.4% of the value before tempering. The improvement of residual stress is still insufficient.
[0033] When adopting this method: firstly, the hot-rolled steel plate is subjected to 5% pre-deformation treatment through a flattening unit. Then, the tempering treatment is carried out. In the rapid heating stage and the surface and core equalization stage, the tempering furnace is heated to 550°C, and the hot-rolled steel plate is directly placed in the tempering furnace and kept warm for 2 minutes, so as to induce the formation of sufficient alloy carbide precipitation sites in the organization and make the surface and core of the material equalized; in the slow heating stage, the hot-rolled steel plate is heated from 550°C to 650°C at a heating rate of 1°C / s, and the temperature difference between the surface and the core of the material is ensured to be less than 50°C during the heating process; in the Mn partitioning and stress relief stage, the 650°C hot-rolled steel plate is kept warm for 2 minutes, so as to induce the Mn on the surface and the core of the material to gather synchronously at the interface of α and θ phases, and gradually complete the partitioning of Mn between α and θ phases, strengthen the plastic strain generated inside the material during the Mn partitioning process, and enhance the relaxation ability of the residual stress during the tempering process; in the cooling stage, the hot-rolled steel plate is taken out of the tempering furnace and air-cooled to room temperature.
[0034] After adopting this method, the stress and material properties are measured, such as Figure 3 As shown in (a), the residual stress in the hot-rolled steel sheet is reduced to 73 MPa, which is 20.3% of that before tempering.
[0035] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
Claims
1. A method for regulating residual stress of low carbon steel for enhancing Mn partitioning plasticity, characterized in that: For low-carbon microalloy steels with low carbon content and weak plastic behavior caused by carbide precipitation, pre-deformation is used to inhibit cementite precipitation before tempering to promote the formation of more alloy carbides in the matrix structure; a Mn partitioning stress relief stage is set before the cooling stage of the tempering process, and the plastic strain generated by the Mn partitioning process is used to relax the residual stress in the structure. Mn induces plastic strain in three forms, namely, Mn partitioning between alloy carbides and matrix structures, Mn aggregation at the interface between alloy carbides and matrix structures, and Mn inducing C aggregation at the interface between alloy carbides and matrix structures; pre-deformation is carried out through a leveling unit.
2. The method for controlling residual stress of low carbon steel for enhancing Mn partitioning plasticity according to claim 1, characterized in that: The deformation amount of pre-deformation is 0.3%-5%.
3. The method for controlling residual stress of low carbon steel for enhancing Mn partitioning plasticity according to claim 1, characterized in that: During the Mn partitioning stress relief stage, the hot-rolled steel plate heated to 650 °C is kept warm for 2-30 min to induce the Mn on the surface and core of the material to simultaneously aggregate at the interface between the α and θ phases, and gradually complete the partitioning of Mn between the α and θ phases, thereby strengthening the plastic strain generated inside the material during the Mn partitioning process and enhancing the relaxation ability of residual stress during the tempering process.
4. The method for controlling residual stress of low carbon steel for enhancing Mn partitioning plasticity according to claim 3, characterized in that: The entire tempering process is divided into a rapid heating stage, a surface-core soaking stage, a slow heating stage, a Mn partitioning stress relief stage and a cooling stage; in the rapid heating stage, the hot-rolled steel plate is rapidly heated at the highest heating rate to induce the formation of sufficient alloy carbide precipitation sites in the structure; in the surface-core soaking stage, the rapidly heated hot-rolled steel plate is kept warm for a certain period of time to make the surface and core of the material soaked; in the slow heating stage, the hot-rolled steel plate is heated to 650°C at a low heating rate to ensure that the temperature difference between the surface and the core of the material is below a certain level; In the rapid heating stage, the hot-rolled steel plate is rapidly heated to 500℃-550℃ at the highest heating rate. In the surface and core equalization stage, the hot-rolled steel plate at 500℃-550℃ is kept warm for 2-15 min. In the slow heating stage, the temperature difference between the surface and the core of the material is ensured to be less than 50℃.
Citation Information
Patent Citations
Building steel plate and production method thereof
CN109930071A
Tempering method for reducing residual stress
CN110527792A
Low-temperature residual stress regulation and control method for hot-rolled high-strength strip steel
CN110527808A
Low-carbon medium-manganese high-residual-austenite high-strength and high-toughness steel and heat treatment method thereof
CN112063931A
Rolling element and method of producing the same
US20040256029A1