Transparent substrate with anti-reflective film

By adopting a multi-layer film structure in the anti-reflection film of the image display device, combining silicon oxide and mixed oxide layers, the transmittance change problem caused by external intrusion of moisture is solved, and higher density and aesthetics are achieved.

CN115734951BActive Publication Date: 2024-11-29AGC INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202180046554.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-29
Publication Date
2024-11-29
Estimated Expiration
2041-06-29

AI Technical Summary

Technical Problem

When the existing anti-reflection film faces external invasion of moisture, the transmittance change cannot be effectively suppressed, which affects the aesthetics and performance of the image display device.

Method used

A multi-layer film structure is adopted, wherein at least one layer is a silicon oxide layer, and its moisture permeability is 300 g/m2/day or less, a surface roughness is preferably 1.00 nm or less, and a hardness is preferably 5.0 GPa or more. By laminating high refractive index and low refractive index The dielectric layer of rate, including a mixed oxide layer of Mo and Nb, combines with the SiOx layer to form an anti-reflection film with light absorption capacity.

Benefits of technology

It effectively suppresses the transmittance changes caused by moisture intrusion, improves the density and durability of the anti-reflection film, and enhances the aesthetics and performance of the image display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115734951B_ABST
    Figure CN115734951B_ABST
Patent Text Reader

Abstract

The present invention relates to a transparent substrate with an antireflection film, wherein a multilayer film is provided on at least one main surface of the transparent substrate having two main surfaces, wherein the multilayer film is formed by stacking at least two layers having different refractive indices, and wherein at least one silicon oxide layer in the multilayer film has a moisture permeability of 300 g / m 2 / day or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a transparent substrate with an anti-reflection film. Background Art

[0002] In recent years, from the viewpoint of aesthetics, a method of providing a cover glass on the front surface of an image display device such as a liquid crystal display has been used.

[0003] In the above-mentioned technologies, reflection caused by the reflection of external light by the cover glass is becoming a problem. In order to solve the above-mentioned problem, a multilayer film with a laminated structure is often provided on the surface of the cover glass. However, the existing anti-reflection film makes the boundary between the black frame part and the image display part of the image display device obvious and the aesthetics are poor.

[0004] Therefore, it is known to impart light absorption capability to an anti-reflection film, which is a multilayer film formed by stacking at least two dielectric layers having different refractive indices. Thus, the boundary between the black frame portion and the image display portion of the image display device can be made less obvious. Furthermore, reflection from the interface between the cover glass and the anti-reflection film can also be suppressed.

[0005] For example, Patent Document 1 discloses a transparent substrate with an antireflection film which has light absorption capability and is insulating.

[0006] Patent Document 2 discloses a transparent conductive laminate in which a silicon oxide layer and a copper layer are sequentially stacked.

[0007] Patent Document 3 discloses an antireflection film having a film made of a high refractive index material and a film made of a low refractive index material on the surface of a glass plate, with the film made of the low refractive index material being arranged on the outermost surface.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2018-115105

[0011] Patent Document 2: Japanese Patent Application Publication No. 2016-068470

[0012] Patent Document 3: Japanese Patent Application Publication No. 2008-201633 Summary of the invention

[0013] As described above, there is known a technique for providing a multilayer film with light absorption capability to provide aesthetics and further suppress reflection from the interface between a cover glass and an anti-reflection film.

[0014] However, a technology that has light absorption capability and satisfies the requirement of suppressing a change in transmittance of an antireflection film due to the intrusion of moisture from the outside has not yet been achieved.

[0015] Therefore, an object of the present invention is to provide a transparent substrate with an antireflection film which has light absorbing capability and in which a change in transmittance of the antireflection film due to the intrusion of moisture from the outside is suppressed.

[0016] The inventors of the present invention have found that the above-mentioned problems can be solved by using a transparent substrate with an anti-reflection film, and have completed the present invention. The transparent substrate with an anti-reflection film has a multilayer film on at least one of the main surfaces of the transparent substrate having two main surfaces, and the multilayer film is formed by stacking at least two layers having different refractive indices, and at least one of the layers of the multilayer film has a moisture permeability of 300 g / m 2 / day or less.

[0017] In a transparent substrate with an anti-reflection film in one embodiment of the present invention, the multilayer film is a structure formed by stacking at least two layers with different refractive indices, at least one layer of the multilayer film is mainly composed of Si oxide, and another at least one layer of the multilayer film is mainly composed of a mixed oxide, which is a mixed oxide of at least one oxide selected from group A composed of Mo and W and at least one oxide selected from group B composed of Si, Nb, Ti, Zr, Ta, Al, Sn and In, and the content of the elements of group B contained in the mixed oxide is preferably less than 80% by mass relative to the total of the elements of group A contained in the mixed oxide and the elements of group B contained in the mixed oxide.

[0018] In the transparent substrate with an antireflection film according to one embodiment of the present invention, the arithmetic mean height (Sa) indicating the surface roughness of at least one silicon oxide layer in the multilayer film is preferably 1.00 nm or less within a measurement range of 1 μm×1 μm.

[0019] In the transparent substrate with an antireflection film according to one embodiment of the present invention, the arithmetic mean height (Sa) indicating the surface roughness of at least one silicon oxide layer in the multilayer film is preferably 0.90 nm or less within a measurement range of 5 μm×5 μm.

[0020] In the transparent substrate with an antireflection film according to one embodiment of the present invention, the hardness of at least one silicon oxide layer in the layers of the multilayer film is preferably 5.0 GPa or more.

[0021] In the transparent substrate with an antireflection film according to one embodiment of the present invention, the elastic modulus of at least one silicon oxide layer in the layers of the multilayer film is preferably 70 GPa or more.

[0022] In the transparent substrate with an antireflection film according to one embodiment of the present invention, it is preferred that an antifouling film is further provided on the antireflection film.

[0023] In the transparent substrate with an antireflection film according to one embodiment of the present invention, the transparent substrate is preferably a glass substrate.

[0024] In the transparent substrate with an antireflection film according to one embodiment of the present invention, the transparent substrate is preferably a resin substrate.

[0025] In the transparent substrate with an antireflection film according to one embodiment of the present invention, the transparent substrate is preferably a laminate composed of glass and a resin substrate.

[0026] In the transparent substrate with an antireflection film according to one embodiment of the present invention, the glass is preferably chemically strengthened.

[0027] In the transparent substrate with an antireflection film according to one embodiment of the present invention, it is preferred that an antiglare treatment be applied to a main surface of the transparent substrate on the side having the antireflection film.

[0028] In the transparent substrate with an antireflection film according to one embodiment of the present invention, an image display device including the transparent substrate with an antireflection film is preferred.

[0029] According to one embodiment of the present invention, it is possible to provide a transparent substrate with an antireflection film which has light absorption capability and in which a change in transmittance of the antireflection film due to the intrusion of moisture from the outside is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a cross-sectional view schematically showing a configuration example of a transparent substrate with an antireflection film. DETAILED DESCRIPTION

[0031] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0032] A transparent substrate with an antireflection film according to one embodiment of the present invention comprises a multilayer film on at least one of the main surfaces of a transparent substrate having two main surfaces, wherein the multilayer film is formed by laminating at least two layers having different refractive indices, and a silicon oxide layer of at least one of the layers of the multilayer film has a moisture permeability of 300 g / m 2 / day or less.

[0033] The transparent substrate in the present embodiment is not particularly limited as long as it is a transparent substrate having excellent light transmittance, and examples thereof include glass and resin.

[0034] The multilayer film in the transparent substrate with an antireflection film (transparent substrate with a multilayer film) of the present embodiment preferably has the following structure.

[0035] Figure 1 1 is a cross-sectional view schematically showing a configuration example of a transparent substrate with a multilayer film. A multilayer film 30 is formed on a transparent substrate 10 . Figure 1The multilayer film 30 shown is a laminated structure formed by laminating two dielectric layers 32 and 34 having different refractive indices. The reflection of light is suppressed by laminating dielectric layers 32 and 34 having different refractive indices. Dielectric layer 32 is a high refractive index layer, and dielectric layer 34 is a low refractive index layer.

[0036] Figure 1 In the multilayer film 30 shown, the dielectric layer 32 is preferably composed of a mixed oxide, which is a mixed oxide of at least one selected from the A group consisting of Mo and W and at least one selected from the B group consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In. In the mixed oxide, the content of the elements of the B group contained in the mixed oxide relative to the total of the elements of the A group contained in the mixed oxide and the elements of the B group contained in the mixed oxide (hereinafter referred to as the B group content) is preferably less than 80% by mass.

[0037] The dielectric layer 34 is preferably made of SiO x constitute.

[0038] The dielectric layer 32 is preferably composed of a mixed oxide of at least one oxide selected from the group A consisting of Mo and W and at least one oxide selected from the group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn, and In. Among them, Mo is preferred as the group A, and Nb is preferred as the group B.

[0039] By using Mo and Nb in dielectric layer 34 and dielectric layer 32 which are oxygen-deficient silicon oxide layers, conventional oxygen-deficient silicon oxide layers have a yellowish color in visible light, but by using Mo and Nb, the silicon oxide layer does not have a yellowish color even if oxygen deficiencies occur, which is more preferable.

[0040] The refractive index of the dielectric layer 32 at a wavelength of 550 nm is preferably 1.8 to 2.3 from the viewpoint of transmittance with the transparent substrate. The extinction coefficient of the dielectric layer 32 is preferably 0.005 to 3, more preferably 0.01 to 1, and further preferably 0.04 to 0.38.

[0041] If the extinction coefficient is 0.005 or more, a desired absorptivity can be achieved with an appropriate number of layers. In addition, if the extinction coefficient is 3 or less, it is easier to achieve a balance between reflection chromaticity and transmittance.

[0042] Figure 1 The multilayer film 30 shown is a stacked structure formed by stacking two dielectric layers 32 and 34, but the multilayer film of this embodiment is not limited to this, and can also be a stacked structure formed by stacking more than three layers with different refractive indices. In this case, the refractive indices of all layers do not need to be different.

[0043] For example, under the situation of 3-layer laminated structures, can be 3-layer laminated structures of low-index layer, high refractive index layer, low refractive index layer, or 3-layer laminated structures of high refractive index layer, low refractive index layer, high refractive index layer.In the situation of the former, there are 2 layers of low refractive index layer and can be identical refractive index, and in the situation of the latter, there are 2 layers of high refractive index layer and can be identical refractive index.

[0044] In the case of 4 layers of stacked structures, can be 4 layers of stacked structures of low refractive index layer, high refractive index layer, low refractive index layer, high refractive index layer, or 4 layers of stacked structures of high refractive index layer, low refractive index layer, high refractive index layer, low refractive index layer. In this case, having 2 layers of low refractive index layer and the high refractive index layer respectively can be identical refractive index.

[0045] The high refractive index layer mentioned here refers to a layer having a refractive index of 1.8 or more at a wavelength of 550 nm, for example, and the low refractive index layer refers to a layer having a refractive index of 1.6 or less at a wavelength of 550 nm.

[0046] As a light-transmitting film having light absorption capability and insulating properties, a half-tone mask used in the semiconductor manufacturing field is known. As a half-tone mask, Mo-SiO containing a small amount of Mo is used. x In addition, as a light-transmitting film having light absorption capability and insulating properties, there is a narrow bandgap film used in the field of semiconductor manufacturing.

[0047] However, these films have high light absorption capability on the short-wavelength side of visible light, and thus the transmitted light has a yellowish tint. Therefore, they are not suitable for cover glasses of image display devices.

[0048] In this embodiment, the dielectric layer 32 has a high Mo content and the SiO x The dielectric layer 34 thus constructed can provide a transparent substrate with an antireflection film having light absorbing ability, insulating properties, and excellent adhesion and strength.

[0049] Figure 1 The transparent substrate with an antireflection film shown has the above-mentioned structure through the multilayer film 30 and satisfies the above-mentioned characteristics of the transparent substrate with an antireflection film according to the present embodiment.

[0050] If the content of the mixed oxide of at least one oxide selected from the group A consisting of Mo and W and at least one oxide selected from the group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In in the layer (ABO) 32 consisting of the group B is less than 80 mass %, the b * The value exceeds 5. The content of the group B is more preferably 70% by mass or less, and even more preferably 60% by mass or less.

[0051] In the case of a laminated structure in which three or more layers having different refractive indices are laminated, the following may be included except for the layer (ABO) and the layer (SiO x In this case, it is necessary to form a layer containing the layer (ABO) and the layer (SiO x ) or a 3-layer laminated structure of a high refractive index layer, a low refractive index layer, and a high refractive index layer, or a 4-layer laminated structure of a low refractive index layer, a high refractive index layer, a low refractive index layer, and a high refractive index layer, or a 4-layer laminated structure of a high refractive index layer, a low refractive index layer, a high refractive index layer, and a low refractive index layer.

[0052] Among them, the outermost layer is preferably a layer (SiO x ). This is because in order to obtain low reflectivity, if the outermost layer is a layer (SiO x ), it can be easily produced. In addition, in the case of forming an antifouling film, from the viewpoint of bonding related to the durability of the antifouling film, it is preferably formed on the layer (SiO x )superior.

[0053] The layer (ABO) 32 is preferably amorphous. If it is amorphous, it can be produced at a relatively low temperature, and when the transparent substrate is a resin, the resin is not damaged by heat, and can be appropriately used.

[0054] In the transparent substrate with a multilayer film of the present embodiment, the moisture permeability of at least one silicon oxide layer in the multilayer film is 300 g / m 2 When the water vapor permeability is within the above range, the intrusion of moisture from the outside can be suppressed, and thus the change in the transmittance of the antireflection film due to the intrusion of moisture can be suppressed.

[0055] It should be noted that the moisture permeability can be measured by the method specified in JIS Z 0208 (1976) as described in the examples described later. The moisture permeability of the transparent substrate with a multilayer film of the present embodiment is preferably 0.1 to 300 g / m 2 / day, more preferably 0.1 to 100 g / m 2 / day.

[0056] For the transparent substrate with a multilayer film of the present embodiment, the surface roughness (arithmetic mean height (Sa)) of the silicon oxide layer of at least one layer in the multilayer film within the measurement range of 1 μm×1 μm is preferably 1.00 nm or less. If the surface roughness (arithmetic mean height (Sa)) is within the above range, the silicon oxide layer becomes dense, which can inhibit the intrusion of moisture from the outside, thereby inhibiting the change in the transmittance of the anti-reflection film caused by the intrusion of moisture.

[0057] The surface roughness (arithmetic mean height (Sa)) within a measurement range of 1 μm×1 μm can be measured using a scanning probe microscope, for example, in accordance with the provisions of the international standard ISO 25178, as described in the examples described below.

[0058] The surface roughness (arithmetic mean height (Sa)) of the silicon oxide layer in the transparent substrate with a multilayer film of the present embodiment within a measurement range of 1 μm×1 μm is preferably 0.05 to 0.99 nm, more preferably 0.05 to 0.98 nm.

[0059] For the transparent substrate with a multilayer film of the present embodiment, the surface roughness (arithmetic mean height (Sa)) of the silicon oxide layer of at least one layer in the multilayer film within a measurement range of 5 μm×5 μm is preferably 0.90 nm or less. If the surface roughness (arithmetic mean height (Sa)) is within the above range, the silicon oxide layer becomes dense, and the intrusion of water from the outside can be suppressed, thereby suppressing the change in the transmittance of the anti-reflection film caused by the intrusion of water.

[0060] The surface roughness (arithmetic mean height (Sa)) within a measurement range of 5 μm×5 μm can be measured using a scanning probe microscope, for example, in accordance with the provisions of the international standard ISO 25178, as described in the examples described below.

[0061] The surface roughness (arithmetic mean height (Sa)) of the silicon oxide layer in the transparent substrate with a multilayer film of the present embodiment in a measurement range of 5 μm×5 μm is preferably 0.05 to 0.90 nm, more preferably 0.05 to 0.87 nm.

[0062] For the transparent substrate with multilayer film of the present embodiment, the hardness of at least one silicon oxide layer in the multilayer film is preferably 5.0 GPa or more when measured with a load of 0.1 mN. If the hardness is within the above range, the silicon oxide layer becomes dense, and the intrusion of water from the outside can be suppressed, so that the transmittance change of the anti-reflection film caused by the intrusion of water can be suppressed.

[0063] The hardness of the silicon oxide layer can be measured, for example, using a surface force measuring device (nanoindenter) as described in the examples below.

[0064] The hardness of the silicon oxide layer of the transparent substrate with a multilayer film according to the present embodiment when measured with a load of 0.1 mN applied thereto is preferably 5.0 to 20.0 GPa, more preferably 5.2 to 15.0 GPa.

[0065] For the transparent substrate with multilayer film of the present embodiment, the hardness of at least one silicon oxide layer in the multilayer film is preferably 6.6 GPa or more when measured with a load of 1 mN. If the hardness is within the above range, the silicon oxide layer becomes dense and can inhibit water from invading from the outside, thereby inhibiting the change in transmittance of the anti-reflection film caused by water invading.

[0066] The hardness of the silicon oxide layer can be measured, for example, using a surface force measuring device (nanoindenter) as described in the examples below.

[0067] The hardness of the silicon oxide layer of the transparent substrate with a multilayer film according to the present embodiment when measured with a load of 1 mN applied thereto is preferably 6.6 to 20.0 GPa, more preferably 6.7 to 15.0 GPa.

[0068] For the transparent substrate with multilayer film of the present embodiment, the elastic modulus of at least one silicon oxide layer in the multilayer film is preferably 70 GPa or more when measured with a load of 0.1 mN. If the elastic modulus is within the above range, the silicon oxide layer becomes dense, and the intrusion of water from the outside can be suppressed, so that the transmittance change of the anti-reflection film caused by the intrusion of water can be suppressed.

[0069] The elastic modulus of the silicon oxide layer can be measured, for example, using a surface force measuring device (nanoindenter) as described in the examples below.

[0070] The elastic modulus of the silicon oxide layer of the transparent substrate with a multilayer film according to the present embodiment, when measured with a load of 0.1 mN applied thereto, is preferably 70 to 200 GPa, more preferably 72 to 150 GPa.

[0071] For the transparent substrate with multilayer film of the present embodiment, the elastic modulus of at least one silicon oxide layer in the multilayer film is preferably 81 GPa or more when measured with a load of 1 mN. If the elastic modulus is within the above range, the silicon oxide layer becomes dense and can suppress the intrusion of water from the outside, thereby suppressing the change in the transmittance of the anti-reflection film caused by the intrusion of water.

[0072] The elastic modulus of the silicon oxide layer can be measured, for example, using a surface force measuring device (nanoindenter) as described in the examples described later. The elastic modulus when a load of 1 mN is applied to the silicon oxide layer of the transparent substrate with a multilayer film of the present embodiment is preferably 81 to 200 GPa, more preferably 81 to 150 GPa.

[0073] The transparent substrate with a multilayer film according to this embodiment will be further described below.

[0074] <Transparent substrate>

[0075] The transparent substrate is preferably made of a material having a refractive index of 1.4 to 1.7 because it can sufficiently suppress reflection on the bonding surface when optically bonding displays, touch panels, and the like.

[0076] As the transparent substrate, a glass substrate or a resin substrate is preferred. The transparent substrate may be a laminate composed of a glass substrate and a resin substrate.

[0077] As the glass substrate, glasses having various compositions can be used. For example, the glass used in the present embodiment preferably contains sodium, and preferably has a composition that can be molded and strengthened by chemical strengthening treatment. Specifically, for example, aluminosilicate glass, soda-lime glass, borosilicate glass, lead glass, alkali-barium glass, aluminoborosilicate glass, etc. can be cited.

[0078] The thickness of the glass substrate is not particularly limited, but is usually preferably 5 mm or less, more preferably 3 mm or less, in order to effectively perform the chemical strengthening treatment.

[0079] The glass substrate is preferably a chemically strengthened glass that has been chemically strengthened in order to improve the strength of the cover glass. When the glass substrate is subjected to an anti-glare treatment, chemical strengthening is performed after the anti-glare treatment and before the multilayer film is formed.

[0080] It is preferred that the main surface of the glass substrate having the multilayer film is subjected to an anti-glare treatment. The anti-glare treatment method is not particularly limited, and a method of performing a surface treatment on the main surface of the glass to form desired irregularities can be used.

[0081] Specifically, the main surface of the glass substrate may be subjected to chemical treatment, such as frosting. The frosting may be performed by immersing the glass substrate as a treatment object in a mixed solution of hydrogen fluoride and ammonium fluoride to chemically treat the immersed surface.

[0082] In addition to using such chemical treatment methods, for example, the following methods can also be used: a so-called sandblasting method in which crystalline silica powder, silicon carbide powder, etc. are blown onto the surface of the glass substrate with pressurized air, or a physical treatment method such as wetting a brush to which crystalline silica powder, silicon carbide powder, etc. is attached with water and then rubbing the brush.

[0083] As the resin substrate, a resin film is preferred. As the resin film, a thermoplastic resin or a thermosetting resin can be used. For example, polyvinyl chloride resin, polyethylene resin, polypropylene resin, polystyrene resin, polyvinyl acetate resin, polyester resin, polyurethane resin, cellulose resin, acrylic resin, AS (acrylonitrile-styrene) resin, ABS (acrylonitrile-butadiene-styrene) resin, fluorine resin, thermoplastic elastomer, polyamide resin, polyimide resin, polyacetal resin, polycarbonate resin, modified polyphenylene ether resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polylactic acid resin, cyclic polyolefin resin, polyphenylene sulfide resin, etc. can be cited.

[0084] Among these, cellulose resins are preferred, and cellulose triacetate resins, polycarbonate resins, and polyethylene terephthalate resins are more preferred. These resins may be used alone or in combination of two or more.

[0085] The thickness of the film is not particularly limited, but is preferably 20 to 150 μm, more preferably 40 to 80 μm.

[0086] When a film is used as the transparent substrate 10 , the present embodiment may have a configuration in which a hard coat layer (not shown) or an antiglare layer (not shown) is provided on the transparent substrate 10 and the multilayer film 30 is provided thereon.

[0087] Furthermore, as another embodiment, an anti-glare layer may be provided on the hard coat layer, and the multilayer film 30 may be provided thereon.

[0088] As the hard coat layer, a material in which a polymer resin is dissolved may be applied.

[0089] The anti-glare layer is a layer that imparts anti-glare properties by forming a concavo-convex shape on one side of the film to increase haze. The anti-glare layer can be coated with a substance dissolved with a polymer resin in the same manner as the hard coat layer. The anti-glare layer composition constituting the anti-glare layer is composed of a substance in which a particulate substance having at least anti-glare properties is dispersed in a solution dissolved with a polymer resin as a binder.

[0090] Examples of particulate substances having the above-mentioned anti-glare properties include inorganic particles of silica, clay, talc, calcium carbonate, calcium sulfate, barium sulfate, aluminum silicate, titanium oxide, synthetic zeolite, alumina, montmorillonite, and organic particles composed of styrene resins, polyurethane resins, benzoguanamine resins, silicone resins, acrylic resins, and the like.

[0091] In addition, as the polymer resin used as the binder for the above-mentioned hard coat layer and the above-mentioned anti-glare layer, a polymer resin composed of polyester resin, acrylic resin, acrylic urethane resin, polyester acrylate resin, polyurethane acrylate resin, epoxy acrylate resin, and urethane resin can be used.

[0092] <Multilayer film>

[0093] The above-mentioned multilayer film can be formed on the main surface of the transparent substrate by a known film forming method such as sputtering, vacuum evaporation, coating, etc. That is, the dielectric layer or layers constituting the multilayer film can be formed on the main surface of the transparent substrate by a known film forming method such as sputtering, vacuum evaporation, coating, etc. according to the stacking order thereof.

[0094] Examples of the sputtering method include magnetron sputtering, pulse sputtering, AC sputtering, and digital sputtering.

[0095] For example, magnetron sputtering is a method of sputtering a film with a thickness of several nanometers by placing a magnet on the back of a dielectric material that serves as a matrix to generate a magnetic field, causing gas ion atoms to collide with the surface of the dielectric material and be bombarded. The magnetron sputtering method can form a continuous film of a dielectric oxide or nitride that is a dielectric material.

[0096] For example, the digital sputtering method is different from the usual magnetron sputtering. It is a method of first forming an extremely thin film of metal by sputtering, and then irradiating oxygen plasma or oxygen ions or oxygen free radicals for oxidation, and repeating such a process in the same chamber to form a thin film of metal oxide. In this case, the film-forming molecules are metal when they are plated (filmed) on the substrate, so it is presumed that they have ductility compared to the case of metal oxide coating. Therefore, it is believed that even with the same energy, the rearrangement of the film-forming molecules is likely to occur, resulting in a dense and smooth film.

[0097] The material of the anti-reflection film is not particularly limited, and various materials can be used as long as it is a material that can suppress the reflection of light. For example, as the anti-reflection film, it can be a structure formed by stacking a high refractive index layer and a low refractive index layer. The high refractive index layer mentioned here refers to a layer with a refractive index of 1.8 or more at a wavelength of 550nm, and the low refractive index layer refers to a layer with a refractive index of 1.6 or less at a wavelength of 550nm.

[0098] In addition, in the transparent substrate with an antireflection film of the present embodiment, the antireflection film only needs to be provided on at least one main surface of the transparent substrate, but may be provided on both main surfaces of the transparent substrate as necessary.

[0099] <Antifouling film>

[0100] The transparent substrate with a multilayer film of this embodiment may further have an antifouling film (also referred to as an "anti-fingerprint (AFP) film") on the multilayer film from the viewpoint of protecting the outermost surface of the film. The antifouling film may be composed of, for example, a fluorine-containing organosilicon compound.

[0101] As the fluorinated organosilicon compound, any fluorinated organosilicon compound can be used without particular limitation as long as it can impart antifouling properties, water repellency, and oil repellency. As the fluorinated organosilicon compound, for example, a fluorinated organosilicon compound having one or more groups selected from a polyfluoropolyether group, a polyfluoroalkylene group, and a polyfluoroalkyl group can be cited. It should be noted that a polyfluoropolyether group refers to a divalent group having a structure formed by alternating bonding of a polyfluoroalkylene group and an etheric oxygen atom.

[0102] In addition, as commercially available fluorine-containing silicone compounds having one or more groups selected from a polyfluoropolyether group, a polyfluoroalkylene group and a polyfluoroalkyl group, KP-801 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY178 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY-130 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY-185 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), OPTOOL (registered trademark) DSX and OPTOOL AES (both trade names, manufactured by DAIKIN Co., Ltd.) and the like can be preferably used.

[0103] The antifouling film is laminated on the antireflection film. When the antireflection film is formed on both main surfaces of the glass substrate or the resin substrate, the antifouling film can also be formed on both antireflection films, but it can also be a structure in which the antifouling film is laminated on only one surface. This is because the antifouling film can be set at a position that may be touched by a hand or the like, and can be selected according to its use, etc.

[0104] The transparent substrate with a multilayer film of the present embodiment is suitable as a cover glass for an image display device, particularly a cover glass for an image display device mounted in a vehicle or the like, such as an image display device of a navigation system mounted in a vehicle or the like.

[0105] Example

[0106] The present invention is specifically described below with reference to examples, but the present invention is not limited thereto. Examples 1 and 2 are examples, and Examples 3 and 4 are comparative examples.

[0107] (Example 3)

[0108] An antireflection film was formed on one main surface of a transparent substrate by the following method to produce a transparent substrate with an antireflection film.

[0109] A 40 μm-thick triacetyl cellulose resin film (hereinafter referred to as a TAC film) was used as the transparent substrate.

[0110] Next, by the following method, on one main surface of a transparent substrate, as a dielectric layer (1) (metal oxide layer), a target prepared by mixing niobium and molybdenum in a weight ratio of 60:40 and sintering is used by digital sputtering method, while maintaining the pressure at 0.2 Pa, the operation of forming a metal film of a very small film thickness with argon gas and then oxidizing it with oxygen is repeated at a high speed, thereby forming an oxide film, and forming a 10nm Mo-Nb-O layer on the main surface of the transparent substrate bonded with the diffusion layer.

[0111] Next, as a dielectric layer (2) (silicon oxide layer), a digital sputtering method was used with an organic silicon target. While maintaining the pressure at 0.3 Pa, an operation of forming an organic silicon film with argon gas and then oxidizing it with oxygen was repeated at a high speed, thereby forming an organic silicon oxide film, which was superimposed on the Mo-Nb-O layer to form a film of silicon oxide [SiO x Here, the oxygen flow rate during oxidation with oxygen gas was 500 sccm, and the input power of the oxidation source was 200W.

[0112] Next, as a dielectric layer (3) (metal oxide layer), a digital sputtering method is adopted and a target prepared by mixing niobium and molybdenum in a weight ratio of 60:40 and sintering is used. While the pressure is maintained at 0.2 Pa, the operation of forming a metal film with a very small film thickness with argon gas and then oxidizing it with oxygen is repeated at a high speed, thereby forming an oxide film, which is overlapped on the silicon oxide layer to form a Mo-Nb-O layer with a thickness of 120 nm.

[0113] Next, as a dielectric layer (4) (silicon oxide layer), a digital sputtering method was used with an organic silicon target. While the pressure was maintained at 0.3 Pa, an operation of forming an organic silicon film with argon gas and then oxidizing it with oxygen was repeated at a high speed, thereby forming a silicon oxide film, which was superimposed on the Mo-Nb-O layer, and a film thickness of 100 nm of silicon oxide [SiO x Here, the oxygen flow rate during oxidation with oxygen gas was 500 sccm, and the input power of the oxidation source was 200W.

[0114] In addition, for the transparent substrate with an anti-reflection film obtained in this manner, the spectral transmittance of the above-mentioned transparent substrate before and 500 hours after being put into a 95°C reliability test tank was measured using a spectrophotometer (manufactured by Shimadzu Corporation, trade name: SolidSpec-3700), and the light transmittance (stimulation value Y specified in JIS Z 8701:1999) was calculated. The change in light transmittance was calculated from the light transmittance before putting into the tank and the light transmittance after 500 hours.

[0115] As a result, the change in light transmittance in Example 3 was 5%.

[0116] (Example 1)

[0117] A transparent substrate with an antireflection film was prepared in the same manner as in Example 3 except that the pressure during the formation of the silicon oxide layer of the dielectric layer (2) and the dielectric layer (4) was changed to 0.1 Pa. The change in light transmittance in Example 1 was 2%.

[0118] (Example 2)

[0119] When forming the silicon oxide layers of the dielectric layer (2) and the dielectric layer (4), a linear ion source (manufactured by ULVAC) was used to release high-energy argon ions onto the film-forming surface at an input voltage of 2 kV, and a transparent substrate with an antireflection film was produced in the same manner as in Example 1. The light transmittance change in Example 2 was 1.5%.

[0120] (Example 4)

[0121] No antireflection film is formed on one main surface of the transparent substrate in Example 3.

[0122] (Measurement of moisture permeability of silicon oxide layer)

[0123] The moisture permeability of the silicon oxide layer with a thickness of 100 nm formed on the cellulose triacetate resin film with a thickness of 40 μm and a length of 100 mm×width of 100 mm under the film forming conditions of Examples 1, 2 and 3 was measured using a moisture permeability cup in accordance with JIS Z 0208 (1976) "Test method for moisture permeation of moisture-proof packaging materials". The measurement was carried out by sealing a moisture absorbent / calcium chloride (anhydrous) in the moisture permeability cup, repeatedly weighing the cup at a certain interval (every 24 hours or every 48 hours), and evaluating the increase in the cup mass as the amount of water vapor permeation. The results of the following evaluation are shown in Table 1 below.

[0124] The following evaluation results are shown in Table 1 for a 100 nm thick silicon oxide layer formed on a chemically strengthened glass substrate (Dragon Trail: registered trademark, manufactured by AGC Corporation) of 100 mm in length×100 mm in width×1.1 mm in thickness under the film forming conditions of Examples 1, 2 and 3.

[0125] (Surface roughness of silicon oxide layer (arithmetic mean height (Sa)))

[0126] The measurement was performed using a measuring device [manufactured by Hitachi High-Tech Corporation, device name: scanning probe microscope AFM5100N] with a measuring range of 1 μm×1 μm (or 5 μm×5 μm), an operating frequency of 1.2 Hz, and a tapping number of 256×256.

[0127] (Hardness of silicon oxide layer)

[0128] The measurement was performed using a measuring device [manufactured by ELIONIX, device name: surface force measuring device (nanoindenter) ESF-5000Plus], with a load of 0.1 mN (or 1 mN) applied.

[0129] (Elastic modulus of silicon oxide layer)

[0130] The measurement was performed using a measuring device [manufactured by ELIONIX, device name: surface force measuring device (nanoindenter) ESF-5000Plus], with a load of 0.1 mN (or 1 mN) applied.

[0131] [Table 1]

[0132]

[0133] As shown in Table 1, the moisture permeability of the silicon oxide layer in Examples 1 and 2 is 300 g / m 2 / day or less, the changes in their light transmittance were suppressed compared with Example 3.

[0134] In addition, in Table 1, the silicon oxide layer of the transparent substrate with an anti-reflection film in Examples 1 and 2, in which the surface roughness (arithmetic mean height (Sa)) within the measurement range of 1 μm×1 μm of the silicon oxide layer is less than 1.00 nm, becomes dense and can inhibit the intrusion of moisture from the outside, so the change in light transmittance is suppressed compared with Example 3.

[0135] Above, various embodiments have been described with reference to the accompanying drawings, but it goes without saying that the present invention is not limited to these examples. It is obvious that those skilled in the art can think of various variations or modifications within the scope of the scope of the patent claims, and it can be understood that they certainly also belong to the technical scope of the present invention. In addition, the various constituent elements in the above-mentioned embodiments can also be arbitrarily combined within the scope of not departing from the main purpose of the invention.

[0136] It should be noted that the present application is based on Japanese patent application (Japanese Patent Application No. 2020-115919) filed on July 3, 2020, the contents of which are incorporated herein by reference.

[0137] Explanation of symbols

[0138] 10 Transparent substrate

[0139] 30 layers of film

[0140] 32, 34 dielectric layer

Claims

1. A resin substrate with an antireflection film, comprising a multilayer film on at least one of the main surfaces of the resin substrate having two main surfaces, wherein the multilayer film is formed by laminating at least two layers having different refractive indices, and a silicon oxide layer of at least one of the layers of the multilayer film has a moisture permeability of 300 g / m 2 / day or less, At least one layer of the layers of the multilayer film is mainly composed of Si oxide, and another at least one layer of the layers of the multilayer film is mainly composed of a mixed oxide, wherein the mixed oxide is a mixed oxide of at least one oxide selected from the group A consisting of Mo and W and at least one oxide selected from the group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In, and the content of the elements of the group B contained in the mixed oxide is less than 80% by mass relative to the total of the elements of the group A contained in the mixed oxide and the elements of the group B contained in the mixed oxide. At least one silicon oxide layer among the layers of the multilayer film has an arithmetic mean height Sa indicating surface roughness within a measurement range of 1 μm×1 μm of 1.00 nm or less.

2. The resin substrate with an anti-reflection film according to claim 1, wherein At least one silicon oxide layer among the layers of the multilayer film has an arithmetic mean height Sa indicating surface roughness within a measurement range of 5 μm×5 μm of 0.90 nm or less.

3. The resin substrate with an anti-reflection film according to claim 1 or 2, wherein: At least one silicon oxide layer among the layers of the multilayer film has a hardness of 5.0 GPa or more.

4. The resin substrate with an anti-reflection film according to claim 1, wherein: The elastic modulus of at least one silicon oxide layer in the layers of the multilayer film is 70 GPa or more.

5. The resin substrate with an anti-reflection film according to claim 1 or 2, wherein: The multilayer film further has an antifouling film.

6. The resin substrate with an anti-reflection film according to claim 1 or 2, wherein: The resin substrate is subjected to an anti-glare treatment on a main surface thereof having the multi-layer film. 7 . An image display device comprising the resin substrate with an antireflection film according to claim 1 .

Citation Information

Patent Citations

  • Glass sheet with antireflection film and laminated glass for window

    JP2008201633A

  • Transparent conductive laminate and electrostatic capacitance type touch panel

    JP2016068470A

  • Transparent substrate with antireflection film

    JP2018115105A

  • Pachinko game machine

    JP2020115919A

  • Optical device

    CN105122090A