Bagasse-based hard carbon negative electrode active material for sodium ion batteries and its preparation and application
Through acid treatment and asphalt kneading modification technology, the structural defects and supply chain stability problems of sodium-ion battery anode materials prepared from sugarcane bagasse were solved, and high-performance bagasse-based hard carbon anode materials were prepared, which improved the performance of sodium-ion batteries. Electrochemical performance and yield.
Patent Information
- Application Number
- CN202211494878.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-11-26
AI Technical Summary
There is a lack of suitable anode materials in the development of sodium-ion batteries. In particular, the difficulty in the preparation of hard carbon materials lies in the stability, low cost and consistency of the raw material supply chain. In addition, sugarcane bagasse cannot retain the electrochemical beneficial components and repair structural defects. Effective solution.
Sugarcane bagasse is treated with acid solution and then kneaded and modified with asphalt. Through the joint control of modification temperature and atmosphere, the structural components and surface defects of bagasse are collaboratively regulated, its physical and chemical properties are repaired, and a material suitable for sodium ion batteries is prepared. Hard carbon negative active material.
The high-performance preparation of sugarcane bagasse-based hard carbon anode materials for sodium-ion batteries has been achieved, improving the electrochemical performance and productivity of sodium-ion batteries and solving the stability and cost issues of the raw material supply chain.
Smart Images

Figure CN115744871B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of negative electrode materials, and in particular to the field of negative electrode materials for sodium ion batteries. Background Art
[0002] The booming energy storage market has set off a research boom in electrochemical energy storage. As an important component of electrochemical energy storage, secondary batteries have also received much attention in recent years. Among them, lithium-ion batteries are limited by the scarcity of lithium resources, which limits their application in large-scale energy storage scenarios due to resource shortcomings and high prices caused by their lack. The development of sodium-ion batteries will directly solve these pain points of lithium-ion batteries, but due to some thermodynamic problems, the common graphite negative electrode of lithium ions cannot serve as the negative electrode material of sodium-ion batteries to store sodium. For this reason, the development of sodium-ion batteries urgently needs suitable negative electrode materials. Hard carbon materials used as negative electrodes of sodium-ion batteries have suitable sodium storage capacity and low sodium storage potential, and are considered to be more ideal negative electrode materials for sodium-ion batteries.
[0003] At present, the precursor routes of hard carbon materials mainly consist of resin-based, coal tar-based, biomass-based and other technical routes. In the face of sodium-ion battery energy storage application scenarios, the bulk supply and cost of hard carbon precursors are core considerations. The development of resin-based hard carbon materials is relatively easy, but it is difficult to avoid the impact of high raw material prices; the current production process of coal tar-based and other hard carbons is difficult and the performance is poor; the biomass precursor process is less difficult, and biomass hard carbon has excellent performance and is industrialized at a faster speed. However, when the development of sodium-ion batteries enters the growth and volume stage, it will be difficult to ensure the stability, low cost and consistency of the raw material supply chain, which will become a bottleneck. Therefore, it is still a challenge to explore large quantities of biomass raw materials to efficiently synthesize high-performance hard carbon materials. Summary of the invention
[0004] In view of the problem that bagasse is difficult to use to prepare negative electrodes suitable for sodium ion batteries, the first purpose of the present invention is to provide a method for preparing bagasse-based hard carbon negative electrode active materials for sodium ion batteries, aiming to prepare hard carbon negative electrode active materials suitable for sodium ion batteries and having excellent electrochemical properties based on bagasse.
[0005] The second purpose of the present invention is to provide a bagasse-based sodium ion battery hard carbon negative electrode active material prepared by the preparation method, aiming to successfully prepare the new material with the special physical and chemical structure and excellent electrochemical properties.
[0006] The third object of the present invention is to provide the application of the bagasse-based sodium ion battery hard carbon negative electrode active material in sodium ion batteries.
[0007] The fourth object of the present invention is to provide a sodium ion battery comprising the bagasse-based sodium ion battery hard carbon negative electrode active material, and its negative electrode and negative electrode material.
[0008] The sugarcane industry produces a large amount of bagasse, which is the residue formed after the sugarcane stems are squeezed. It contains a large amount of dense fibrous structure, with a hard outer wall and a soft inner core, and the material properties have poor uniformity. The use of bagasse to prepare sodium ion battery materials faces many preparation difficulties: for example: (1) How to selectively retain the electrochemical beneficial components in the bagasse and reduce the electrochemical unhelpful components, (2) How to solve the problem of prominent structural defects in the prepared materials due to the physicochemical structural characteristics of the bagasse; (3) How to construct a physicochemical structure suitable for sodium ions; (4) How to solve the problem of poor yield of negative electrode active materials prepared from bagasse. In view of the problems faced by bagasse in preparing negative electrode materials for sodium ion batteries, the present invention provides the following solutions:
[0009] A method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material, comprising treating bagasse with an acid solution to obtain pretreated bagasse;
[0010] The pretreated bagasse and asphalt are kneaded and modified to obtain a composite modified material; the temperature of the modification reaction is above the softening point of the asphalt and less than or equal to 400°C;
[0011] The modified material is calcined to obtain the bagasse-based sodium ion battery hard carbon negative electrode active material.
[0012] In view of the many problems faced by bagasse in preparing the negative electrode of sodium ion batteries, the present invention innovatively finds that the bagasse is pre-treated with acid solution, and then modified with asphalt by kneading method, and further coordinated with the joint control of the modification temperature, so that synergy can be achieved. The characteristics of bagasse can be used to carry out oxygen chemical modification of asphalt, thereby solving the problem that asphalt is easy to graphitize in the carbonization stage and it is difficult to prepare a hard carbon structure suitable for sodium ions. In addition, based on the modification reaction of asphalt, the surface flatness of bagasse due to material characteristics is not ideal and there are many defects. In the present invention, based on the acid treatment and the asphalt composite mixed double synergistic modification, the structural components of bagasse can be selectively regulated. In addition, surface defects can be unexpectedly repaired, and negative electrode active materials suitable for sodium ions and having excellent sodium ion battery performance can be synergistically prepared.
[0013] The bagasse is the residue obtained by squeezing sugarcane stems;
[0014] Preferably, the bagasse is soaked in an acid solution, followed by solid-liquid separation to obtain pretreated bagasse; or the bagasse is sprayed with an acid solution, followed by solid-liquid separation to obtain pretreated bagasse. In the present invention, the acid treatment and the subsequent asphalt-assisted kneading double modification treatment can achieve synergy, help regulate the electrochemically active beneficial components in the bagasse, reduce structural defects, construct a sodium ion-adapted structure, and help synergistically improve the electrochemical performance of sodium ion batteries.
[0015] Preferably, the acid solution is an aqueous solution of an inorganic acid; preferably an aqueous solution of at least one of hydrochloric acid, sulfuric acid, nitric acid, and hydrofluoric acid;
[0016] Preferably, the concentration of the solute in the acid solution is 0.5-3M.
[0017] In the present invention, the composite modification of acid-treated bagasse and asphalt by kneading and the joint control of the modification temperature are the key to synergistically improving the dual modification effect, improving the carbon yield and sodium ion adaptability, and improving the electrochemical performance of sodium ion batteries.
[0018] Asphalt will undergo a certain degree of graphitization during the carbonization process, making it difficult to successfully prepare hard carbon materials. However, in the present invention, acid-treated bagasse and asphalt are innovatively used for composite mixing and modification treatment, which can modify the asphalt based on the oxygenation capacity of the bagasse, and can further facilitate the modification reaction to repair the defects and consistency of the bagasse. In this way, based on the synergistic dual modification of the two, the sodium ion battery performance and production capacity of the material can be synergistically improved.
[0019] In the present invention, there is no particular requirement for the type of asphalt, for example, its softening point temperature is 50 to 250° C., preferably 150 to 175° C. In the present invention, the preferred asphalt helps to further improve the kneading double modification effect, and helps to further synergistically improve the sodium ion battery performance of the prepared material.
[0020] The weight ratio of the pretreated bagasse to asphalt is 1:0.1-1.5, preferably 1:0.1-0.5. Studies have found that at the preferred ratio, a better double kneading modification effect can be obtained, which helps to further synergistically improve the electrochemical performance of the sodium ion battery of the prepared material.
[0021] Preferably, the pretreated bagasse and asphalt are pre-kneaded and pre-treated, and then the subsequent kneading modification reaction is carried out. The present invention also found that the innovative pre-kneading of the pretreated bagasse and asphalt can further synergistically improve the dual kneading modification effect.
[0022] In the present invention, the pressure in the pretreatment stage of mixing and kneading bagasse and asphalt is normal pressure or negative pressure.
[0023] It is further preferred that the pretreated bagasse and asphalt are pre-kneaded under negative pressure beforehand, and then the subsequent kneading modification reaction is performed. In the present invention, negative pressure pretreatment is performed beforehand, and then the temperature is increased for subsequent kneading modification. Based on the gas change, pressure change and gradient temperature control method, the dual modification effect of the two can be further synergistically improved, which helps to further synergistically solve the problem of bagasse preparation, and can synergistically regulate the electrochemical beneficial components, construct a sodium ion-compatible physicochemical structure, repair defects, and synergistically improve the electrochemical performance of the material in the sodium ion battery.
[0024] Preferably, the pretreatment temperature is 0.9 to 1.2 times the softening point of asphalt, and more preferably 1 to 1.2 times.
[0025] Preferably, the negative pressure is less than or equal to 0.5 atm (standard atmospheric pressure), preferably less than or equal to 0.1 atm.
[0026] Preferably, the atmosphere in the kneading modification reaction is an oxygen-containing atmosphere. In the present invention, kneading modification is carried out under the preferred atmosphere, which helps to further synergistically improve the dual synergistic modification effect, helps to further solve the problem of bagasse preparation, and can further improve the electrochemical performance of the prepared material in sodium ion batteries.
[0027] The oxygen-containing atmosphere is, for example, oxygen, an oxygen-nitrogen mixed gas, an oxygen-inert gas mixed gas, air, etc. Preferably, the oxygen content of the oxygen-containing atmosphere is 10 to 70 v%, more preferably 20 to 60 v%;
[0028] The temperature of the kneading modification reaction is greater than or equal to 1.4 times the softening point of the asphalt; more preferably, greater than or equal to 1.45 to 1.55 times the softening point of the asphalt.
[0029] In the present invention, in order to improve the kneading modification effect, the temperature in the kneading modification stage is preferably greater than or equal to 200°C, more preferably 240-320°C, and most preferably 250-260°C; in the present invention, the preferred kneading modification temperature helps to further improve the kneading dual modification effect, and helps to further synergistically improve the sodium ion battery performance of the prepared material.
[0030] Preferably, the kneading modification reaction time is 1 to 3 hours.
[0031] Preferably, the atmosphere of the calcination process is at least one of ammonia, nitrogen, an inert gas, and carbon dioxide; preferably, it is an atmosphere containing ammonia; in the present invention, the preferred ammonia-containing atmosphere can unexpectedly further cooperate with other processes to further improve the sodium ion battery performance of the material.
[0032] Preferably, the roasting process includes a first roasting process and a second roasting process, wherein the temperature of the first roasting process is 500-800°C, preferably 600-650°C, and the temperature of the second roasting process is 1200-1600°C, preferably 1300-1400°C;
[0033] Preferably, the first stage of roasting is 1 to 3 hours, and the second stage of roasting is 1 to 5 hours;
[0034] Preferably, the first stage of roasting treatment is followed by crushing, gas grinding, and sieving to obtain a powder with a D50 of 5 to 35 um before the second stage of roasting treatment is performed.
[0035] The present invention provides a specific method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material, comprising the following steps:
[0036] Step (1):
[0037] Sugarcane bagasse from the sugar industry is selected as raw material, and is subjected to acid solution treatment and drying treatment; the acid in the acid solution is one or more of hydrochloric acid, sulfuric acid, nitric acid and hydrofluoric acid.
[0038] Step (2):
[0039] The bagasse of step (1) is mixed with a certain amount of asphalt and kneaded and modified in a kneading pot to obtain a raw material; wherein the weight ratio of the dried bagasse to the asphalt is 1:0.1-1.5; the kneading temperature of the kneading pot is 80-400°C, and the kneading time is 1-3h.
[0040] Step (3):
[0041] The blank is placed in an atmosphere furnace for high-temperature pyrolysis to obtain a pyrolysis carbon blank; the pyrolysis temperature of the high-temperature pyrolysis is 500-800°C, the pyrolysis time is 1-3 hours, and the protective atmosphere is one of ammonia, argon, nitrogen, and carbon dioxide.
[0042] Step (4):
[0043] The pyrolysis carbon embryo is crushed, gas-milled, and the powder with suitable particle size is screened for secondary carbonization, and the screened particle size entering the furnace is 5-25um D50 to obtain the hard carbon material. The tail powder with too fine particle size obtained by screening can be added as an additive to the kneading pot in step (2) for further kneading and fusion.
[0044] The present invention also provides a method for preparing bagasse-based sodium ion battery hard carbon negative electrode active material.
[0045] The preparation method of the present invention can give the product a special physical and chemical structure, and the preparation method has an excellent yield. In addition, the prepared material can exhibit excellent electrochemical properties in a sodium ion battery.
[0046] The present invention also provides the use of the bagasse-based sodium ion battery hard carbon negative electrode active material, which is used as a negative electrode active material to prepare a sodium ion battery;
[0047] Preferably, it is used as a negative electrode active material to prepare a negative electrode of a sodium ion battery;
[0048] The present invention can prepare the required sodium ion battery and its negative electrode and negative electrode material by preparing the active material based on the existing method.
[0049] The present invention also provides a sodium ion battery negative electrode, comprising a current collector and a negative electrode material composited on the surface of the current collector, wherein the negative electrode material comprises a bagasse-based sodium ion battery hard carbon negative electrode active material prepared by the preparation method of the present invention;
[0050] Preferably, the negative electrode material further comprises a conductive agent and a binder.
[0051] The present invention also provides a sodium ion battery, which comprises the negative electrode described in the present invention.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] The present invention innovatively pre-treats the sugarcane bagasse from the sugarcane industry with acid solution, and then kneads and modifies it with asphalt at the temperature, and cooperates with the joint control of temperature, so that synergy can be achieved, and the characteristics of the bagasse can be used to chemically modify the asphalt, thereby solving the problem that the asphalt is easy to graphitize during the carbonization stage and it is difficult to prepare a hard carbon structure that is compatible with sodium ions. In addition, based on the modification reaction of asphalt, the surface flatness of the bagasse due to the material characteristics is not ideal and there are many defects. In the present invention, based on the acid treatment and the asphalt composite mixed double synergistic modification, the electrochemical composition of the bagasse can be selectively regulated. In addition, surface defects can be unexpectedly repaired, graphitization can be reduced, and sodium ion compatible negative electrode active materials with excellent sodium ion battery performance can be synergistically prepared.
[0054] In the present invention, kneading treatment is carried out under an oxygen-containing atmosphere and at the temperature, which helps to further synergistically improve the effect of the dual modification of the two, helps to further solve the problem of bagasse preparation, and improves the performance of the prepared material in the sodium ion battery. In addition, the present invention also found that the bagasse and asphalt are pre-kneaded under negative pressure and then kneaded and modified at the temperature, which can further synergize and help to further improve the effects of electrochemical composition regulation, sodium ion adaptation structure construction, etc., help to further synergistically improve the performance of the material sodium ion battery, not only that, but also help to improve the negative electrode yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 The long cycle data diagram of Example 1
[0056] Figure 2 The relationship curve between voltage and capacity of Example 1 is DETAILED DESCRIPTION
[0057] The present invention will be further described in detail below in conjunction with the embodiments, but the invention is not limited to its protection scope.
[0058] Bagasse is the residue produced by the sugar industry, which is the residue left after the sugar cane stalks are pressed to remove the sugar juice.
[0059] Example 1
[0060] Step (1):
[0061] The bagasse powder obtained from the sugar industry is added to 1M hydrochloric acid solution to obtain a mixed phase, the solid content of the mixed phase is controlled at 60%, and the mixture is filtered after stirring. The filter residue is washed with water and then dried to obtain the pretreated bagasse powder.
[0062] Step (2):
[0063] The bagasse powder and asphalt (softening point of 171°C) prepared in step (1) are added to a kneading pot (the weight ratio of bagasse (by dry weight) to asphalt is 1:0.25), and the temperature is raised to 190°C (marked as T1) under vacuum conditions (pressure less than or equal to 0.1atm), and pre-kneaded at this temperature for 30 minutes (pre-kneading section), and then switched to a mixed gas with an oxygen content of 45v% (oxygen-N2 mixed gas), and the temperature of the kneading pot is raised to 260°C (marked as T2) and kneading and modification are continued for 2 hours (kneading modification section) to obtain a modified blank.
[0064] Step (3):
[0065] The modified blank was added into a pyrolysis furnace for high-temperature pyrolysis. The pyrolysis temperature was 600°C (marked as T3), the atmosphere was ammonia, the pyrolysis time was 2 hours, and the heating rate was 5°C / min.
[0066] The blocky blank obtained by pyrolysis was crushed, pulverized and screened into powder with a particle size D50 of 10 μm and put into a furnace for high-temperature carbonization. The carbonization temperature was 1400°C (marked as T4), the atmosphere was ammonia, and the carbonization time was 2 hours to obtain a hard carbon material with low specific surface area and high sub-nanometer pores. The comprehensive carbon yield of the modified blank was 62%.
[0067] The hard carbon composite material, conductive carbon black and sodium carboxymethyl cellulose (CMC) obtained in Example 1 were uniformly mixed in a mass ratio of 90:5:5, and dispersed in a certain mass of deionized water to make a slurry, which was then coated on an aluminum foil current collector and vacuum dried at 80°C to obtain a sodium ion battery negative electrode sheet. The battery assembly and test were as follows: the negative electrode sheet was punched into an electrode sheet with a diameter of 10 mm, metallic sodium was used as the counter electrode, the electrolyte was 1M NaPF6 / EC:DEC (1:1), and a CR2032 button cell was assembled in a glove box filled with argon. Constant current charge and discharge tests were carried out at room temperature (25°C) with a current density of 30 mA / g, and the charge and discharge cut-off voltage was 0 to 3 V. The first discharge specific capacity was 382 mAh / g, the first cycle coulomb efficiency was 94.1%, and the capacity retention rate after 100 cycles was 98.8%.
[0068] Example 2
[0069] Compared with Example 1, the only difference is that in step (2), the sugarcane treated in step (1) is changed to
[0070] The mass ratios of slag powder and asphalt are:
[0071] Group A: The weight ratio of bagasse to asphalt was 1:0.1, and other process parameters were consistent with those in Example 1.
[0072] Group B: The weight ratio of bagasse to asphalt was 1:0.5, and other process parameters were consistent with those in Example 1. Group C: The weight ratio of bagasse to asphalt was 1:1, and other process parameters were consistent with those in Example 1;
[0073] Group D: The weight ratio of bagasse to asphalt is 1:1.5. The results are as follows:
[0074] The electrochemical test results of group A: the first discharge specific capacity is 368mAh / g, the first cycle coulombic efficiency is 91.20%, and the capacity retention rate after 100 cycles is 98.2%.
[0075] The electrochemical test results of group B: the first discharge specific capacity was 362mAh / g, the first cycle coulombic efficiency was 90.24%, and the capacity retention rate after 100 cycles was 97.6%.
[0076] Electrochemical test results of group C: the first discharge specific capacity was 358 mAh / g, the first cycle coulombic efficiency was 91.35%, and the capacity retention rate after 100 cycles was 96.8%.
[0077] The electrochemical test results of group D: the first discharge specific capacity was 348 mAh / g, the first cycle coulombic efficiency was 90.36%, and the capacity retention rate after 100 cycles was 95.8%.
[0078] It can be seen from Examples 2 and 1 that based on the innovative process of the present invention, dual synergistic modification of different bagasse and asphalt can be achieved, and good electrochemical properties can be obtained. The study also found that controlling the ratio of bagasse to asphalt to 1:0.1-0.5, especially 1:0.2-0.3, can further synergistically improve the sodium ion battery performance of the material.
[0079] Example 3
[0080] Compared with Example 1, the only difference is that the softening point temperature of the asphalt in step (2) is changed to.
[0081] Group A: The softening point of the asphalt is 93°C, and the temperature ratio of T1 and T2 to the softening point is the same as in Example 1.
[0082] Other process parameters are consistent with those in Example 1;
[0083] Group B: The softening point of the asphalt is 127°C, and the temperature ratio of T1 and T2 to the softening point is the same as in Example 1.
[0084] Other process parameters are consistent with those in Example 1;
[0085] Group C: The softening point of the asphalt is 154°C, and the temperature ratio of T1 and T2 to the softening point is the same as in Example 1.
[0086] Other process parameters are consistent with those in Example 1;
[0087] Group D: The softening point of the asphalt is 218°C, and the temperature ratio of T1 and T2 to the softening point is the same as in Example 1.
[0088] Other process parameters are consistent with those in Example 1;
[0089] Group E: The softening point of the asphalt is 241°C, and the temperature ratio of T1 and T2 to the softening point is the same as in Example 1.
[0090] Other process parameters are consistent with those in Example 1;
[0091] The results were as follows:
[0092] Electrochemical test results of group A: the first discharge specific capacity is 341 mAh / g, the first cycle coulombic efficiency is 89.10%, and the capacity retention rate after 100 cycles is 94.9%.
[0093] The electrochemical test results of group B: the first discharge specific capacity was 349 mAh / g, the first cycle coulombic efficiency was 90.52%, and the capacity retention rate after 100 cycles was 95.9%.
[0094] Electrochemical test results of group C: the first discharge specific capacity was 371 mAh / g, the first cycle coulombic efficiency was 91.51%, and the capacity retention rate after 100 cycles was 98.1%.
[0095] The electrochemical test results of group D: the first discharge specific capacity was 365 mAh / g, the first cycle coulombic efficiency was 90.63%, and the capacity retention rate after 100 cycles was 97.8%.
[0096] The electrochemical test results of group E: the first discharge specific capacity is 355mAh / g, the first cycle coulombic efficiency is 91.36%, and the capacity retention rate after 100 cycles is 97.9%.
[0097] In the present invention, thanks to the innovative scheme described in the present invention, different asphalts have good modification effects and can obtain ideal electrochemical properties, especially asphalts with a softening point of 150 to 200°C, which can be coordinated with other processes to obtain better electrochemical performance of sodium ion batteries.
[0098] Example 4
[0099] Compared with Example 1, the only difference is that the pre-kneading process in step (2) is changed, that is, the temperature is raised to T1 in air, and pre-kneading is carried out in this atmosphere and temperature, and then the kneading modification treatment in stage T2 is carried out, and the other processes remain unchanged;
[0100] Electrochemical test results: The first discharge specific capacity is 356mAh / g, the first cycle coulombic efficiency is 91.30%, and the capacity retention rate after 100 cycles is 93.6%.
[0101] Example 5
[0102] Compared with Example 1, the only difference is that in step 2, the pre-kneading step is omitted, and the kneading modification treatment of the T2 stage is directly performed, and the other processes remain unchanged;
[0103] Electrochemical test results: The first discharge specific capacity is 349mAh / g, the first cycle coulombic efficiency is 90.20%, and the capacity retention rate after 100 cycles is 91.6%.
[0104] It can be seen from Examples 1, 4 and 5 that pre-kneading and subsequent kneading modification can further synergistically improve the dual modification effect, and pre-kneading under negative pressure can further improve the synergistic modification effect of the two.
[0105] Example 6
[0106] Compared with Example 1, the only difference is that the atmosphere in the kneading and modification stage in step (2) is changed. The experimental groups are:
[0107] Group A: The oxygen content of the oxygen-containing atmosphere in the kneading modification was replaced with air, and the other processes remained unchanged;
[0108] Group B: The oxygen content of the kneading modified oxygen-containing atmosphere was changed to 60% (oxygen-N2 composite gas), and the other processes remained unchanged.
[0109] Group C: The oxygen content of the oxygen-containing atmosphere in the kneading modification was changed to N2, and the other processes remained unchanged.
[0110] The results were as follows:
[0111] Electrochemical test results of group A: the first discharge specific capacity is 370mAh / g, the first cycle coulombic efficiency is 91.83%, and the capacity retention rate after 100 cycles is 97.4%.
[0112] The electrochemical test results of group B: the first discharge specific capacity was 368 mAh / g, the first cycle coulombic efficiency was 90.51%, and the capacity retention rate after 100 cycles was 98.1%.
[0113] The electrochemical test results of group C: the first discharge specific capacity was 351 mAh / g, the first cycle coulombic efficiency was 90.51%, and the capacity retention rate after 100 cycles was 95.2%.
[0114] It can be seen from Examples 1 and 6 that the kneading and modification stage under an oxygen-containing atmosphere is helpful to further improve the performance of the sodium ion battery.
[0115] Example 7
[0116] Compared with Example 1, the only difference is that the temperature and time of T1 and T2 in the pre-mixing and kneading modification stages of step (2) are changed to:
[0117] Group A: The temperature of T1 was 180°C (1.05 times the softening point of asphalt), and the pre-mixing time was 45 minutes;
[0118] Group B: The temperature of T1 was 200°C (1.17 times the softening point of asphalt), and the pre-mixing time was 45 minutes;
[0119] Group C: In the kneading modification stage, the temperature of T2 was 240°C (1.4 times the softening point of asphalt), and the kneading time was 3 hours.
[0120] Group D: In the kneading modification stage, the temperature of T2 was 250°C (1.46 times the softening point of asphalt), and the kneading time was 2 hours.
[0121] Group E: In the kneading modification stage, the temperature of T2 was 280°C (1.63 times the softening point of asphalt), and the kneading time was 1 hour.
[0122] The results were as follows:
[0123] The electrochemical test results of group A: the first discharge specific capacity is 356mAh / g, the first cycle coulombic efficiency is 90.98%, and the capacity retention rate after 100 cycles is 97.2%.
[0124] The electrochemical test results of group B: the first discharge specific capacity was 357 mAh / g, the first cycle coulombic efficiency was 90.24%, and the capacity retention rate after 100 cycles was 97.3%.
[0125] Electrochemical test results of group C: the first discharge specific capacity was 355 mAh / g, the first cycle coulombic efficiency was 93.2%, and the capacity retention rate after 100 cycles was 97.0%.
[0126] Electrochemical test results of group D: the first discharge specific capacity was 367 mAh / g, the first cycle coulombic efficiency was 91.44%, and the capacity retention rate after 100 cycles was 98.2%.
[0127] The electrochemical test results of group E: the first discharge specific capacity was 359 mAh / g, the first cycle coulombic efficiency was 92.2%, and the capacity retention rate after 100 cycles was 98.0%.
[0128] It can be seen from Examples 7 and 1 that the process adjustment of the kneading temperature and the kneading time can further synergistically improve the adaptability of the prepared material in the sodium ion battery, which helps to further improve the performance of the sodium ion battery.
[0129] Example 8
[0130] Compared with Example 1, the only difference is that the pyrolysis atmosphere in step (3) is changed to:
[0131] Group A: The atmosphere in the T3 roasting stage was changed to argon atmosphere, and the other processes remained unchanged
[0132] Group B: The atmosphere in the T4 roasting stage was changed to argon atmosphere, and the other processes remained unchanged
[0133] Group C: The atmosphere of the T3 / T4 roasting stage was changed to argon atmosphere, and other processes remained unchanged.
[0134] The results were as follows:
[0135] Electrochemical test results of group A: the first discharge specific capacity is 362mAh / g, the first cycle coulombic efficiency is 90.30%, and the capacity retention rate after 100 cycles is 98.1%.
[0136] The electrochemical test results of group B: the first discharge specific capacity was 358 mAh / g, the first cycle coulombic efficiency was 91.38%, and the capacity retention rate after 100 cycles was 97.6%.
[0137] Electrochemical test results of group C: the first discharge specific capacity was 352 mAh / g, the first cycle coulombic efficiency was 91.15%, and the capacity retention rate after 100 cycles was 98.3%.
[0138] Example 9
[0139] Compared with Example 1, the only difference is that the temperature and time of pyrolysis T3 are changed, respectively:
[0140] Group A: T3 temperature is 500℃, time is 3h;
[0141] Group B: The temperature of T3 is 800℃ and the time is 1h.
[0142] The results were as follows:
[0143] The electrochemical test results of group A: the first discharge specific capacity is 366mAh / g, the first cycle coulombic efficiency is 90.98%, and the capacity retention rate after 100 cycles is 96.6%.
[0144] The electrochemical test results of group B: the first discharge specific capacity was 362mAh / g, the first cycle coulombic efficiency was 90.59%, and the capacity retention rate after 100 cycles was 95.9%.
[0145] It can be seen from Examples 7 and 1 that the process adjustment of the pyrolysis temperature and time can further synergistically improve the adaptability of the prepared material in sodium ion batteries, which helps to further improve the performance of sodium ion batteries.
[0146] Example 10
[0147] Compared with Example 1, the only difference is that the temperature of high temperature carbonization T4 is:
[0148] Group A: T4 carbonization temperature is 1200℃ and carbonization time is 5 hours;
[0149] Group B: T4 carbonization temperature is 1600℃, carbonization time is 1 hour
[0150] The results were as follows:
[0151] The electrochemical test results of group A: the first discharge specific capacity is 346 mAh / g, the first cycle coulombic efficiency is 89.82%, and the capacity retention rate after 100 cycles is 95.6%.
[0152] The electrochemical test results of group B: the first discharge specific capacity was 358 mAh / g, the first cycle coulombic efficiency was 92.59%, and the capacity retention rate after 100 cycles was 97.9%.
[0153] Comparative Example 1
[0154] Compared with Example 1, the only difference is that the treatment in step 1 is not performed, and the bagasse is directly subjected to step 2 and subsequent treatments, and the other operations and parameters are the same as those in Example 1. According to the scheme of Example 1, the results are as follows: the comprehensive carbon yield of the material is 48%, the first discharge specific capacity is 316 mAh / g, the first cycle coulomb efficiency is 82.18%, and the capacity retention rate after 100 cycles is 83.6%.
[0155] Comparative Example 2
[0156] Compared with Example 1, the only difference is that 1M sodium hydroxide solution is used to replace 1M hydrochloric acid, and other operations and parameters are the same as Example 1. According to the scheme of Example 1, the results are as follows: the comprehensive carbon yield of the material is 45%. The first discharge specific capacity is 328mAh / g, the first cycle coulomb efficiency is 86.36%, and the capacity retention rate after 100 cycles is 86.4%.
[0157] Comparative Example 3
[0158] Compared with Example 1, the only difference is that in step (2), asphalt is not added, and other operations and parameters are the same as Example 1. The comprehensive carbon yield is 36%, and the electrochemical test results show that the first discharge capacity is 352 mAh / g, the first cycle coulomb efficiency is 85.18%, and the capacity retention rate after 100 cycles is 89.2%.
[0159] Comparative Example 4
[0160] Compared with Example 1, the only difference is that in step (2), the asphalt and bagasse are not modified under kneading, but are stirred and mixed in a stirred tank; other operations and parameters are the same as in Example 1.
[0161] The comprehensive carbon production rate is 43%. The electrochemical test results show that the first discharge capacity is 312 mAh / g, the first cycle coulomb efficiency is 83.18%, and the capacity retention rate after 100 cycles is 83.2%.
[0162] Comparative Example 5
[0163] Compared with Example 1, the only difference is that in step (2), the asphalt and bagasse are not modified under kneading, but the mixing method is changed to hot pressing molding, and the hot pressing temperature is 260° C. to obtain a modified blank. Other operations and parameters are the same as those in Example 1.
[0164] The comprehensive carbon production rate is 46%. The electrochemical test results show that the first discharge capacity is 302mAh / g, the first cycle coulomb efficiency is 83.28%, and the capacity retention rate after 100 cycles is 86.0%.
[0165] Comparative Example 6
[0166] Compared with Example 1, the only difference is that in step (2), the temperature T2 of the kneading and modification stage is 450°C.
[0167] The comprehensive carbon production rate is 45%. The electrochemical test results show that the first discharge capacity is 318 mAh / g, the first cycle coulomb efficiency is 84.34%, and the capacity retention rate after 100 cycles is 84.2%.
[0168] Comparative Example 7
[0169] Step (1):
[0170] The sugarcane bagasse powder obtained from the sugar industry is added with 1M hydrochloric acid to obtain a mixed phase, the solid content of the mixed phase is controlled at 60%, and the mixture is filtered after stirring. The filter residue is washed with water and then dried to obtain the pre-treated sugarcane bagasse powder. The sugarcane bagasse powder is added to a pyrolysis furnace for high-temperature pyrolysis at a pyrolysis temperature of 600°C to obtain the sugarcane bagasse pre-carbonized powder.
[0171] Step (2):
[0172] The bagasse pre-carbonized powder and asphalt (softening point of 171° C.) prepared in step (1) are added to a kneading pot. The subsequent process is consistent with the embodiment. According to the scheme of embodiment 1, the comprehensive carbon yield is 58%, and the electrochemical results are: the first discharge specific capacity is 323 mAh / g, the first cycle coulomb efficiency is 81.28%, and the capacity retention rate after 100 cycles is 81.9%.
Claims
1. A method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material, characterized in that: Treating bagasse with acid to obtain pretreated bagasse; The pretreated bagasse and asphalt are kneaded and modified to obtain a composite modified material; the temperature of the modification reaction is above the softening point of the asphalt and less than or equal to 400°C; The modified material is subjected to a roasting treatment to obtain the bagasse-based sodium ion battery hard carbon negative electrode active material; The softening point temperature of the asphalt is 50-250°C; The weight ratio of the pretreated bagasse to asphalt is 1:0.1-1.5; The pretreated bagasse and asphalt are pre-kneaded and pre-treated in advance, and then a subsequent kneading modification reaction is performed; the temperature of the kneading pre-treatment is 0.9 to 1.2 times the softening point temperature of the asphalt; the temperature of the kneading modification reaction is greater than or equal to 1.4 times the softening point temperature of the asphalt; The kneading pretreatment process is carried out under negative pressure; the atmosphere in the kneading modification reaction is an oxygen-containing atmosphere.
2. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The bagasse is the residue obtained by squeezing sugarcane stems.
3. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The sugarcane bagasse is soaked in acid solution, followed by solid-liquid separation to obtain pretreated sugarcane bagasse; or the sugarcane bagasse is sprayed with acid solution, followed by solid-liquid separation to obtain pretreated sugarcane bagasse.
4. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The acid solution is an aqueous solution of an inorganic acid.
5. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 4, characterized in that: The acid solution is an aqueous solution of at least one of hydrochloric acid, sulfuric acid, nitric acid and hydrofluoric acid.
6. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 4, characterized in that: The concentration of the solute in the acid solution is 0.5 to 3M.
7. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The softening point temperature of the asphalt is 150-175°C.
8. The method for preparing bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The weight ratio of the pretreated bagasse to asphalt is 1:0.1-0.
5.
9. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The temperature of the kneading pretreatment is 1 to 1.2 times the softening point of the asphalt.
10. The method for preparing bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The temperature of the kneading modification reaction is greater than or equal to 1.45 to 1.55 times the softening point of asphalt.
11. The method for preparing bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The temperature of the kneading modification reaction is greater than or equal to 200°C.
12. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 11, characterized in that: The temperature of the kneading modification reaction is 240-320°C.
13. The method for preparing bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 12, characterized in that: The temperature of the kneading modification reaction is 250-260°C.
14. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The oxygen content of the oxygen-containing atmosphere is 10-70v%.
15. The method for preparing bagasse-based hard carbon negative electrode active material for sodium ion battery according to claim 1, characterized in that: The kneading modification reaction time is 1 to 3 hours.
16. The method for preparing a bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The atmosphere during the calcination process is at least one of ammonia, nitrogen, inert gas and carbon dioxide.
17. The method for preparing bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 16, characterized in that: The atmosphere during the calcination process is an atmosphere containing ammonia.
18. The method for preparing bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 1, characterized in that: The roasting process includes a first roasting process and a second roasting process, wherein the temperature of the first roasting process is 500-800°C, and the temperature of the second roasting process is 1200-1600°C.
19. The method for preparing bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 18, characterized in that: The first stage of roasting takes 1 to 3 hours, and the second stage of roasting takes 1 to 5 hours.
20. The method for preparing bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 18, characterized in that: After the first stage of roasting, the powder is crushed and pulverized by gas grinding, and the powder with D50 of 5 to 35 μm is sieved and then subjected to the second stage of roasting.
21. A bagasse-based sodium ion battery hard carbon negative electrode active material prepared by the method according to any one of claims 1 to 20.
22. An application of the bagasse-based sodium ion battery hard carbon negative electrode active material according to any one of claims 1 to 20, characterized in that: It is used as negative electrode active material to prepare sodium ion batteries.
23. The use of bagasse-based sodium ion battery hard carbon negative electrode active material according to claim 22, characterized in that: It is used as negative electrode active material to prepare the negative electrode of sodium ion battery.
24. A negative electrode for a sodium ion battery, comprising a current collector and a negative electrode material composited on the surface of the current collector, characterized in that: The negative electrode material comprises a bagasse-based sodium ion battery hard carbon negative electrode active material obtained by the preparation method according to any one of claims 1 to 20.
25. The sodium ion battery negative electrode according to claim 24, characterized in that: The negative electrode material also includes a conductive agent and a binder.
26. A sodium ion battery, characterized in that: Comprising the negative electrode according to claim 24 or 25.
Citation Information
Patent Citations
Preparation method of sodium ion hard carbon negative electrode material
CN114709408A
Biomass-based hard carbon, preparation method thereof and application of biomass-based hard carbon in sodium-ion battery
CN115020643A