A quaternary manganese-based infrared nonlinear optical crystal, its preparation method and applications
By preparing the quaternary manganese-based infrared nonlinear optical crystal AMn3Ga5S11, the problems of low laser damage threshold and two-photon absorption of existing infrared nonlinear optical crystal materials are solved, and the balance between high laser damage threshold and wide optical band gap is achieved, which improves the Performance of infrared detectors and lasers.
Patent Information
- Application Number
- CN202111039974.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-09-06
AI Technical Summary
The existing infrared nonlinear optical crystal materials have serious disadvantages in terms of low laser damage threshold and two-photon absorption, which limits their application range.
A quaternary manganese-based infrared nonlinear optical crystal AMn3Ga5S11 was developed, prepared by high-temperature solid phase method, with a monoclinic crystal structure and a three-dimensional diamond grid structure, with alkali metal elements A (K, Rb or Cs) as charges. Equilibrium filling achieves wide optical band gap and high laser damage threshold.
The powder frequency doubling intensity of this material reaches 0.8-1.5 times that of commercial material AgGaS2, and the laser damage threshold is 30-35 times that of AgGaS2, achieving the balance of the large second-order frequency doubling coefficient and wide optical band gap. It is suitable for infrared detectors, High-tech fields such as lasers and photorefractive information processing.
Smart Images

Figure CN115772706B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic nonlinear optical materials, and in particular relates to a quaternary manganese-based infrared nonlinear optical crystal, and a preparation method and application thereof. Background Art
[0002] Nonlinear optical crystals are a very important type of functional material, which are widely used in laser communications, optical information processing, integrated circuits and military technology. Generally speaking, an ideal nonlinear optical crystal must meet the following conditions: (1) a large second-order harmonic frequency coefficient; (2) a high laser damage threshold; (3) an appropriate birefringence; (4) a wide optical transmission range; (5) good physical, chemical and mechanical properties. Nonlinear optical materials can be divided into inorganic materials, organic materials, polymer materials and organometallic complex materials according to their physical and chemical properties. At present, the vast majority of nonlinear optical crystals on the market are inorganic materials. According to their different application bands, they can be divided into three categories: ultraviolet band, visible band and infrared band. Among them, nonlinear optical crystal materials in the ultraviolet and visible bands can already meet the requirements of practical applications.
[0003] The nonlinear optical crystal material in the infrared band is mainly ABC 2 A typical example of a chalcopyrite-structured semiconductor material is AgGaS. 2 、AgGaSe 2 、ZnGeP 2 Such compounds have large nonlinear optical coefficients and high mid- and far-infrared transmittance, but they also have serious disadvantages such as low laser damage threshold and two-photon absorption, which limits their application. Therefore, exploring new infrared nonlinear optical crystal materials with application prospects is a difficulty and hot spot in the current research field of nonlinear optical materials. Summary of the invention
[0004] The present invention aims to provide a quaternary manganese-based infrared nonlinear optical crystal, a preparation method and use thereof. The optical crystal material has excellent second-order nonlinear optical properties, can achieve phase matching in the infrared band, and has a wide optical band gap (E g >3.0eV), and its powder frequency-doubled intensity can reach that of commercial material AgGaS 2 0.8-1.5 times of AgGaS, and its laser damage threshold is 2 The crystal has a power of 30-35 times that of the original crystal, achieving a good balance between a large second-order frequency doubling coefficient and a wide optical band gap.
[0005] The present invention provides the following technical solutions:
[0006] The present invention provides an optical crystal, the molecular formula of which is AMn 3Ga 5 S 11 ; wherein A is an alkali metal element, and the alkali metal element is selected from K, Rb or Cs.
[0007] According to an embodiment of the present invention, the structure of the optical crystal belongs to the monoclinic system, the space group is Pc, and its unit cell parameters are α=90°, β=100~110°, γ=90°.
[0008] Exemplarily, the optical crystal is KMn 3 Ga 5 S 11 , whose unit cell parameters are α=90°, β=105.197±0.02°, γ=90°.
[0009] Exemplarily, the optical crystal is RbMn 3 Ga 5 S 11 , whose unit cell parameters are α=90°, β=105.273±0.02°, γ=90°.
[0010] Exemplarily, the optical crystal is CsMn 3 Ga 5 S 11 , whose unit cell parameters are α=90°, β=105.354±0.02°, γ=90°.
[0011] According to an embodiment of the present invention, the optical crystal has a three-dimensional diamond-like grid structure, and the three-dimensional diamond-like grid structure is mainly composed of [MnS 4 ] and [GaS 4 ] Tetrahedrons are used as basic structural units and are connected to each other through common vertices S. The alkali metal element A is dispersed and filled in the three-dimensional diamond-like grid structure as a charge balance.
[0012] Preferably, the structure of the optical crystal is as follows Figure 1 shown.
[0013] According to an embodiment of the present invention, the optical crystal CsMn 3 Ga 5 S 11 The basic Figure 2 The X-ray crystal diffraction pattern shown in a.
[0014] According to an embodiment of the present invention, the optical crystal RbMn 3Ga 5 S 11 The basic Figure 3 The X-ray crystal diffraction pattern shown in a.
[0015] According to an embodiment of the present invention, the optical crystal is an infrared nonlinear optical crystal. For example, the optical crystal can achieve phase matching in the infrared band and has a wide optical band gap (E g >3.0eV).
[0016] According to the embodiment of the present invention, the powder frequency doubling intensity of the optical crystal is the commercial material AgGaS 2 0.8-1.5 times of the crystal.
[0017] According to an embodiment of the present invention, the laser damage threshold of the optical crystal is the commercial material AgGaS 2 30-35 times of crystal.
[0018] The present invention also provides a method for preparing the above optical crystal, comprising the following steps: mixing raw materials uniformly, and preparing the optical crystal by a high-temperature solid phase method;
[0019] The raw materials include alkali metal halide AX, gallium oxide Ga 2 O 3 , elemental Mn, elemental S and elemental B.
[0020] According to an embodiment of the present invention, in the alkali metal halide AX, A is selected from K, Rb or Cs, and X is selected from Cl, Br or I.
[0021] According to an embodiment of the present invention, AX, Ga 2 O 3 The molar ratio of Mn, S and B is AX:Ga 2 O 3 :Mn:S:B=(1-10):5:6:(20-25):10, preferably AX:Ga 2 O 3 :Mn:S:B=(2-5):5:6:(21-23):10; For example, the molar ratio can be AX:Ga 2 O 3 :Mn:S:B=2:5:6:22:10; or AX:Ga 2 O 3 :Mn:S:B=3:5:6:23:10.
[0022] According to an embodiment of the present invention, the high temperature solid phase method specifically comprises: putting the raw materials into a sealed container and placing it in a heating device, heating up, keeping the high temperature, and cooling down to room temperature to obtain the optical crystal.
[0023] Preferably, the high temperature solid phase method is carried out under vacuum conditions. Further preferably, the sealed container has a vacuum environment, for example, the vacuum pressure is 10 -4 -10 -3 Pa.
[0024] Preferably, the sealed container is a sealed quartz reaction tube.
[0025] Preferably, the heating refers to heating to a holding temperature, and the holding temperature is selected from 800 to 1200°C, preferably 900 to 1100°C, such as 950-1050°C.
[0026] Preferably, the high temperature insulation time is not less than 50 hours, preferably 50-100 hours.
[0027] Exemplarily, the high temperature insulation refers to insulation at 950° C. for 120 hours, or insulation at 1000° C. for 100 hours.
[0028] Preferably, the cooling includes cooling to 400° C. and then naturally cooling to room temperature. Further preferably, the cooling is performed at a rate of no more than 2° C. / hour.
[0029] Preferably, the preparation method further comprises washing and drying the product obtained by naturally cooling to room temperature to obtain the optical crystal, for example, washing with water (such as deionized water) and drying with ethanol.
[0030] The present invention also provides the optical crystal prepared by the above method.
[0031] The present invention further provides uses of the optical crystal, such as infrared detectors, infrared lasers, photorefractive information processing, etc.
[0032] The present invention also provides use of the optical crystal, for example, for laser frequency conversion.
[0033] The present invention also provides use of the optical crystal, for example, in a near-infrared probe.
[0034] The present invention further provides an infrared detector comprising the above optical crystal.
[0035] The present invention further provides an infrared laser, which contains the above optical crystal.
[0036] Beneficial effects of the present invention:
[0037] The present invention provides a quaternary manganese-based infrared nonlinear optical crystal material, which has excellent second-order nonlinear optical properties, that is, it can achieve phase matching in the infrared band and has a wide optical band gap (Eg >3.0eV), and its powder frequency-doubled intensity can reach that of commercial material AgGaS 2 0.8-1.5 times of AgGaS, and its laser damage threshold is 2 The crystal has a power of 30-35 times that of the original crystal, achieving a good balance between a large second-order frequency doubling coefficient and a wide optical band gap.
[0038] This infrared nonlinear optical crystal has important application value in high-tech fields such as laser frequency conversion, near-infrared probes, and photorefractive information processing, especially in infrared detectors and infrared lasers. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 AMn of the present invention 3 Ga 5 S 11 Schematic diagram of the crystal structure.
[0040] Figure 2 The sample CsMn prepared in Example 1 3 Ga 5 S 11 X-ray diffraction pattern of .
[0041] Figure 3 The sample RbMn prepared in Example 2 3 Ga 5 S 11 X-ray diffraction pattern of . DETAILED DESCRIPTION
[0042] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0043] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0044] Example 1
[0045] CsI, Ga 2 O 3 , Mn, S and B were mixed evenly in a molar ratio of 2:5:6:22:10 to obtain a raw material. The raw material was placed in a quartz crucible, and the quartz crucible containing the raw material was placed in a quartz reaction tube, and vacuum was drawn to 10 -3Pa and melt the sealed quartz reaction tube with hydrogen-oxygen flame. Place the quartz reaction tube in a tube furnace with a temperature controller, heat it to 1000°C, and keep it warm for 100 hours. Then cool it to 400°C at a rate not exceeding 2°C / hour, stop heating, and cool it naturally to room temperature. The product is washed with deionized water and dried with ethanol to obtain the infrared nonlinear optical crystal CsMn 3 Ga 5 S 11 , recorded as sample 1.
[0046] Example 2
[0047] The difference between this embodiment and embodiment 1 is that CsI is replaced with RbI to obtain an infrared nonlinear optical crystal RbMn 3 Ga 5 S 11 , recorded as sample 2.
[0048] Example 3
[0049] The difference between this embodiment and embodiment 1 is that CsI is replaced with KI to obtain the infrared nonlinear optical crystal KMn 3 Ga 5 S 11 , recorded as sample 3.
[0050] Test Case
[0051] (1) Structural characterization of samples
[0052] The samples of Examples 1-3 were subjected to X-ray single crystal diffraction tests under the following test conditions: on a Saturn 724 single crystal diffractometer, Mo target, Kα radiation source (λ=0.07107nm), and test temperature 293K. The samples were structurally analyzed by Shelx-2014. The crystallographic data results of the samples are shown in Table 1, and the crystal structure diagram is shown in Figure 1 shown.
[0053] Table 1 Sample AMn 3 Ga 5 S 11 Crystallographic data of (A=Cs,Rb,K)
[0054]
[0055] like Figure 1 As shown, the obtained crystals are mainly composed of [MnS 4 ] and [GaS 4 ] Tetrahedrons are the basic structural units, which are connected to each other through shared vertices S to form a three-dimensional diamond-like grid structure. Alkali metal ions A, which serve as charge balance, are dispersed and filled in the three-dimensional grid structure.
[0056] X-ray powder diffraction phase analysis (XRD) was performed on Sample 1-2 on a Rigaku MiniFlex II X-ray diffractometer, using a Cu target and a Kα radiation source (λ = 0.154184 nm). The XRD spectrum obtained by fitting the powder XRD pattern of the sample with the single crystal diffraction data is shown in the figure below: Figure 2-3 As shown. Figure 2 It can be seen that the XRD pattern of sample 1 is fitted with the XRD spectrum obtained by single crystal diffraction data. Figure 1 due to Figure 3 It can be seen that the XRD pattern of sample 2 is fitted with the XRD spectrum obtained by single crystal diffraction data. Figure 1 It shows that the samples obtained in Examples 1-2 have high crystallinity and purity.
[0057] (2) Characterization of optical properties of samples
[0058] The optical properties of samples 1-3 were tested under the following conditions: characterization on a Perkin-Elmer FT-IR infrared spectrometer and a Perkin-Elmer Lambda 950 UV-visible (near infrared) absorption or diffuse reflectance spectrometer. The light transmission properties, frequency doubling properties, laser damage threshold and optical band gap of samples 1-3 are shown in Table 2.
[0059] Table 2 Optical performance data of samples
[0060]
[0061] The exemplary embodiments of the present invention are described above. However, the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An optical crystal, characterized in that: The molecular formula of the optical crystal is AMn3Ga5S 11 ; Wherein, A is an alkali metal element, and the alkali metal element is selected from K, Rb or Cs; The structure of the optical crystal belongs to the monoclinic system, and the space group is Pc , whose unit cell parameters are a=8~10Å, b=14~16Å, c=13~15Å, α=90°, β=100~110°, γ=90°; The optical crystal has a three-dimensional diamond-like grid structure, which is mainly composed of [MnS4] and [GaS4] tetrahedrons as basic structural units, which are interconnected through common vertices S. The alkali metal element A is dispersed and filled in the three-dimensional diamond-like grid structure as a charge balance.
2. The optical crystal according to claim 1, characterized in that: The optical crystal is KMn3Ga5S 11 , whose unit cell parameters are a=8.891±0.02Å, b=15.044±0.02Å, c=13.859±0.02Å, α=90°, β=105.197±0.02°, γ=90°; Or, the optical crystal is RbMn3Ga5S 11 , whose unit cell parameters are a=8.953±0.02Å, b=15.124±0.02Å, c=13.932±0.02Å, α=90°, β=105.273±0.02°, γ=90°; Or, the optical crystal is CsMn3Ga5S 11 , and its unit cell parameters are a=9.007±0.02Å, b=15.185±0.02Å, c=13.995±0.02Å, α=90°, β=105.354±0.02°, and γ=90°.
3. The optical crystal according to claim 1 or 2, characterized in that: The optical crystal is an infrared nonlinear optical crystal; And / or, the powder frequency-doubled intensity of the optical crystal is 0.8-1.5 times that of the commercial material AgGaS2 crystal; And / or, the laser damage threshold of the optical crystal is 30-35 times that of the commercial material AgGaS2 crystal.
4. The method for preparing an optical crystal according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: mixing raw materials uniformly, and preparing the optical crystal by a high-temperature solid phase method; The raw materials include alkali metal halide AX, gallium oxide Ga2O3, simple Mn, simple S and simple B; In the alkali metal halide AX, A is selected from K, Rb or Cs, and X is selected from Cl, Br or I; the molar ratio of AX, Ga2O3, Mn, S and B is AX: Ga2O3: Mn: S: B = (1-10): 5: 6: (20-25):
10.
5. The preparation method according to claim 4, characterized in that: AX: Ga2O3: Mn: S: B = (2-5): 5:6: (21-23):
10.
6. The preparation method according to claim 4, characterized in that: The high temperature solid phase method specifically comprises: putting the raw material into a sealed container and placing it in a heating device, heating and heating, high temperature insulation, and cooling to room temperature to obtain the optical crystal; the temperature of the high temperature insulation is selected from 800 to 1200°C; And / or, the high temperature solid phase method is carried out under vacuum conditions.
7. The preparation method according to claim 6, characterized in that: The sealed container has a vacuum environment; And / or, the sealed container is a sealed quartz reaction tube; And / or, the heating refers to raising the temperature to a high temperature insulation temperature; And / or, the high temperature insulation time is not less than 50 hours; And / or, the cooling includes cooling to 400° C. and then naturally cooling to room temperature.
8. The preparation method according to claim 6, characterized in that: The vacuum pressure of the sealed container is 10 -4 -10 - 3 Pa; And / or, the high temperature insulation temperature is 900-1100°C; And / or, the high temperature insulation time is 50-100 hours; And / or, the temperature is lowered at a rate not exceeding 2°C / hour.
9. The preparation method according to claim 4, characterized in that: The preparation method further comprises washing and drying the product obtained by naturally cooling to room temperature to obtain the optical crystal.
10. Use of the optical crystal according to any one of claims 1 to 3 in infrared detectors, infrared lasers, and photorefractive information processing.
11. Use of the optical crystal according to any one of claims 1 to 3 in laser frequency conversion.
12. Use of the optical crystal according to any one of claims 1 to 3 in near-infrared probes.
13. An infrared detector comprising the optical crystal according to any one of claims 1 to 3.
14. An infrared laser comprising the optical crystal according to any one of claims 1 to 3.