Preparation method and application of antler-shaped bismuth-based lithium battery negative electrode nanomaterial
By preparing antler-shaped Bi13S18X2 lithium battery negative electrode nanomaterials, using hydrothermal reaction and PEDOT:PSS coating technology, the problems of low conductivity and volume expansion of binary metal bismuth sulfide materials have been solved, and lithium ions with high energy density and long life have been achieved. Battery negative electrode material significantly improves the cycle stability and electrochemical performance of the battery.
Patent Information
- Application Number
- CN202211665147.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The existing binary metal bismuth sulfide anode material causes the capacity of lithium-ion batteries to decay rapidly due to low conductivity and volume expansion problems, and the theoretical specific capacity is low, which cannot meet the demand for high energy density.
A preparation method of antler-shaped Bi13S18X2 lithium battery negative electrode nanomaterials is adopted. By reacting bismuth nitrate pentahydrate and thiourea in a hydrothermal kettle, polyvinylpyrrolene and PEDOT:PSS coating are added, and the process parameters are controlled to obtain nanoscale ternary materials. Bismuth-based sulfide material improves electrical conductivity and structural stability.
Through the unique nanostructure, the volume stress is relieved, the ion migration distance is reduced, the battery charge and discharge performance and cycle stability are improved, the battery specific capacity and conductivity are increased, and the cycle stability and electrochemical performance of the material are significantly improved.
Smart Images

Figure BDA0004014510270000031 
Figure BDA0004014510270000041 
Figure BDA0004014510270000051
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a preparation method and application of a antler-shaped bismuth-based lithium battery negative electrode nanomaterial. Background Art
[0002] With the rapid development of social economy, the extensive use of fossil energy such as coal, oil and natural gas has caused energy shortages and huge environmental pollution. In order to meet future energy needs and achieve a green and efficient sustainable development strategy, it is urgent to find renewable green energy to replace fossil fuels and traditional energy to achieve an effective energy storage strategy. Due to the advantages of lithium battery such as high energy density, long cycle life and low self-discharge characteristics, lithium-ion batteries have attracted widespread attention as the most widely studied and applied secondary batteries. The progress and achievements made by lithium-ion batteries in an increasingly wide range of applications have led to higher and higher requirements for their energy density. In order to achieve this goal, it is urgent to develop innovative battery technologies and advanced materials to achieve lithium-ion batteries with high energy density and long life. The negative electrode material is one of the important components of lithium-ion batteries and has a decisive influence on the performance of lithium-ion batteries. The development of high-performance negative electrode materials is one of the key factors in the preparation of high-performance lithium-ion batteries. Graphite is the most commonly used negative electrode material in commercial lithium-ion batteries due to its low working potential, low cost and long cycle life. However, the graphite negative electrode 372mAhg -1 The low theoretical specific capacity is increasingly unable to meet the current demand for high-performance, especially high-energy-density lithium-ion batteries. Therefore, it is urgent to develop new negative electrode materials with high performance, especially high specific capacity, to replace traditional graphite negative electrodes, thereby improving the energy and power density of batteries.
[0003] In recent years, sulfur-based lithium battery negative electrode materials have received widespread attention because sulfur is abundant in the earth's crust, is cheap, and non-toxic. More importantly, the binary metal negative electrode materials they form with bismuth have a relatively high theoretical specific capacity, which is required as high-performance lithium battery negative electrode materials. However, negative electrode materials such as metal sulfides have low electrical conductivity, which will lead to low ion and electron migration rates. At the same time, there are certain volume expansion problems during the battery charging and discharging process, which will cause the sample powder structure to be destroyed or the particles to be pulverized. Therefore, the application range of the material is limited. Nano-sizing and coating are both very effective methods to improve the cycle stability of negative electrode materials. Therefore, we need to use a new method that combines the advantages of previous optimization methods to optimize the new Bi 13 S 18 X2 (X = Cl, Br, I ... X is not limited to the listed elements) bismuth-based materials are optimized. The present invention prepares antler-shaped Bi 13 S 18X2 lithium battery negative electrode nanomaterial and its application, the preparation method is simple, and the prepared antler-shaped Bi 13 S 18 X2 negative electrode nanomaterials have excellent electrochemical properties. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a antler-shaped bismuth-based lithium battery negative electrode nanomaterial to solve the problems of rapid battery capacity decay and low capacity caused by low electrical conductivity and large volume expansion of existing binary metal bismuth sulfide negative electrode materials.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] A method for preparing a antler-shaped bismuth-based lithium battery negative electrode nanomaterial comprises the following steps:
[0007] (1) Preparation of Precursor A:
[0008] According to the molecular formula, a molar percentage of bismuth nitrate pentahydrate is dissolved in ethylene glycol, and thiourea is dissolved in deionized water. After stirring until completely dissolved, the thiourea solution is slowly dripped into the bismuth nitrate solution, and then a molar percentage of Y is added, and an appropriate amount of polyvinyl pyrrolidone is added. The mixture is stirred at 70-100° C., and after 10 minutes, it is transferred to a hydrothermal kettle for insulation. After the reaction obtains a mixed solution, it is centrifuged and washed for more than 3 times, and dried for more than 12 hours to obtain a precursor A.
[0009] (2) Preparation of PEDOT:PSS-coated negative electrode powder:
[0010] Take 300-500 mg of precursor A and disperse it in deionized water, add an appropriate amount of PEDOT:PSS (PEDOT:PSS is poly (3,4-ethylenedioxythiophene-polystyrene sulfonic acid), stir until dry to obtain PEDOT:PSS-wrapped Bi 13 S 18 X2 negative electrode powder.
[0011] Furthermore, in step (1), the amount of ethylene glycol is 0-75 ml, the amount of deionized water is 0-75 ml, the dissolution temperature is 80-100°C, and the stirring speed is 300-500 rpm. 13 S 18 X2 powder has good crystallinity and is less likely to contain impurities.
[0012] Further, in the step (1), the amount of polyvinyl pyrrolidone is 0.02-0.1 g, the hydrothermal kettle is kept at 80-160°C, and the time is 6-18 hours. 13 S 18X2 powder, convenient for subsequent operations.
[0013] Furthermore, in step (1), the centrifuge speed is 3000-5000 rpm, the time is 3-5 min, and the drying temperature is 60-80°C. 13 S 18 The surface of X2 powder is cleaner, which is convenient for subsequent operations.
[0014] Furthermore, in step (2), the amount of deionized water is 10-20 ml, the amount of PEDOT:PSS added is 3-7% of the mass of the precursor, the stirring temperature is 80-100°C, and the stirring speed is 300-500 rpm. The operation is simple, and the obtained lithium-ion battery has stable electrochemical performance, high battery specific capacity, and optimal cycle stability.
[0015] Furthermore, in step (1), Y is selected as sodium halide, and the sodium halide is a soluble salt such as NaCl, NaBr and NaI.
[0016] Further; in the step (2), Bi 13 S 18 In X2, X is a halogen element, and X=Cl, Br, I… is selected.
[0017] Further; an application of a antler-shaped bismuth-based lithium battery negative electrode nanomaterial in batteries.
[0018] Compared with the prior art, the present invention has at least one of the following beneficial effects:
[0019] 1. This technical solution obtains a nano-scale ternary new bismuth-based sulfide material with a deer antler shape by controlling the design of the synthesis process parameters. The unique nanostructure makes it conducive to the release of volume stress during the charge and discharge process, thereby alleviating the capacity attenuation problem caused by volume stress. At the same time, the nanostructure can reduce the migration distance of ions and improve the charge and discharge performance of the battery; PEDOT:PSS has a high conductivity of 100-200Scm -1 The use of PEDOT:PSS coating can not only greatly optimize the conductivity of the material and enhance electron transmission, but also further inhibit the volume expansion of the material during the charging and discharging process, thereby improving the structural stability and cycle stability of the battery.
[0020] 2. The added polyvinyl pyrrolidone is beneficial to adjust Bi 13 S 18 X2 morphology makes it easy to obtain antler-like micro-nanostructures.
[0021] 3. By using PEDOT:PSS for coating treatment, not only can the electronic conductivity of the nanomaterial be improved, but also the volume stress of the material during the charge and discharge process can be suppressed, making the antler-shaped Bi provided by this scheme 13 S 18 X2 negative electrode material has high cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the XRD pattern of the negative electrode material prepared by the technical solution of Example 1;
[0023] Figure 2 This is a SEM image of the negative electrode material prepared by the technical solution of Example 1;
[0024] Figure 3 This is a SEM image of the negative electrode material prepared by the technical solution of Example 1 at a high magnification;
[0025] Figure 4 This is a SEM image of the negative electrode material prepared by the technical solution of Comparative Example 4;
[0026] Figure 5 This is a SEM image of the negative electrode material prepared by the technical solution of Comparative Example 6;
[0027] Figure 6 This is a cycle performance diagram of the negative electrode material prepared by the technical solution of Experimental Example 1;
[0028] Figure 7 This is a cycle performance diagram of the negative electrode material prepared by the technical solution of Comparative Example 4;
[0029] Figure 8 This is a cycle performance diagram of the negative electrode material prepared by the technical solution of Comparative Example 6. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0031] The parameters of a method for constructing a surface migration channel of a bismuth-based negative electrode material and an application example thereof of the present invention are shown in Table 1.
[0032] Table 1
[0033]
[0034]
[0035] Taking Example 1 as an example, the preparation method of a antler-shaped bismuth-based lithium battery negative electrode nanomaterial of the present invention is described.
[0036] The present invention provides a method for preparing a antler-shaped bismuth-based lithium battery negative electrode nanomaterial, which specifically comprises the following steps:
[0037] Step (1) Preparation of Precursor A:
[0038] Weigh 3.153g of bismuth nitrate pentahydrate and dissolve it in 0-75ml of ethylene glycol and 0.6851g of thiourea in 0-75ml of deionized water. In this embodiment, the amount of ethylene glycol is 50ml, and the amount of deionized water is 25ml. Stir at 80-100°C and a stirring speed of 300-500rpm until it is completely dissolved. In this embodiment, the dissolution temperature is 80°C and the stirring speed is 500rpm. Slowly drip the thiourea solution into the bismuth nitrate solution, add 1.5g of sodium iodide, and add 0.02-0.1g of polyvinyl pyrrolidone (PVP). P), the amount of PVP in this embodiment is 0.05g, stirred at 70-100°C, the stirring temperature in this embodiment is 80°C, transferred to a hydrothermal kettle after 10min and kept warm at 80-160°C for 6-18h, the hydrothermal kettle keeping temperature in this embodiment is 80°C, and the time is 6h; after the reaction to obtain a mixed solution, centrifuged at 3000-5000rpm for 3-5min, washed more than 3 times, the centrifuge speed in this embodiment is 3000rpm, the time is 5min, and dried for more than 12h to obtain a precursor A.
[0039] Step (2) Preparation of PEDOT:PSS-wrapped negative electrode powder:
[0040] Take 300-500 mg of precursor A and disperse it in deionized water. In this embodiment, the amount of precursor is 300 mg, the amount of deionized water is 10 ml, add an appropriate amount of PEDOT:PSS, in this embodiment, the amount of PEDOT:PSS is 3% of the mass of the precursor, stir until dry to obtain PEDOT:PSS-wrapped Bi 13 S 18 I2 negative electrode powder, in this embodiment, the stirring temperature is 80°C and the stirring speed is 500 rpm.
[0041] The difference between Examples 2 to 6 and Example 1 is only that the parameters shown in Table 1 are different.
[0042] Six groups of comparative examples were set up for experimental comparison with the bismuth-based nanomaterials provided in Examples 1-6. The parameters of Comparative Examples 1-6 are shown in Table 2:
[0043] Table 2
[0044]
[0045] The difference between Comparative Examples 1-6 and Examples 1-6 is only that the parameters shown in Table 2 are different.
[0046] The following tests were performed using the negative electrode materials provided in Examples 1-6 and Comparative Examples 1-6:
[0047] XRD (X-ray diffraction) characterization:
[0048] Figure 1 The XRD pattern of the sample prepared in Example 1 is given. Figure 1 It can be seen that there are strong diffraction peaks at 2θ = 23.8°, 28.3°, 29.8°, 31.9°, and 42.7°, and they are similar to Bi 13 S 18 The (120), (121), (201), (221), and (520) crystal planes of I2 in standard PDF#65-2345 are consistent, and no impurity peaks appear, proving that the synthesized material is pure Bi. 13 S 18 I2.
[0049] SEM Characterization:
[0050] Figure 2 The powder morphology prepared in Example 1 is shown. At the micron level, the powder is obviously antler-like. At the nanometer level, each antler-like morphology is as follows: Figure 3 As shown, each antler is composed of countless nanorods.
[0051] The morphologies prepared in Examples 2 to 6 are basically consistent with that in Example 1, and are antler-like nanostructures.
[0052] Electrochemical performance characterization:
[0053] The powder materials obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were assembled into button cells and charged at 0.1Ag -1 The charge and discharge test and cycle stability test were carried out under constant current conditions.
[0054] The preparation process of button batteries is as follows: in a glove box protected by argon atmosphere, the positive electrode shell, lithium sheet, diaphragm, LiPF6 electrolyte, negative electrode sheet, gasket, spring, and negative electrode shell are assembled in sequence, and finally the battery is packaged using a tablet press.
[0055] Bi prepared in Example 1 and Comparative Examples 4 and 6 13 S 18 Taking I2 negative electrode material as an example, the test results of the first charge and discharge and 15 cycles are as follows Figures 6 to 8 The initial charge and discharge results of Examples 1 to 6 and Comparative Examples 1 to 6 and the capacity results after 15 cycles are shown in Table 3.
[0056] Table 3
[0057]
[0058] The experiment proved that the prepared Bi with special nanostructure 13 S 18 The X2 negative electrode material can relieve volume stress to the greatest extent during the charge and discharge process, while reducing the migration distance of lithium ions, thereby improving the cycle stability of the material, and the PEDOT:PSS coating can not only improve the conductivity of the negative electrode material, but also suppress the expansion problem of the material during the charging process, thereby improving the material capacity and improving the capacity retention rate. Although the present invention is described herein with reference to a plurality of illustrative embodiments of the present invention, it should be understood that those skilled in the art can design many other modifications and implementations, which will fall within the scope and spirit of the principles disclosed in this application. More specifically, within the scope of the present application, the drawings and the claims, various modifications and improvements may be made to the components and / or layout of the subject combination layout. In addition to the deformation and improvement of the components and / or layout, other uses will also be obvious to those skilled in the art.
Claims
1. A method for preparing antler-shaped bismuth-based lithium battery negative electrode nanomaterial, Features: The steps include: (1) Preparation of Precursor A: According to the molecular formula, bismuth nitrate pentahydrate with a molar percentage is dissolved in ethylene glycol, thiourea is dissolved in deionized water, and after stirring until completely dissolved, the thiourea solution is slowly dripped into the bismuth nitrate solution, and then a molar percentage of Y is added, Y is selected as sodium halide, and an appropriate amount of polyvinyl pyrrolidone is added, and stirred at 70-100° C. After 10 minutes, it is transferred to a hydrothermal autoclave for heat preservation; after the reaction obtains a mixed solution, it is centrifuged and washed for more than 3 times, and dried for more than 12 hours to obtain a precursor A; (2) Preparation of PEDOT:PSS-coated negative electrode powder: Take 300-500 mg of precursor A and disperse it in deionized water, add an appropriate amount of PEDOT:PSS, and stir until dry to obtain PEDOT:PSS-wrapped Bi 13 S 18 X 2 Negative electrode powder, Bi 13 S 18 X 2 Where X is a halogen element.
2. The method for preparing a antler-shaped bismuth-based lithium battery negative electrode nanomaterial according to claim 1, Features: In the step (1), the amount of ethylene glycol is 0-75 ml, the amount of deionized water is 0-75 ml, the dissolution temperature is 80-100° C., and the stirring speed is 300-500 rpm.
3. A method for preparing a antler-shaped bismuth-based lithium battery negative electrode nanomaterial according to claim 1, Features: In the step (1), the amount of polyvinyl pyrrolidone is 0.02-0.1 g, the hydrothermal autoclave insulation temperature is 80-160° C., and the time is 6-18 h.
4. The method for preparing a antler-shaped bismuth-based lithium battery negative electrode nanomaterial according to claim 1, Features: In the step (1), the centrifuge speed is 3000-5000 rpm, the time is 3-5 min, and the drying temperature is 60-80°C.
5. The method for preparing a antler-shaped bismuth-based lithium battery negative electrode nanomaterial according to claim 1, Features: In the step (2), the amount of deionized water is 10-20 ml, the amount of PEDOT:PSS added is 3-7% of the mass of the precursor, the stirring temperature is 80-100° C., and the stirring speed is 300-500 rpm.
6. Application of the material prepared by the method for preparing a antler-shaped bismuth-based lithium battery negative electrode nanomaterial according to any one of claims 1 to 5 in a battery.