Manufacturing method of all-solid-state batteries containing solid electrolyte materials

By employing a stepwise pressurization method, the reaction problem between lithium metal and sulfide-based solid electrolyte materials during the pressurization process was solved, achieving high yield and low porosity of solid-state batteries and improving battery performance.

CN115777158BActive Publication Date: 2026-11-17LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180047154.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-07-08
Filing Date
2021-07-08
Publication Date
2026-11-17
Estimated Expiration
2041-07-08

AI Technical Summary

Technical Problem

In existing solid-state battery manufacturing methods, lithium metal and sulfide-based solid electrolyte materials are prone to react during pressurization, leading to short circuits. Furthermore, the porosity of the solid electrolyte membrane is difficult to reduce, affecting the battery yield.

Method used

A stepwise pressurization method is adopted. First, the positive electrode and the first solid electrolyte membrane are pressurized. Then, the second solid electrolyte membrane is prepared and pressurized. Then, it is stacked with the negative electrode and pressurized. The pressure and temperature of each step are controlled to prevent reaction and reduce porosity.

Benefits of technology

It effectively prevents the reaction between lithium metal and sulfide-based solid electrolyte materials, reduces the porosity of the solid electrolyte membrane, improves the yield and ion conductivity of the battery, and avoids short circuits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115777158B_ABST
    Figure CN115777158B_ABST
Patent Text Reader

Abstract

This invention relates to a method for manufacturing a solid-state battery. The method controls the reaction between the negative electrode and the solid electrolyte membrane during pressurization to bond the electrode elements together. In particular, when the negative electrode contains lithium metal and the solid electrolyte membrane contains a sulfide-based solid electrolyte material, the invention can control the reaction between the lithium metal and the sulfide-based solid electrolyte material. Furthermore, the solid-state battery obtained by the method of this invention exhibits low porosity in both the positive electrode and the solid electrolyte membrane, preventing short circuits by suppressing the reaction between the solid electrolyte membrane and the lithium metal at the negative electrode, and providing improved battery yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims priority to Korean Patent Application No. 10-2020-0084326, filed in Korea on July 8, 2020. The present invention relates to a solid-state battery comprising a solid electrolyte material and a method for manufacturing the same. Background Technology

[0002] Typically, solid-state batteries are manufactured by sequentially stacking a negative electrode, a solid electrolyte membrane, and a positive electrode, and then pressurizing the resulting structure to achieve interlayer bonding. Since such solid-state batteries do not use a liquid electrolyte, it is important that the electrode devices are tightly bonded together rather than spaced apart to prevent increased interfacial resistance. Reducing porosity through the pressurization process is also crucial, as this improves ionic conductivity.

[0003] Figure 1 This is a schematic diagram illustrating the manufacturing method of solid-state batteries using related technologies. (Reference) Figure 1 A positive electrode (comprising a positive electrode active material layer 1 formed on one surface of a positive electrode current collector 2), a solid electrolyte membrane 5, and a negative electrode (comprising a negative electrode active material layer 4 formed on one surface of a negative electrode current collector 3) are stacked sequentially, and then the resulting structure is immediately pressurized to obtain an electrode assembly 100. Since solid-state batteries do not use a liquid electrolyte, strong pressure can be applied to ensure close contact between the electrode active material and the solid electrolyte material, which acts as an ion conductor, and to minimize unused spaces (pores) where electrochemical reactions do not occur. However, when lithium metal is used as the negative electrode material and a solid electrolyte membrane containing sulfide-based solid electrolyte materials is used, the lithium metal may react with the sulfide-based solid electrolyte material during pressurization, leading to a short circuit. Therefore, in this case, the battery yield of this method is low. Simultaneously, when the applied pressure is reduced to control the reaction between the negative electrode and the solid electrolyte membrane, the porosity of the solid electrolyte membrane may not decrease to the desired level.

[0004] In this context, a new solid-state battery manufacturing method is needed that can prevent the reaction between lithium metal and sulfide-based solid electrolyte materials, maintain the low porosity of the solid electrolyte membrane, and exhibit high battery yield. Summary of the Invention

[0005] [Technical Issues]

[0006] This invention aims to address the problems of related technologies, and therefore aims to provide a method for manufacturing a solid-state battery that prevents the reaction between lithium metal and a solid electrolyte layer to provide a high battery yield. It is readily understood that the objects and advantages of this invention can be achieved by the means shown in the appended claims and combinations thereof.

[0007] [Technical Solution]

[0008] According to a first embodiment of the present invention, a method for manufacturing a solid-state battery is provided, comprising the following steps: S1) a first pressurization step: stacking a positive electrode and a first solid electrolyte membrane and pressurizing the resulting structure to obtain a positive electrode component; S2) a second pressurization step: preparing a second solid electrolyte membrane and pressurizing the second solid electrolyte membrane; S3) a third pressurization step: sequentially stacking the positive electrode component, the pressurized second solid electrolyte membrane, and the negative electrode, and pressurizing the resulting structure to obtain an electrode assembly.

[0009] According to a second embodiment of the present invention, a method for manufacturing a solid-state battery as defined in the first embodiment is provided, wherein the first pressurization step is performed at a temperature of 15-30°C and a pressure of 300-600 MPa.

[0010] According to a third embodiment of the present invention, a method for manufacturing a solid-state battery as defined in the first or second embodiment is provided, wherein the porosity of the first solid electrolyte membrane in the positive electrode component is 45-60% by volume.

[0011] According to a fourth embodiment of the present invention, a method for manufacturing a solid-state battery as described in any one of the first to third embodiments is provided, wherein the second pressurization step is performed at a temperature of 15-30°C and a pressure of 300-600 MPa.

[0012] According to a fifth embodiment of the present invention, a method for manufacturing a solid-state battery as described in any one of the first to fourth embodiments is provided, wherein the third pressurization step is performed at a pressure lower than the pressure applied in each of the first and second pressurization steps.

[0013] According to a sixth embodiment of the present invention, a method for manufacturing a solid-state battery as described in any one of the first to fifth embodiments is provided, wherein the third pressurization step is performed at a pressure of 100-300 MPa.

[0014] According to a seventh embodiment of the present invention, a method for manufacturing a solid-state battery as described in any one of the first to sixth embodiments is provided, wherein the negative electrode comprises a current collector and an electrode active material layer formed on the surface of the current collector, the electrode active material layer comprising lithium metal.

[0015] According to an eighth embodiment of the present invention, a method for manufacturing a solid-state battery as defined in any one of the first to seventh embodiments is provided, wherein the first and second solid electrolyte membranes each comprise a solid electrolyte material, the solid electrolyte material including a sulfide-based solid electrolyte material.

[0016] According to a ninth embodiment of the present invention, a method for manufacturing a solid-state battery as described in any one of the first to eighth embodiments is provided, wherein a third pressurization step is performed at a pressure lower than the pressure applied in each of the first and second pressurization steps, the negative electrode comprises lithium metal as a negative electrode active material, the first and second solid electrolyte membranes each comprise a solid electrolyte material, and the solid electrolyte material comprises a sulfide-based solid electrolyte material.

[0017] According to a tenth embodiment of the present invention, a method for manufacturing a solid-state battery as described in any one of the first to ninth embodiments is provided, wherein, in the first pressurization step, the positive electrode is surrounded at its edge by a protective member, thereby preventing damage to the solid electrolyte membrane.

[0018] [Beneficial Effects]

[0019] The solid-state battery manufacturing method according to embodiments of the present invention controls the reaction between the negative electrode and the solid electrolyte membrane during the pressurization process that bonds the electrode devices together. In particular, when the negative electrode contains lithium metal and the solid electrolyte membrane contains a sulfide-based solid electrolyte material, the reaction between the lithium metal and the sulfide-based solid electrolyte material can be prevented. Furthermore, the solid-state battery obtained by the solid-state battery manufacturing method according to embodiments of the present invention exhibits low porosity in both the positive electrode and the solid electrolyte membrane, preventing short circuits by suppressing the reaction between the solid electrolyte membrane and the lithium metal at the negative electrode, and providing improved battery yield. Attached Figure Description

[0020] The accompanying drawings illustrate preferred embodiments of the invention and, together with the foregoing disclosure, serve to provide a further understanding of the technical features of the invention. Therefore, the invention should not be construed as limited to the drawings. Furthermore, for clarity, the shape, size, scale, or proportion of certain constituent elements in the drawings may be exaggerated.

[0021] Figure 1 This is a schematic diagram illustrating the solid-state battery manufacturing method of the relevant technology.

[0022] Figures 2a to 2c This is a schematic diagram illustrating the solid-state battery manufacturing method according to an embodiment of the present invention.

[0023] Figure 3 An embodiment is shown in which the positive electrode is surrounded by a protective component at its edge during the first pressurization step.

[0024] Figure 4 This is a graph showing the charge / discharge curve of the battery in Example 1.

[0025] Figure 5 This is a graph showing the charge / discharge curves of the battery in Comparative Example 1. Detailed Implementation

[0026] Preferred embodiments of the invention will be described in detail below with reference to the accompanying drawings. Before description, it should be understood that the terminology used in the specification and appended claims should not be construed as limited to its general or dictionary meaning, but rather is interpreted based on the principle of allowing the inventors to appropriately define terms for best interpretation, and on the meanings and concepts corresponding to the technical aspects of the invention. Therefore, the description presented herein is merely a preferred example, for illustrative purposes only, and is not intended to limit the scope of the invention. It should be understood that other equivalent substitutions and modifications can be made without departing from the scope of the invention.

[0027] Throughout the specification, the statement "a component includes one element" does not preclude the existence of any additional elements, but rather means that the component may further include other elements, unless otherwise stated.

[0028] As used herein, the terms “about,” “substantially,” etc., are used to indicate that the stated numerical values ​​extend to the vicinity to represent acceptable manufacturing and material errors specific to the meaning of the statement, and to prevent unethical infringers from improperly using the disclosure, which includes accurate or absolute numerical values. Providing accurate or absolute numerical values ​​is to aid in understanding the invention.

[0029] As used in this article, the expression "A and / or B" means "A, B, or both of them".

[0030] This invention relates to a method for manufacturing a solid-state battery using a solid electrolyte as the electrolyte material. According to embodiments of the invention, the solid-state battery can be a lithium-ion secondary battery.

[0031] Figures 2a to 2c This is a schematic diagram illustrating a solid-state battery manufacturing method according to an embodiment of the present invention. The solid-state battery manufacturing method according to an embodiment of the present invention will be explained in more detail below with reference to the accompanying drawings.

[0032] First, a positive electrode, a first solid electrolyte membrane, a second solid electrolyte membrane, and a negative electrode are prepared.

[0033] According to an embodiment of the present invention, first and second solid electrolyte membranes are disposed between a negative electrode and a positive electrode, such that the negative and positive electrodes are electrically insulated from each other, and are configured as ion transport channels between the negative and positive electrodes. Each solid electrolyte membrane can be prepared in the form of a sheet comprising a solid electrolyte material. If desired, each solid electrolyte membrane may further comprise an adhesive resin to give the membrane shape-retaining stability.

[0034] The solid electrolyte material may include at least one selected from sulfide-based solid electrolyte materials, oxide-based solid electrolyte materials, and polymeric solid electrolyte materials. According to an embodiment of the invention, preferably, the first and second solid electrolyte membranes may each contain a sulfide-based solid electrolyte material. According to an embodiment of the invention, the first and second solid electrolyte membranes may contain only sulfide-based solid electrolyte materials as solid electrolyte materials.

[0035] According to the present invention, the method for preparing the solid electrolyte membrane is not limited to a specific method, as long as the solid electrolyte membrane can be prepared in the form of a sheet containing solid electrolyte material. For example, the solid electrolyte membrane can be prepared as follows: introducing solid electrolyte material into a solvent to prepare a slurry for forming the electrolyte membrane, coating the slurry onto a release film, and then drying. The release film is removed from the solid electrolyte membrane, and then the positive electrode and the solid electrolyte membrane are stacked in the steps described below.

[0036] According to the present invention, the first solid electrolyte membrane may be the same as or different from the second solid electrolyte membrane.

[0037] According to embodiments of the present invention, the solvent used to prepare the solid electrolyte membrane can be a nonpolar solvent. When sulfide-based solid electrolyte components come into contact with polar solvents, their physical properties may deteriorate, such as reduced ionic conductivity. Therefore, according to the present invention, nonpolar solvents can be used as solvents for manufacturing batteries. Nonpolar solvents may include solvents with a polarity index of 0-3 and / or a dielectric constant less than 5. When such nonpolar solvents are used, the reduction in ionic conductivity of sulfide-based solid electrolytes caused by the use of polar solvents can be prevented. Non-limiting examples of nonpolar solvents include pentane, cyclohexane, toluene, benzene, xylene, hexane, anisole, heptane, chloroform, diethyl ether, butyl butyrate, etc. These solvents can be used alone or in combination.

[0038] The negative electrode includes a negative electrode current collector 30 and a negative electrode active material layer 40 formed on the surface of the negative electrode current collector. The negative electrode active material layer may contain lithium metal as the negative electrode active material. The negative electrode active material layer may be configured as a lithium metal foil stacked on the surface of the current collector. In a variation, the negative electrode active material layer may be formed by electrodepositing metal on the surface of the current collector or by a chemical or physical vapor deposition process.

[0039] The positive electrode includes a positive electrode current collector 20 and a positive electrode active material layer 10 formed on the surface of the current collector. The active material layer may include a plurality of electrode active material particles and a solid electrolyte material. According to embodiments of the present invention, if desired, the positive electrode may further include at least one of a conductive material and a binder resin. Furthermore, the positive electrode may further include various additives to supplement or improve electrochemical performance. According to the present invention, the method of manufacturing the positive electrode is not limited to a specific method, as long as the positive electrode can be prepared in the form of a sheet containing the positive electrode active material and the solid electrolyte. For example, the positive electrode may be manufactured as follows: introducing the positive electrode active material and the solid electrolyte material into a solvent to prepare a slurry for forming the positive electrode, coating the slurry onto the current collector, and then drying it.

[0040] The positive electrode active material is not limited to a specific composition, as long as it can be used as a positive electrode active material for lithium-ion secondary batteries. Non-limiting examples of positive electrode active materials include any of the following: layered compounds, such as lithium manganese composite oxides (LiMn2O4, LiMnO2, etc.), lithium cobalt oxides (LiCoO2), and lithium nickel oxides (LiNiO2), or those compounds substituted with one or more transition metals; lithium manganese oxides, such as those composed of the chemical formula Li... 1+x Mn 2-x Those represented by O4 (where x is 0-0.33), LiMnO3, LiMn2O3 and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides, such as LiV3O8, LiV3O4, V2O5 or Cu2V2O7; and those represented by the chemical formula LiNi. 1-x M x Ni-type lithium nickel oxide represented by O2 (where M is Co, Mn, Al, Cu, Fe, Mg, B, or Ga, and x is 0.01-0.3); LiMn 2-x M x Lithium manganese composite oxides represented by O2 (where M is Co, Ni, Fe, Cr, Zn, or Ta, and x is 0.01-0.1) or Li2Mn3MO8 (where M is Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which Li is partially substituted by alkaline earth metal ions; disulfides; and Fe2(MoO4)3; or mixtures of two or more thereof. According to the present invention, the positive electrode may include at least one of polymer solid electrolytes, oxide solid electrolytes, and sulfide solid electrolytes as a solid electrolyte material.

[0041] Next, the positive electrode and the first solid electrolyte membrane 50a are stacked, and a pressurization step (first pressurization step) is performed to prepare the positive electrode component. The positive electrode includes a positive electrode current collector 20 and a positive electrode active material layer 10 formed on the surface of the current collector. The positive electrode component is a product obtained by bringing the positive electrode and the first solid electrolyte membrane into close contact with each other and / or bonding them together. During pressurization, the first solid electrolyte membrane is stacked in such a way that it can face the positive electrode active material layer. The first pressurization step can be performed at room temperature. As used herein, the term "room temperature" refers to a temperature controlled within a predetermined range of 15-30°C. For example, the term "room temperature" can refer to a temperature of 18°C ​​to 25°C. The pressure applied during the pressurization step can be controlled at about 300-600 MPa. According to an embodiment of the invention, in order to reduce the porosity of the positive electrode and the first solid electrolyte membrane, the pressurization step can preferably maintain a pressure of about 450 MPa or more within the above range. For example, the pressurization can be controlled at a pressure of about 450-550 MPa. Meanwhile, the pressurization can be performed for 1-30 minutes. Meanwhile, the positive electrode and the first solid electrolyte membrane obtained after the first pressurization step preferably each maintain a porosity of 45-60% by volume. However, the pressure or time in the first pressurization step is not limited to a specific range and can be appropriately controlled by taking into account the thickness of the positive electrode and / or the thickness of the solid electrolyte membrane, the desired porosity level, etc.

[0042] In addition, a pressurization step (second pressurization step) is performed on the second solid electrolyte membrane 50b.

[0043] The second pressurization step can be performed at room temperature (15-30°C). The pressure applied in this pressurization step can be controlled at about 300-600 MPa. According to one embodiment of the invention, in order to reduce the porosity of the second solid electrolyte membrane, the pressurization step can preferably maintain a pressure of about 450 MPa or higher within the above range. For example, the pressurization can be controlled at about 450-550 MPa. Simultaneously, the pressurization can be carried out for 1-30 minutes. Meanwhile, the second solid electrolyte membrane obtained after the second pressurization step preferably maintains a porosity of 45-60% by volume. However, the pressure or time in the second pressurization step is not limited to a specific range and can be appropriately controlled taking into account the thickness of the second solid electrolyte membrane or the desired porosity level.

[0044] Then, the positive electrode component and the negative electrode are stacked sequentially and a pressurization step (third pressurization step) is performed to obtain the electrode assembly 200. The negative electrode includes a negative electrode current collector 30 and a negative electrode active material layer 40 formed on the surface of the negative electrode current collector.

[0045] According to an embodiment of the invention, the pressure applied in the third pressurization step is controlled to be lower than the pressure applied in each of the first and second pressurization steps. In the third pressurization step, the first solid electrolyte membrane 50a and the second solid electrolyte membrane 50b bond together to form a single solid electrolyte membrane 50. In other words, the first and second solid electrolyte membranes merge together through the bonding of their facing interface portions, thus making the interface portions unclear or completely eliminated, thereby forming a single solid electrolyte membrane 50.

[0046] The third pressurization step can be performed at room temperature (15-30°C). The pressure applied in the third pressurization step is controlled at approximately 100-300 MPa, provided that the pressure is lower than the pressure applied in the second pressurization step. The third pressurization step can be performed for 1-5 minutes. Furthermore, in the electrode assembly obtained after the third pressurization step, the porosity of the individual solid electrolyte membrane provided by the combination of the first and second solid electrolyte membranes is 1-10% by volume. Additionally, the porosity of the positive electrode in the electrode assembly is preferably maintained at a level of 1-20% by volume.

[0047] Furthermore, according to the present invention, porosity can be determined by using the relationship between true density and apparent density [(1-true density) / (apparent density)], the weight and thickness of the test object.

[0048] Because the solid electrolyte membrane undergoes two pressurization steps, the resulting electrode assembly can have reduced porosity and improved ion conductivity. Preferably, the porosity of the solid electrolyte membrane can be controlled to be below 5% by volume. Furthermore, the solid electrolyte membrane and the negative electrode are bonded together through a third pressurization step, wherein the pressure applied in the third pressurization step is lower than the pressure applied in each of the first and second pressurization steps. Therefore, since the lamination process is performed under such low-pressure conditions, the reaction between the negative electrode and the solid electrolyte membrane can be suppressed.

[0049] According to the present invention, the pressurization step can be any process, as long as it ensures the bonding between the positive electrode and the solid electrolyte membrane and a suitable porosity level. According to embodiments of the present invention, pressurization can be performed by a method appropriately selected from known pressurization processes, such as rolling, compression pressing, and cold isostatic pressing (CIP), and is not limited to any particular process.

[0050] Furthermore, according to an embodiment of the present invention, a protective component can be disposed on the edge of the positive electrode during the first pressurization step. Typically, to electrically insulate the positive and negative electrodes from each other and prevent short circuits between the two electrodes, the solid electrolyte membrane is prepared to have an area larger than the electrodes, and the positive and negative electrodes are disposed within the solid electrolyte membrane during the lamination process of the electrodes and the solid electrolyte membrane. Therefore, since the positive electrode has a smaller area compared to the solid electrolyte membrane, the surface of the solid electrolyte membrane may be damaged by the edge of the positive electrode during the pressurization step. Therefore, when a protective component capable of compensating for this area difference between the positive electrode and the solid electrolyte membrane is disposed at the entire or at least a portion of the positive electrode edge, and then the pressurization step is performed, damage to the solid electrolyte membrane can be prevented. Furthermore, according to an embodiment of the present invention, the protective component can be removed after the pressurization step.

[0051] Figure 3 An embodiment of a protective member 60 disposed corresponding to the area difference between the positive electrode and the solid electrolyte membrane is shown. When the protective member is disposed, the side portions of the protective member and the side portions of the positive electrode can be disposed in such a way that they are not separated from each other but can contact each other. More preferably, the external dimensions of the protective member can be equal to or larger than the dimensions of the solid electrolyte membrane, such that the surface of the solid electrolyte membrane exposed due to the area difference with the positive electrode can be completely covered by the protective member. In other words, it is preferable that the protective member is disposed in such a way that the surface of the solid electrolyte membrane is not squeezed and deformed by the outer edge or edge of the protective member. Furthermore, the protective member preferably has the same height as the positive electrode. When the protective member has the same height as the positive electrode, uniform pressure can be applied to the entire solid electrolyte membrane through the protective member and the positive electrode during the pressurization step.

[0052] According to embodiments of the present invention, the material of the protective component is not particularly limited, as long as it does not damage the solid electrolyte membrane during pressurization, can be removed after pressurization, and does not damage the positive electrode or the solid electrolyte membrane. For example, the protective component may include an insulating polymer resin. According to embodiments of the present invention, the insulating polymer resin may include an elastic material, such as styrene-butadiene rubber (SBR).

[0053] Furthermore, according to the present invention, the current collector comprises a metal plate having electronic conductivity, and can be appropriately selected according to the polarity of the electrodes known in the field of secondary batteries.

[0054] According to the present invention, the amount of conductive material added is typically 1-30% by weight, based on the total weight of the mixture containing the electrode active materials. There are no particular limitations on the conductive material, as long as it does not cause a chemical change in the corresponding battery and is conductive. For example, conductive materials include any of the following: graphite, such as natural or artificial graphite; carbon black, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lampblack, or thermally cracked black; conductive fibers, such as carbon fibers or metal fibers; metal powders, such as fluorinated carbon, aluminum, or nickel powder; conductive whiskers, such as zinc oxide or potassium titanate; conductive metal oxides, such as titanium oxide; and conductive materials such as polyphenylene derivatives, or mixtures of two or more thereof.

[0055] According to the present invention, the adhesive resin is not particularly limited, as long as it is a component that facilitates the bonding of the electrode active material with the conductive material and with the current collector. Specific examples of adhesive resins include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers. Typically, based on 100% by weight of the electrode active material layer, the amount of adhesive resin can be 1-30% by weight, or 1-10% by weight.

[0056] Furthermore, according to the present invention, if necessary, each electrode active material layer may include at least one additive, such as an oxidation stabilizer, a reduction stabilizer, a flame retardant, a heat stabilizer, an anti-fogging agent, etc.

[0057] According to the present invention, the sulfide-based solid electrolyte contains sulfur (S), has the conductivity of a metal ion belonging to Group 1 or Group 2 of the periodic table, and may include Li-PS glass or Li-PS glass-ceramic. Non-limiting examples of sulfide-based solid electrolytes include at least one of the following: Li₂S-P₂S₅, Li₂S-LiI-P₂S₅, Li₂S-LiI-Li₂O-P₂S₅, Li₂S-LiBr-P₂S₅, Li₂S-Li₂O-P₂S₅, Li₂S-Li₃PO₄-P₂S₅, Li₂S-P₂S₅-P₂O₅, Li₂S-P₂S₅-SiS₂, Li₂S-P₂S₅-SnS, Li₂S-P₂S₅-Al₂S₃, Li₂S-GeS₂, Li₂S-GeS₂-ZnS, etc. However, the scope of the present invention is not limited thereto.

[0058] Furthermore, oxide-based solid electrolytes contain oxygen (O) and possess the conductivity of metal ions from Group 1 or Group 2 of the periodic table. Non-limiting examples of oxide-based solid electrolytes include at least one of the following: LLTO compounds, Li6La2CaTa2O 12 Li6La2ANb2O 12 (where A is Ca or Sr), Li2Nd3TeSbO 12 Li3BO 2.5 N 0.5 Li9SiAlO8, LAGP compounds, LATP compounds, Li 1+x Ti 2-x Al x Si y (PO4) 3-y (where 0≤x≤1, 0≤y≤1), LiAl x Zr 2-x (PO4)3 (where 0 ≤ x ≤ 1, 0 ≤ y ≤ 1), LiTi x Zr 2-x (PO4)3 (where 0≤x≤1, 0≤y≤1), LISICON compounds, LIPON compounds, perovskite compounds, NASICON compounds, and LLZO compounds. However, the scope of the invention is not limited thereto.

[0059] Regarding solid electrolyte materials, in the case of the positive electrode, an electrolyte material with high oxidation stability can be used as the solid electrolyte. Furthermore, in the case of the negative electrode, an electrolyte with high reduction stability can be used as the solid electrolyte. However, the scope of the present invention is not limited thereto. Since the main function of the solid electrolyte is to conduct lithium ions in the electrode, any material with high ionic conductivity can be used, such as 10... -7 S / cm or higher, or 10 -5 The S / cm ratio is above 1, and the solid electrolyte material is not limited to any specific composition.

[0060] In another aspect of the invention, a secondary battery having the above-described structure is provided. A battery module including the secondary battery as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source are also provided. Specific examples of this device may include, but are not limited to: power tools driven by an electric motor; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), etc.; electric freight vehicles, including electric bicycles (E-bicycles) and electric scooters (E-scooters); electric golf carts; power storage systems; etc.

[0061] Embodiments will be described more fully below to facilitate a better understanding of the invention. However, the following embodiments are for illustrative purposes only, and the scope of the invention is not limited thereto.

[0062] [Example]

[0063] (1) Electrode preparation

[0064] Example 1

[0065] First, LiNi, as the positive electrode active material, 0.8 Co 0.1 Mn 0.1 O2, Li2S-P2S5 as a solid electrolyte, nitrile rubber (NBR) as a binder, and vapor-grown carbon fiber (VGCF) as a conductive material were introduced into anisole in a weight ratio of 75.5:22.1:1.5:1 to prepare a slurry (70% by weight solids) for forming the positive electrode active material layer. This slurry was coated onto one surface of an aluminum foil (thickness: approximately 10 μm) and dried at 60 °C for 6 hours to prepare the positive electrode.

[0066] Next, Li₂S-P₂S₅ as the solid electrolyte and NBR as the binder were introduced into anisole at a weight ratio of 95:5 to prepare a slurry (60% by weight of solids) for forming a solid electrolyte membrane. The slurry was prepared by mixing these components at 2000 rpm for 1 minute in a Thinkky mixer. This slurry was coated onto one surface of a release sheet made of polyethylene terephthalate and dried overnight at room temperature and atmospheric pressure. The release sheet was then removed to prepare the first solid electrolyte membrane. Furthermore, a second solid electrolyte membrane was prepared in the same manner as described above. Both the first and second solid electrolyte membranes had a thickness of 30 μm.

[0067] Next, the negative electrode is prepared. A 20 μm thick lithium metal foil is attached to the surface of a 10 μm thick nickel foil current collector to prepare the negative electrode.

[0068] Next, the positive electrode and the first solid electrolyte membrane were stacked, and the resulting structure was pressurized at 500 MPa for 5 minutes to laminate the positive electrode and the first solid electrolyte membrane, obtaining a laminate. In the obtained laminate, the porosity of the positive electrode was 15% by volume, and the porosity of the first solid electrolyte membrane was 50% by volume. Furthermore, the second solid electrolyte membrane was pressurized at 500 MPa for 5 minutes. The porosity of the resulting second solid electrolyte membrane was 50% by volume. Then, the above laminate, the second solid electrolyte membrane, and the negative electrode were stacked sequentially, and the resulting structure was pressurized at 200 MPa for 5 minutes to obtain an electrode assembly. In the obtained electrode assembly, the porosity of the positive electrode was 15% by volume, and the porosity of the solid electrolyte membrane was 5% by volume. Each pressurization was performed using a cold isostatic pressing (CIP) machine.

[0069] Example 2

[0070] The electrode assembly was obtained in the same manner as in Example 1, except that a pressure of 450 MPa was applied in the first and second pressurization steps, and a pressure of 100 MPa was applied in the third pressurization step.

[0071] Comparative Example 1

[0072] A positive electrode, a negative electrode, and a solid electrolyte membrane (60 μm) were prepared and stacked sequentially in the same manner as in Example 1. The resulting structure was pressurized at 500 MPa for 5 minutes to obtain the electrode assembly. In the resulting electrode assembly, the porosity of the positive electrode was 20% by volume, and the porosity of the solid electrolyte membrane was 10% by volume. Pressurization was performed using a cold isostatic pressing (CIP) machine.

[0073] Comparative Example 2

[0074] The electrode assembly was obtained in the same manner as in Comparative Example 1, except that a pressure of 450 MPa was applied.

[0075] (2) Comparison results of electrochemical performance

[0076] Solid-state batteries were obtained using each electrode assembly of Examples 1 and 2 and Comparative Examples 1 and 2. Each battery was repeatedly charged / discharged three times to determine the open-circuit voltage (OCV). Each battery was charged at 0.1C to 4.25V (0.01C cutoff) in constant-current-constant-voltage (CC-CV) mode and discharged at 0.1C to 3V. The open-circuit voltage was determined using a voltmeter available from Hioki. The initial charge / discharge results of Examples 1 and 2 and Comparative Examples 1 and 2 are shown in Table 1 below. In the cases of Comparative Examples 1 and 2, each battery exhibited a low charge / discharge efficiency (approximately 43%), indicating a deterioration in battery quality. Meanwhile, in the cases of Examples 1 and 2, each battery exhibited a high charge / discharge efficiency of up to approximately 93%. Furthermore, Figure 4(Example 1) and Figure 5 (Comparative Example 1) shows the first to third charge / discharge curves of Example 1 and Comparative Example 1. The results show that the battery of Comparative Example 1 has a high irreversible capacity and cannot achieve sufficient discharge capacity. Therefore, the battery quality is lower than that of Example 1.

[0077] [Table 1]

[0078] Example 1 Example 2 Comparative Example 1 Comparative Example 2 OCV(V) 3.012 3.013 1.853 1.921

Claims

1. A method for manufacturing a solid-state battery, comprising the following steps: S1) First pressurization step: Stack the positive electrode and the first solid electrolyte membrane and pressurize the resulting structure to obtain the positive electrode component; S2) Second pressurization step: preparing the second solid electrolyte membrane and pressurizing the second solid electrolyte membrane; and S3) Third pressurization step: Stack the positive electrode component, the pressurized second solid electrolyte membrane and the negative electrode in sequence, and pressurize the resulting structure to obtain the electrode assembly; The third pressurization step is performed at a pressure lower than that applied in each of the first and second pressurization steps. The negative electrode contains lithium metal as the negative electrode active material, and the first and second solid electrolyte membranes each contain a solid electrolyte material, wherein the solid electrolyte material contains a sulfide-based solid electrolyte material.

2. The method for manufacturing a solid-state battery as described in claim 1, wherein, The first pressurization step is carried out at a temperature of 15 to 30°C and a pressure of 300 to 600 MPa.

3. The method for manufacturing a solid-state battery as described in claim 1, wherein, The porosity of the first solid electrolyte membrane in the positive electrode component is 45 to 60% by volume.

4. The method for manufacturing a solid-state battery as described in claim 1, wherein, The second pressurization step is carried out at a temperature of 15 to 30°C and a pressure of 300 to 600 MPa.

5. The method for manufacturing a solid-state battery as described in claim 1, wherein, The third pressurization step is carried out at a temperature of 15 to 30°C.

6. The method for manufacturing a solid-state battery as described in claim 1, wherein, The third pressurization step is carried out at a pressure of 100 to 300 MPa.

7. The method for manufacturing a solid-state battery as described in claim 1, wherein, The negative electrode includes a current collector and an electrode active material layer formed on the surface of the current collector, the electrode active material layer comprising lithium metal.

8. The method for manufacturing a solid-state battery according to any one of claims 1 to 7, wherein, In the first pressurization step, the positive electrode is surrounded by a protective component at its edges to prevent damage to the solid electrolyte membrane.

Citation Information

Patent Citations

  • Hydroponic cultivation device and hydroponic cultivation method

    KR1020200084326A

  • Method of producing solid electrolyte-electrode assembly

    CN102122711A

  • All solid battery and manufacturing method therefor

    JP2014216131A