A kind of electrolyte durable coding tape and preparation method thereof

By using a pressure-sensitive adhesive layer and curing agent combination of a specific composition in the lithium battery tape, the problem of poor durability and high temperature performance of the lithium battery tape in the electrolyte is solved, and long-term adhesion and protection at 85°C are achieved. The corrosive effect extends the service life of lithium battery tape.

CN115820157BActive Publication Date: 2024-10-11GUANGDONG DONGLI NEW MATERIALS SCI & TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211131713.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-15
Publication Date
2024-10-11
Estimated Expiration
2042-09-15

AI Technical Summary

Technical Problem

Existing lithium battery tapes have low durability and poor high temperature resistance in the electrolyte, resulting in reduced adhesion and dissolution, affecting the safety performance and traceability of lithium batteries.

Method used

An electrolyte durable engraving tape including a base layer, a pressure-sensitive adhesive layer and a release layer is used. The pressure-sensitive adhesive layer is composed of an acrylic material and a curing agent. It is composed of lauryl methacrylate and glycidyl methacrylate. The mass ratio adjusts the molecular weight and cross-linking degree, and combines the use of isocyanate and epoxy curing agents to improve the adhesiveness and thermal stability of the tape.

Benefits of technology

It can maintain adhesion performance for a long time at 85°C, prevent electrolyte corrosion and stabilize viscosity, significantly improve the electrolyte durability and thermal stability of lithium battery tape, and extend the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003848177380000081
    Figure BDA0003848177380000081
  • Figure BDA0003848177380000091
    Figure BDA0003848177380000091
Patent Text Reader

Abstract

The present invention relates to the field of lithium battery assembly, in particular to the field of IPC D09J133, and specifically to a durable electrolyte coding tape and a preparation method thereof. The pressure-sensitive adhesive layer of the durable electrolyte coding tape is measured by mass, including 45-65 parts of isooctyl acrylate, 15-20 parts of butyl acrylate, 1-5 parts of acrylic acid, 1-3 parts of hydroxybutyl acrylate, 10-15 parts of lauryl acrylate, 5-15 parts of isobornyl acrylate, 0.5-1 parts of azobisisobutyronitrile, 100-200 parts of ethyl acetate, 5-10 parts of lauryl methacrylate, 1-10 parts of glycidyl methacrylate, 3-10 parts of curing agent, and 3-15 parts of color paste. The durable electrolyte coding tape provided by the present invention has good adhesion, does not fade, can withstand long-term immersion of electrolyte at high temperature, and effectively solves the problem of low durability of lithium battery tape electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium battery assembly, in particular to the field of IPC C09J133, and specifically to an electrolyte durable coding tape and a preparation method of the electrolyte durable coding tape. Background Art

[0002] As new energy vehicles and other electric-powered products become more and more popular, the safety performance of lithium batteries has become a problem of great concern to the society. In the production and assembly process of lithium batteries, lithium battery tape has an impact on the safety performance of lithium batteries that cannot be ignored. Lithium battery tape is generally used for insulation and fixed protection of electrode windings, cell terminations, and pole pieces during the production and assembly of lithium batteries. This requires that the lithium battery tape needs to have certain initial adhesion, sustained adhesion, high temperature resistance, and electrolyte corrosion resistance. Today, the market has higher and higher requirements for the controllability and traceability of lithium battery product quality. Engraving a QR code on the lithium battery tape can well complete the traceability of lithium batteries.

[0003] In recent years, the lithium battery assembly field has a great demand for the electrolyte durability of lithium battery tape. During the lithium battery assembly process and in later applications, the lithium battery tape will directly contact the electrolyte, which requires the tape to withstand long-term immersion in the electrolyte without losing its viscosity and dissolving impurities to pollute the electrolyte. The tape in the prior art will fade to varying degrees, have reduced adhesion, and have a slight swelling of the adhesive layer after being immersed in the electrolyte, which fails to improve or solve the problem of electrolyte durability of lithium battery tape.

[0004] Chinese patent application CN204676029U discloses a new type of pressure-sensitive tape, the structure of which is to bond a combination of a PET base layer and an adhesive layer into two layers, which effectively improves the electrolyte corrosion resistance and puncture resistance of the pressure-sensitive tape. However, as the preparation of electronic products becomes thinner and lighter, the thickness requirements for lithium batteries and lithium battery materials are also thinner and lighter. It is not enough to improve the electrolyte durability only by structural modification. It is also necessary to study the pressure-sensitive adhesive layer to solve the fundamental problem of the adhesive layer's resistance to electrolyte. Chinese patent application CN103911088A discloses an acrylate pressure-sensitive tape, a preparation method thereof, and a lithium-ion battery, which prepares an acrylate pressure-sensitive tape by an acrylate copolymer obtained by polymerization of a combination of specific acrylate monomers. The tape maintains its original color when immersed in an electrolyte at 90°C for 48 hours, but its viscosity decreases and the periphery of the sample is warped after being immersed in the electrolyte. Based on this, the study of a lithium battery tape with high electrolyte durability and good high temperature resistance has become an urgent problem to be solved in this field. Summary of the invention

[0005] The present invention solves the problems of low electrolyte durability and poor high temperature resistance of existing lithium battery tapes by providing an electrolyte durable engraved coding tape which is simple to prepare, has high electrolyte durability, good adhesion, and can withstand long-term electrolyte immersion at high temperature, and a preparation method thereof, thereby effectively improving the service life of the lithium battery tape.

[0006] A first aspect of the present invention provides an electrolyte durable coding tape, comprising a base layer, a pressure-sensitive adhesive layer and a release layer, wherein the release layer and the adhesive layer are located on both sides of the base layer.

[0007] As a preferred solution, the base layer is one of PET film, PP film and PC film.

[0008] As a preferred solution, the base layer is a PET film.

[0009] As a preferred solution, the PET film has a thickness of 20 to 30 μm.

[0010] As a preferred solution, the raw materials of the pressure-sensitive adhesive layer include, by weight, 45-65 parts of isooctyl acrylate (CAS No.: 103-11-7), 15-20 parts of butyl acrylate (CAS No.: 141-32-2), 1-5 parts of acrylic acid (CAS No.: 79-10-7), 1-3 parts of hydroxybutyl acrylate, 10-15 parts of lauryl acrylate (CAS No.: 2156-97-0), and 10-15 parts of isobornyl acrylate (CAS No.: 2156-97-0). AS No.: 5888-33-5) 5-15 parts, azobisisobutyronitrile (CAS No.: 78-67-1) 0.5-1 parts, ethyl acetate (CAS No.: 141-78-6) 100-200 parts, lauryl methacrylate (CAS No.: 142-90-5) 5-10 parts, glycidyl methacrylate (CAS No.: 106-91-2) 1-10 parts, curing agent 3-10 parts, color paste 3-15 parts.

[0011] As a preferred solution, the pressure-sensitive adhesive layer includes, by mass, 50-60 parts of isooctyl acrylate, 16-18 parts of butyl acrylate, 1-4 parts of acrylic acid, 1-3 parts of hydroxybutyl acrylate, 10-12 parts of lauryl acrylate, 5-10 parts of isobornyl acrylate, 0.5-1 part of azobisisobutyronitrile, 100-200 parts of ethyl acetate, 5-8 parts of lauryl methacrylate, 1-6 parts of glycidyl methacrylate, 3-10 parts of curing agent, and 3-10 parts of color paste.

[0012] As a preferred solution, the hydroxybutyl acrylate can be purchased from Jinan Yuanxiang Chemical Co., Ltd. with product number 322.

[0013] The present invention finds that the mass ratio of lauryl methacrylate to glycidyl methacrylate in the range of (1-2):(2-1) can effectively increase the system molecular weight of the pressure-sensitive adhesive and increase the molecular chain length, and the presence of glycidyl methacrylate can coordinate the above system changes to enhance the crosslinking degree of the pressure-sensitive adhesive system, so that the adhesive tape has better stickiness. It is also found that when the mass ratio of isobornyl acrylate to curing agent is in the range of (1-3):1, the larger steric hindrance introduced by isobornyl acrylate can solve the problem that the viscosity of the adhesive tape increases and the thickness is difficult to control when too much curing agent is added, and at the same time, the polar groups on the surface of the copolymer are more evenly dispersed, the exposure of carbon atoms and carbon chains is prevented, and the thermal stability of the pressure-sensitive adhesive is improved. The adhesive tape has significant durability and thermal stability in the electrolyte. When immersed in the electrolyte at 85°C for 7 days, the adhesive tape is tightly attached to the aluminum foil, the surface of the adhesive tape does not warp, and there is no bulging between the adhesive tape and the aluminum foil.

[0014] As a preferred solution, the thickness of the pressure-sensitive adhesive layer is 5-15 μm.

[0015] As a preferred solution, the curing agent in the pressure-sensitive adhesive layer is at least one of an isocyanate curing agent, an epoxy curing agent and an amino curing agent.

[0016] As a preferred solution, the curing agent in the pressure-sensitive adhesive layer is an isocyanate curing agent and an epoxy curing agent, and the mass ratio of the isocyanate curing agent to the epoxy curing agent is 3:1-1:3.

[0017] In the present invention, the curing agent in the pressure-sensitive adhesive is selected from an isocyanate curing agent and an epoxy curing agent, the mass ratio of the isocyanate curing agent to the epoxy curing agent is 3:1-1:3, and the hydroxyl group of the isocyanate curing agent is used in combination with the water-based epoxy curing agent to improve the dispersibility of the curing agent and improve the defect of the water-based epoxy agent that the viscosity becomes low after processing, so that the pressure-sensitive adhesive layer reaches a better curing degree. At the same time, the combined use can also effectively improve the reaction activity of the groups in the colloid, thereby improving the cohesive strength, and further enabling the colloid to obtain extremely strong electrolyte resistance. The adhesive tape is immersed in an electrolyte at 85° C. for 7 days, and the electrolyte has no obvious color change.

[0018] The isocyanate curing agent is used in combination with the water-based epoxy curing agent to effectively improve the yellowing resistance, weather resistance and mechanical properties of the colloid.

[0019] As a preferred solution, the isocyanate content in the isocyanate curing agent is 15-25%, and the viscosity at 23° C. is 2500-4500 mPa·s.

[0020] As a preferred solution, the water-based epoxy curing agent has an amine value of 250-350 and a viscosity of 150-350 mPa·s.

[0021] As a preferred solution, the color paste in the pressure-sensitive adhesive layer is one of phthalocyanine blue, cobalt green and brilliant blue.

[0022] As a preferred solution, the release layer is a silicon-containing or non-silicon release layer.

[0023] As a preferred solution, the release layer is a non-silicon release layer.

[0024] As a preferred solution, the non-silicone release layer includes but is not limited to one or a mixture of two of imported PEELOIL1010, K100H, K100D, K100ES, and RL-600.

[0025] A second aspect of the present invention provides a method for preparing an electrolyte durable coding tape, comprising the following steps:

[0026] (1) Isooctyl acrylate, butyl acrylate, acrylic acid, hydroxybutyl acrylate, lauryl acrylate, isobornyl acrylate, lauryl methacrylate, glycidyl methacrylate and color paste are mixed uniformly according to mass parts and added into a reaction kettle, and then ethyl acetate is added, nitrogen is introduced to remove oxygen, and when the temperature is stirred and raised to 50-100° C., azobisisobutyronitrile is added, and the temperature of the reaction kettle is maintained at 50-100° C. for 10-20 hours. After cooling, an acrylate polymer is obtained.

[0027] (2) adding a certain amount of ethyl acetate to the acrylate polymer obtained in step 1 and stirring evenly, then adding a uniform mixture of an isocyanate curing agent and an epoxy curing agent, and continuing to stir evenly to obtain a pressure-sensitive adhesive solution.

[0028] (3) The non-silicon release agent is directly coated on one surface of the PET film, and then placed at 60-120° C. for heat preservation and curing for 5-20 minutes to obtain a PET film with a non-silicon release layer.

[0029] (4) directly coating the pressure-sensitive adhesive solution obtained in step 2 on the side of the PET film with a non-silicone release layer without the non-silicone release layer, placing it at 60-120° C. for heat preservation and curing for 5-12 min to form a pressure-sensitive adhesive layer, and winding it to obtain a semi-finished adhesive tape.

[0030] (5) Laser engrave an information identification code on the semi-finished tape to obtain an electrolyte-durable engraved tape.

[0031] Beneficial effects:

[0032] The electrolyte durable coding tape provided by the present invention has the following advantages:

[0033] (1) In the present invention, the mass ratio of lauryl methacrylate to glycidyl methacrylate is (1-2): (2-1), which can effectively increase the system molecular weight of the pressure-sensitive adhesive and increase the molecular chain length. The presence of glycidyl methacrylate can coordinate the above-mentioned system changes to enhance the cross-linking degree of the pressure-sensitive adhesive system, so that the electrolyte durable coding tape has excellent adhesion performance and can adhere to the surface of the aluminum foil material for a long time without warping.

[0034] (2) When the mass ratio of isobornyl acrylate to curing agent in the present invention is (1-3):1, the larger steric hindrance introduced by isobornyl acrylate can solve the problem that the viscosity of the tape increases and the thickness is difficult to control when too much curing agent is added. At the same time, the polar groups on the surface of the copolymer are dispersed more evenly, preventing the exposure of carbon atoms and carbon chains. At the same time, the heat resistance of the electrolyte durable coding tape is stable, and the chemical properties can be kept stable at 85°C without decomposing impurities to pollute the electrolyte.

[0035] (3) In the present invention, the mass ratio of isocyanate curing agent to epoxy curing agent is 3:1-1:3. The hydroxyl group of the isocyanate curing agent is used in combination with the water-based epoxy curing agent to improve the dispersion of the curing agent and improve the defect of the water-based epoxy agent that the viscosity becomes low after processing, so that the pressure-sensitive adhesive layer can achieve a better degree of curing. At the same time, the combined use can also effectively improve the reaction activity of the groups in the colloid, thereby improving the cohesive strength, so that the electrolyte-durable coding tape has significant electrolyte resistance. After being stored in the electrolyte for 7 days, the adhesion between the adhesive layer and the aluminum foil is complete and has no bulging. DETAILED DESCRIPTION

[0036] Example 1

[0037] A durable electrolyte coding tape comprises a substrate layer, a pressure-sensitive adhesive layer and a release layer, wherein the release layer and the pressure-sensitive adhesive layer are located on both sides of the substrate layer. The pressure-sensitive adhesive layer comprises, by mass, 50 parts of isooctyl acrylate, 15 parts of butyl acrylate, 3 parts of acrylic acid, 2 parts of hydroxybutyl acrylate, 10 parts of lauryl acrylate, 5 parts of isobornyl acrylate, 1 part of azobisisobutyronitrile, 120 parts of ethyl acetate, 5 parts of lauryl methacrylate, 5 parts of glycidyl methacrylate, 3 parts of curing agent, and 5 parts of color paste. The curing agent is isocyanate and epoxy, and the mass ratio of isocyanate to epoxy is 1:1. The color paste is phthalocyanine blue, and the substrate layer is a PET layer. The release layer is a non-silicon release layer. The non-silicon release layer is coated with a non-silicon release agent.

[0038] The non-silicone release agent was purchased from Guangzhou Rongyu Trading Co., Ltd., and the product model is PEELOIL1010.

[0039] The hydroxybutyl acrylate was purchased from Jinan Yuanxiang Chemical Co., Ltd. with product number 322.

[0040] The isocyanate curing agent can be purchased from Chongqing Jingyi New Materials Co., Ltd., and the product model is BayhydurXP2655.

[0041] The epoxy curing agent was purchased from Jinan Jibin Chemical Co., Ltd., and the product model is epoxy curing agent.

[0042] The color paste was purchased from Shanghai Jiahong Material Technology Co., Ltd., product model 6153.

[0043] A method for preparing an electrolyte durable coding tape comprises the following steps:

[0044] (1) Mix isooctyl acrylate, butyl acrylate, acrylic acid, hydroxybutyl acrylate, lauryl acrylate, isobornyl acrylate, lauryl methacrylate, glycidyl methacrylate and color paste in parts by mass and add them to a reactor. Then add ethyl acetate, introduce nitrogen to remove oxygen, stir and heat to 60±5°C, add azobisisobutyronitrile, and keep the reactor temperature at 60±5°C for 20 hours. After cooling, take out and set aside.

[0045] (2) adding ethyl acetate to the acrylate polymer obtained in step 1 and stirring evenly, then adding a uniform mixture of an isocyanate curing agent and an epoxy curing agent, and continuing to stir evenly to obtain a pressure-sensitive adhesive solution.

[0046] (3) The non-silicone release agent is directly coated on one surface of the PET film, and then placed at 100±5° C. for curing for 10 minutes to obtain a PET film with a non-silicone release layer.

[0047] (4) The pressure-sensitive adhesive solution obtained in step 2 is directly coated on the side of the PET film with the non-silicone release layer without the non-silicone release layer, and is placed at 100±5° C. for 10 min for curing and drying to form a pressure-sensitive adhesive layer, and then rolled up to obtain a semi-finished adhesive tape.

[0048] (5) Laser engrave an information identification code on the semi-finished tape to obtain an electrolyte-durable engraved tape.

[0049] Example 2

[0050] A durable electrolyte coding tape comprises a substrate layer, a pressure-sensitive adhesive layer and a release layer. The pressure-sensitive adhesive layer comprises, by mass, 60 parts of isooctyl acrylate, 18 parts of butyl acrylate, 4 parts of acrylic acid, 3 parts of hydroxybutyl acrylate, 12 parts of lauryl acrylate, 10 parts of isobornyl acrylate, 1 part of azobisisobutyronitrile, 150 parts of ethyl acetate, 5 parts of lauryl methacrylate, 6 parts of glycidyl methacrylate, 3 parts of curing agent, and 5 parts of color paste. The curing agent is isocyanate and epoxy, and the mass ratio of isocyanate to epoxy is 1:1. The color paste is phthalocyanine blue, and the substrate layer is a PET layer. The release layer is a non-silicon release layer. The non-silicon release layer is coated with a non-silicon release agent.

[0051] The non-silicone release agent was purchased from Guangzhou Rongyu Trading Co., Ltd., and the product model is PEELOIL1010.

[0052] The hydroxybutyl acrylate was purchased from Jinan Yuanxiang Chemical Co., Ltd. with product number 322.

[0053] The isocyanate curing agent can be purchased from Chongqing Jingyi New Materials Co., Ltd., and the product model is BayhydurXP2655.

[0054] The epoxy curing agent was purchased from Jinan Jibin Chemical Co., Ltd., and the product model is epoxy curing agent.

[0055] The color paste was purchased from Shanghai Jiahong Material Technology Co., Ltd., product model 6153.

[0056] A method for preparing an electrolyte durable coding tape comprises the following steps:

[0057] (1) Isooctyl acrylate, butyl acrylate, acrylic acid, hydroxybutyl acrylate, lauryl acrylate, isobornyl acrylate, lauryl methacrylate, glycidyl methacrylate and color paste are mixed uniformly according to mass parts and added into a reaction kettle, and then ethyl acetate is added, nitrogen is introduced to remove oxygen, and when the temperature is stirred and raised to 60±5°C, azobisisobutyronitrile is added, and the temperature of the reaction kettle is maintained at 60±5°C for 18 hours. After cooling, an acrylate polymer is obtained.

[0058] (2) adding ethyl acetate to the acrylate polymer obtained in step 1 and stirring evenly, then adding a uniform mixture of an isocyanate curing agent and an epoxy curing agent, and continuing to stir evenly to obtain a pressure-sensitive adhesive solution.

[0059] (3) The non-silicone release agent is directly coated on one surface of the PET film, and then placed at 100±5° C. for curing for 10 minutes to obtain a PET film with a non-silicone release layer.

[0060] (4) The pressure-sensitive adhesive solution obtained in step 2 is directly coated on the side of the PET film with non-silicone release agent without non-silicone release agent, and is placed at 100±5° C. for 10 min for curing and drying to form a pressure-sensitive adhesive layer, and is rolled up to obtain a semi-finished adhesive tape.

[0061] (5) Laser engrave an information identification code on the semi-finished tape to obtain an electrolyte-durable engraved tape.

[0062] Example 3

[0063] A durable electrolyte coding tape comprises a base layer, a pressure-sensitive adhesive layer and a release layer. The pressure-sensitive adhesive layer comprises, by mass, 65 parts of isooctyl acrylate, 20 parts of butyl acrylate, 4 parts of acrylic acid, 3 parts of hydroxybutyl acrylate, 12 parts of lauryl acrylate, 15 parts of isobornyl acrylate, 1 part of azobisisobutyronitrile, 180 parts of ethyl acetate, 6 parts of lauryl methacrylate, 5 parts of glycidyl methacrylate, 3 parts of curing agent and 5 parts of color paste. The curing agent is isocyanate and epoxy, the mass ratio of isocyanate to epoxy is 1:1, the color paste is phthalocyanine blue, and the base layer is a PET layer. The release layer is a non-silicon release layer. The non-silicon release layer is coated with a non-silicon release agent.

[0064] The non-silicone release agent was purchased from Guangzhou Rongyu Trading Co., Ltd., and the product model is PEELOIL1010.

[0065] The hydroxybutyl acrylate was purchased from Jinan Yuanxiang Chemical Co., Ltd. with product number 322.

[0066] The isocyanate curing agent can be purchased from Chongqing Jingyi New Materials Co., Ltd., and the product model is BayhydurXP2655.

[0067] The epoxy curing agent was purchased from Jinan Jibin Chemical Co., Ltd., and the product model is epoxy curing agent.

[0068] The color paste was purchased from Shanghai Jiahong Material Technology Co., Ltd., product model 6153.

[0069] A method for preparing an electrolyte durable coding tape comprises the following steps:

[0070] (1) Isooctyl acrylate, butyl acrylate, acrylic acid, hydroxybutyl acrylate, lauryl acrylate, isobornyl acrylate, lauryl methacrylate, glycidyl methacrylate and color paste were stirred evenly according to mass parts and added into a reaction kettle, and then ethyl acetate was added, nitrogen was introduced to remove oxygen, and when the temperature was stirred and raised to 60±5°C, azobisisobutyronitrile was added, and the temperature of the reaction kettle was maintained at 60±5°C for 16 hours. After cooling, an acrylate polymer was obtained.

[0071] (2) adding ethyl acetate to the acrylate polymer obtained in step 1 and stirring evenly, then adding a uniform mixture of an isocyanate curing agent and an epoxy curing agent, and continuing to stir evenly to obtain a pressure-sensitive adhesive solution.

[0072] (3) The non-silicone release agent is directly coated on one surface of the PET film, and then placed at 100±5° C. for curing for 10 minutes to obtain a PET film with a non-silicone release layer.

[0073] (4) directly coating the pressure-sensitive adhesive solution obtained in step 2 on the side of the PET film with non-silicone release layer without the non-silicone release layer, curing at 100±5° C. for 10 min and drying to form a pressure-sensitive adhesive layer, and then winding up to obtain a semi-finished adhesive tape.

[0074] (5) Laser engrave an information identification code on the semi-finished tape to obtain an electrolyte-durable engraved tape.

[0075] Comparative Example 1

[0076] The curing agent is an isocyanate curing agent and an epoxy curing agent, the mass ratio of the isocyanate curing agent to the epoxy curing agent is 1:5, and the rest is the same as in Example 1.

[0077] Comparative Example 2

[0078] The curing agent is an isocyanate curing agent and an epoxy curing agent, the mass ratio of the isocyanate curing agent to the epoxy curing agent is 5:1, and the rest is the same as in Example 1.

[0079] Comparative Example 3

[0080] The curing agent is an amino curing agent and an epoxy curing agent, the mass ratio of the amino curing agent to the epoxy curing agent is 1:1, and the rest is the same as in Example 1.

[0081] Comparative Example 4

[0082] The curing agent is an isocyanate curing agent and an amino curing agent, the mass ratio of the isocyanate curing agent to the amino curing agent is 1:1, and the rest is the same as in Example 1.

[0083] Comparative Example 5

[0084] 3 parts of lauryl methacrylate, 3 parts of glycidyl methacrylate, and the rest are the same as in Example 1.

[0085] Comparative Example 6

[0086] 5 parts of lauryl methacrylate, 2 parts of glycidyl methacrylate, and the rest are the same as in Example 1.

[0087] Comparative Example 7

[0088] 15 parts of isobornyl acrylate and 3 parts of a curing agent, wherein the curing agent is an isocyanate curing agent and an epoxy curing agent, and the mass ratio of the isocyanate curing agent to the epoxy curing agent is 1:1.

[0089] Performance Testing

[0090] Cut the tape sample into 3 test samples of 40mm*40mm, paste the test samples on the surface of 75um aluminum foil material, roll back and forth 5 times with a 2.0 kg rubber roller, and then put it into a container with electrolyte, and then place the container in an oven at 85℃ for 7 days. Take it out of the oven and cool it to 25℃, observe whether the electrolyte changes color; whether the tape falls off the film material; whether there is bulging between the adhesive layer and the aluminum foil material or the electrolyte penetrates. Grade A: no warping; Grade B: warping area 5-10%; Grade C: warping area 10-20%, Grade D: warping area >20%.

[0091] The electrolyte was purchased from Aladdin Reagent Network, product number: W305304-500ml.

[0092]

[0093]

[0094] It can be seen from the above that the adhesive tape prepared by the present invention has excellent electrolyte durability and is more suitable for insulation and fixed protection of electrode windings, cell terminations, and pole pieces during the production and assembly process of lithium batteries.

Claims

1. An electrolyte durable coding tape, characterized in that: It comprises a base layer, a pressure-sensitive adhesive layer and a release layer, wherein the release layer and the pressure-sensitive adhesive layer are located on both sides of the base layer; the pressure-sensitive adhesive layer comprises, by weight, 50 parts of isooctyl acrylate, 15 parts of butyl acrylate, 3 parts of acrylic acid, 2 parts of hydroxybutyl acrylate, 10 parts of lauryl acrylate, 5 parts of isobornyl acrylate, 1 part of azobisisobutyronitrile, 120 parts of ethyl acetate, 5 parts of lauryl methacrylate, 5 parts of glycidyl methacrylate, 3 parts of curing agent, and 5 parts of color paste; the curing agent is isocyanate and epoxy, the mass ratio of isocyanate to epoxy is 1:1, the color paste is phthalocyanine blue, and the base layer is a PET layer; the release layer is a non-silicon release layer; the non-silicon release layer is obtained by coating the non-silicon release agent; The product model of the non-silicone release agent is PEELOIL1010; The isocyanate curing agent product model is Bayhydur XP2655; The epoxy curing agent was purchased from Jinan Jibin Chemical Co., Ltd., and the product model is epoxy curing agent; The color paste was purchased from Shanghai Jiahong Material Technology Co., Ltd., product model 6153.

2. A method for preparing the electrolyte durable coding tape according to claim 1, characterized in that: The following steps are involved: (1) isooctyl acrylate, butyl acrylate, acrylic acid, hydroxybutyl acrylate, lauryl acrylate, isobornyl acrylate, lauryl methacrylate, glycidyl methacrylate and color paste are mixed uniformly according to mass parts and added into a reaction kettle, ethyl acetate is added, nitrogen is introduced to remove oxygen, and when the temperature is raised to 50-100° C. while stirring, azobisisobutyronitrile is added, the temperature of the reaction kettle is maintained at 50-100° C. for 10-20 hours, and the acrylate polymer is obtained after cooling; (2) adding ethyl acetate to the acrylate polymer obtained in step 1 and stirring evenly, then adding a uniform mixture of isocyanate and epoxy curing agents, and continuing to stir evenly to obtain a pressure-sensitive adhesive solution; (3) directly coating a non-silicon release agent on one surface of the PET film, and then curing it at 60-120° C. for 5-20 minutes to obtain a PET film with a non-silicon release layer; (4) directly coating the pressure-sensitive adhesive solution obtained in step 2 on the PET film surface of the PET film with the non-silicon release layer, placing it at 60-120° C. for 5-20 min for heat preservation and drying to form a pressure-sensitive adhesive layer, and winding it to obtain a semi-finished adhesive tape; (5) Laser engrave an information identification code on the semi-finished tape to obtain an electrolyte-durable engraved tape.

Citation Information

Patent Citations

  • Acrylic ester pressure-sensitive adhesive tape and preparation method thereof and lithium ion battery

    CN103911088A

  • Novel pressure sensitive tape

    CN204676029U

  • Insulating flame-retardant pressure-sensitive adhesive applied to power battery, adhesive tape and preparation method of insulating flame-retardant pressure-sensitive adhesive

    CN112126384A

  • High-temperature-resistant and high-stripping solvent type acrylate pressure-sensitive adhesive and preparation method thereof

    CN113604175A

  • Electrolyte-solvent-resistant acrylate pressure-sensitive adhesive and preparation method thereof

    CN113736398A