Negative electrode sheet, secondary battery and electrical device

By designing the negative electrode capacity and coating structure in different areas on the negative electrode sheet of the lithium-ion battery, the polarization potential is optimized, the problem of lithium precipitation at the edge of the lithium-ion battery is solved, and the cycle performance is improved.

CN115832214BActive Publication Date: 2024-10-11CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211486496.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-24
Publication Date
2024-10-11
Estimated Expiration
2042-11-24

AI Technical Summary

Technical Problem

During the charging and discharging process of lithium-ion batteries, due to the difference in polarization potential between the edge area and the middle area of ​​the negative electrode piece, lithium ions are preferentially precipitated in the edge area, deteriorating the cycle performance.

Method used

Design a negative electrode plate, which is divided into a first area, a middle area and a second area in the width direction. The negative electrode capacity of the middle area is smaller than the first area and the second area. By adjusting the coating weight and active material ratio, the optimization The polarization potential during the lithium ion charging process improves the uniformity of lithium insertion.

Benefits of technology

It effectively reduces the problem of lithium precipitation at the edge of the negative electrode piece, improves the cycle performance of lithium-ion batteries, and the method is simple, easy to operate, and avoids material waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115832214B_ABST
    Figure CN115832214B_ABST
Patent Text Reader

Abstract

The present application discloses a negative electrode plate, a secondary battery and an electric device, and relates to the field of batteries. The negative electrode plate includes a first region, a middle region and a second region arranged in sequence along its width direction, and the negative electrode capacity of the middle region is respectively smaller than the negative electrode capacity of the first region and the negative electrode capacity of the second region. The negative electrode capacity of the middle region is respectively smaller than the negative electrode capacity of the first region and the negative electrode capacity of the second region, thereby reducing the polarization potential of the first region and the second region, thereby optimizing the polarization potential of each part of the negative electrode plate in the width direction during lithium ion charging, improving the uniformity of lithium insertion, thereby improving the problem of lithium deposition at the edge of the plate, and improving the cycle performance of lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular to a negative electrode plate, a secondary battery and an electrical device. Background Art

[0002] During the charge and discharge process of secondary batteries such as lithium ions, due to the interface effect at the edge in the width direction of the negative electrode sheet, there is a difference in polarization potential between the edge area and the middle area. Since the polarization potential of the edge area is large, during the charging process, the polarization potential of the negative electrode edge is larger than that of the middle area, and lithium ions are preferentially precipitated in the edge area with large polarization. This leads to the problem of lithium precipitation at the edge of lithium ion batteries during the cycle process, which deteriorates the cycle performance. Summary of the invention

[0003] The main purpose of this application is to propose a negative electrode plate, a secondary battery and an electrical device, aiming to improve the lithium plating problem of the negative electrode plate and enhance the cycle performance.

[0004] In a first aspect, the present application provides a negative electrode plate, which includes a first region, a middle region, and a second region arranged in sequence along its width direction, and the negative electrode capacity of the middle region is smaller than the negative electrode capacity of the first region and the negative electrode capacity of the second region.

[0005] In the technical solution of the embodiment of the present application, the negative electrode capacity of the middle area is respectively smaller than the negative electrode capacity of the first area and the negative electrode capacity of the second area, thereby reducing the polarization potential of the first area and the second area, thereby optimizing the polarization potential of each part in the width direction of the negative electrode plate during lithium ion charging, improving the uniformity of lithium insertion, and further improving the problem of lithium plating at the edge of the plate, thereby improving the cycle performance of the lithium ion battery.

[0006] In some embodiments, the negative electrode capacity of the first region is C1, the negative electrode capacity of the second region is C2, and the negative electrode capacity of the middle region is C3: 1.01≤C1 / C3≤1.1; 1.01≤C2 / C3≤1.1. If C1 / C3 or C2 / C3 is too small, the purpose of improving edge lithium deposition cannot be achieved; if C1 / C3 or C2 / C3 is too large, it will cause over-design and waste of materials.

[0007] In some embodiments, the negative electrode capacity of the first region is C1, the negative electrode capacity of the second region is C2, and the negative electrode capacity of the middle region is C3: 1.02≤C1 / C3≤1.05; 1.02≤C2 / C3≤1.05. Experiments show that within the above ratio range, the lithium plating problem of the negative electrode plate is improved more significantly.

[0008] In some embodiments, in the width direction of the negative electrode sheet, the size of the first region is H1, the size of the second region is H2, and the size of the middle region is H3: 0.01≤H1 / H3≤0.2; and / or, 0.01≤H2 / H3≤0.2. If the ratio of H1 / H3 or H2 / H3 is too small, the purpose of improving edge lithium deposition cannot be achieved; if the ratio of H1 / H3 or H2 / H3 is too large, it will cause over-design and waste of materials.

[0009] In some embodiments, the negative electrode plate includes a current collector and a negative electrode coating coated on the current collector, the weight of the negative electrode coating in the middle region is x, the weight of the negative electrode coating in the first region is y, and the weight of the negative electrode coating in the second region is z, x<y, and x<z. By adjusting the weight of the negative electrode coating in the middle region to be the smallest, the negative electrode capacity in the middle region is respectively smaller than the negative electrode capacity in the first region and the negative electrode capacity in the second region, which is highly feasible.

[0010] In some embodiments, the negative electrode plate includes a current collector and a negative electrode coating coated on the current collector, the mass proportion of the active material in the negative electrode coating in the middle region is a, the mass proportion of the active material in the negative electrode coating in the first region is b, and the mass proportion of the active material in the negative electrode coating in the second region is c, a<b, and a<c, so that the negative electrode capacity of the middle region is smaller than the negative electrode capacity of the first region and the negative electrode capacity of the second region, respectively. The method is simple and easy to control.

[0011] In some embodiments, the specific capacity of the active material in the middle region is m, the specific capacity of the active material in the first region is n, and the specific capacity of the active material in the second region is p, m<n, and m<p. Specifically, active materials with different specific capacities can be selected in different regions to achieve a negative electrode capacity in the middle region that is smaller than the negative electrode capacity in the first region and the negative electrode capacity in the second region, respectively. The method is simple and easy to operate.

[0012] In a second aspect, the present application provides a method for preparing the negative electrode sheet in the above embodiment, comprising the following steps:

[0013] Provide a current collector, wherein the current collector is divided into a first region, a middle region, and a second region arranged in sequence in a width direction thereof;

[0014] A first coating layer is prepared in the first region, an intermediate coating layer is prepared in the middle region, and a second coating layer is coated in the second region to obtain a negative electrode sheet, wherein the negative electrode capacity of the intermediate coating layer is smaller than the negative electrode capacity of the first coating layer and the negative electrode capacity of the second coating layer, respectively.

[0015] By preparing coating layers with different negative electrode capacities in the middle and other parts in the width direction of the current collector, the negative electrode capacity of the middle area is smaller than the negative electrode capacity of the first area and the negative electrode capacity of the second area. The method is simple and easy to operate.

[0016] In a third aspect, the present application provides a secondary battery, comprising the negative electrode plate in the above embodiment.

[0017] In a fourth aspect, the present application provides an electrical device, comprising the secondary battery in the above-mentioned embodiment. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying any creative work.

[0019] Figure 1 Schematic diagram of the structure of the negative electrode plate of an embodiment of the present application.

[0020] Description of Figure Numbers:

[0021] 1 Middle area 3 Second area 2 First Area

[0022] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0024] It should be noted that, in the embodiments, those without specifying specific conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. Those without specifying the manufacturer for reagents or instruments used are conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, and "A and / or B" is taken as an example, including schemes A, B, or A and B that meet the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve, and when the combination of the technical schemes is contradictory or cannot be achieved, it should be considered that the combination of such technical schemes does not exist, and is not within the scope of protection required in this application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work, all belong to the scope of protection of this application.

[0025] As we all know, during the charge and discharge process of secondary batteries such as lithium ions, due to the interface effect at the edge in the width direction of the negative electrode sheet, there is a difference in polarization potential between the edge area and the middle area. Since the polarization potential of the edge area is large, during the charging process, the polarization potential of the negative electrode edge is larger than that of the middle area, and lithium ions are preferentially precipitated in the edge area with large polarization. This leads to the problem of lithium precipitation at the edge of lithium ion batteries during the cycle process, which deteriorates the cycle performance.

[0026] Therefore, inhibiting lithium plating is the research direction of many scholars. Researchers in related fields mainly study components such as lithium-ion battery electrolytes and battery electrodes. The research in the above directions is relatively blind, costly, and the results are not ideal.

[0027] For example, an existing technical solution provides an electrochemical device, which includes an electrode assembly, wherein the electrode assembly includes a negative electrode plate and a positive electrode plate, wherein the negative electrode plate includes a negative electrode collector and an active material layer located on the surface of the negative electrode collector, wherein the positive electrode plate includes a positive electrode collector and a positive electrode active layer located on the surface of the positive electrode collector, wherein the width of the negative electrode active layer is Ha, and along the width direction of the negative electrode active layer, the negative electrode active layer includes a first edge and a second edge opposite to each other, wherein the negative electrode active layer includes a first region and a second region, wherein the first region is a region from the first edge to Ha / 4 of the first edge, and the second region is a region from Ha / 4 of the first edge to 3H of the first edge. a / 4 region; the electrochemical device is disassembled under a 50% SOC state of charge, the charge transfer impedance per unit area of ​​the first region is Rct1, and the charge transfer impedance per unit area of ​​the second region is Rct2, satisfying 85%≤Rct1 / Rct2≤140%. By regulating the ratio of the charge transfer impedance between the first region and the second region within the above range, on the one hand, it is possible to avoid the charge transfer impedance of the first region being relatively too small, lithium ions being enriched on the surface of its negative electrode active layer and inducing a large number of side reactions, resulting in rapid deterioration of subsequent impedance; on the other hand, it is possible to avoid the charge transfer impedance of the first region being relatively too large, lithium ions being blocked from embedding on the surface of its negative electrode active layer, thereby causing lithium precipitation. By regulating the ratio of the charge transfer impedance between the first region and the second region within the above range, it is beneficial to improve the lithium precipitation phenomenon of the electrochemical device, thereby improving the electrochemical cycle performance. However, the improvement of lithium precipitation by regulating the charge transfer impedance Rct of the first region and the second region in the width direction of the negative electrode sheet has low accuracy and low operability.

[0028] Based on this, the applicant considered that in the design of positive and negative electrodes of lithium-ion batteries, the ratio of the negative electrode capacity to the positive electrode capacity is called Negative / Positive, referred to as N / P. In general, in the design of lithium-ion batteries, the negative electrode capacity is greater than the positive electrode capacity to ensure that the lithium released from the positive electrode can be fully embedded in the negative electrode without lithium deposition. Can the design be optimized by considering the negative electrode capacity at different positions of the negative electrode sheet to suppress edge lithium deposition?

[0029] The applicant noted that by regulating the negative electrode capacity in the edge area of ​​the negative electrode plate, the occurrence of lithium deposition at the edge of the negative electrode plate can be significantly suppressed.

[0030] Based on the above analysis, the applicant discovered after a large number of repeated experiments that by increasing the negative electrode capacity at the edge in the width direction of the negative electrode plate, the N / P of different areas of the lithium-ion battery can be regulated, the consistency of the negative electrode plate can be improved, and the uniformity of lithium embedding into the plate can be improved, thereby slowing down and eliminating the phenomenon of lithium deposition at the edge of the negative electrode plate.

[0031] Specifically, this application proposes a negative electrode plate, see Figure 1 The negative electrode sheet includes a first region 2, a middle region 1, and a second region 3 arranged in sequence along its width direction, and the negative electrode capacity of the middle region 1 is respectively smaller than the negative electrode capacity of the first region 2 and the negative electrode capacity of the second region 3. Compared with the prior art, the beneficial effects of the present application are:

[0032] In the technical solution of the embodiment of the present application, the negative electrode capacity of the middle area is respectively smaller than the negative electrode capacity of the first area and the negative electrode capacity of the second area, thereby reducing the polarization potential of the first area and the second area, and regulating the N / P of different areas of the lithium-ion battery, so as to optimize the polarization potential of each part in the width direction of the negative electrode plate during lithium-ion charging, improve the uniformity of lithium insertion, and further improve the problem of lithium plating at the edge of the plate, thereby improving the cycle performance of the lithium-ion battery.

[0033] It can be understood that the negative electrode capacity described in the present application is determined by the number of electrons in the negative electrode of the battery, and is a mass specific capacity, that is, the amount of electricity that can be released by a unit mass of a substance, and the unit is mAh or Ah.

[0034] In some embodiments, the negative electrode capacity of the first region is C1, the negative electrode capacity of the second region is C2, and the negative electrode capacity of the middle region is C3: 1.01≤C1 / C3≤1.1, for example, C1 / C3 can be 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, etc.; 1.01≤C2 / C3≤1.1, for example, C2 / C3 can be 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1, etc. If C1 / C3 or C2 / C3 is too small, the purpose of improving edge lithium deposition cannot be achieved; if C1 / C3 or C2 / C3 is too large, it will cause over-design and waste of materials.

[0035] It can be understood that the limitations on the C1 / C3 and C2 / C3 ranges in the present application can be met at the same time, or only one of them can be met. In the embodiments of the present application, the above two are met at the same time, so that the effect of improving edge lithium deposition is better.

[0036] In addition, C1 / C3 and C2 / C3 may be equal or unequal. In the embodiment of the present application, C1 / C3 and C2 / C3 are equal. Thus, when preparing the negative electrode sheet, the parameters of the first region and the second region can be made the same, thereby simplifying the preparation process.

[0037] In some embodiments, the negative electrode capacity of the first region is C1, the negative electrode capacity of the second region is C2, and the negative electrode capacity of the middle region is C3: 1.02≤C1 / C3≤1.05, for example, C1 / C3 can be 1.01, 1.02, 1.03, 1.04, 1.05, etc.; 1.02≤C2 / C3≤1.05, for example, C2 / C3 can be 1.01, 1.02, 1.03, 1.04, 1.05, etc. Experiments show that within the above ratio range, the lithium plating problem of the negative electrode sheet is improved more significantly.

[0038] In some embodiments, in the width direction of the negative electrode plate, the size of the first area is H1, the size of the second area is H2, and the size of the middle area is H3: 0.01≤H1 / H3≤0.2, for example, H1 / H3 can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.12, 0.14, 0.15, 0.17, 0.19, 0.2 and the like; 0.01≤H2 / H3≤0.2, for example, H2 / H3 can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.12, 0.14, 0.15, 0.17, 0.19, 0.2 and the like. If the ratio of H1 / H3 or H2 / H3 is too small, the purpose of improving edge lithium deposition cannot be achieved; if the ratio of H1 / H3 or H2 / H3 is too large, it will cause over-design and waste of materials.

[0039] It can be understood that the restrictions on the ranges of H1 / H3 and H2 / H3 in the present application can be met at the same time, or only one of them can be met. In the embodiments of the present application, the above two are met at the same time, so that the effect of improving edge lithium deposition is better.

[0040] In addition, H1 / H3 and H2 / H3 may be equal or unequal. In the embodiment of the present application, H1 / H3 and H2 / H3 are equal. In this way, when preparing the negative electrode sheet, the parameters of the first region and the second region can be made the same, which simplifies the preparation process and forms a symmetrical setting, thereby improving the consistency of the negative electrode sheet.

[0041] The present application does not limit the method of controlling the negative electrode capacity in different regions. In some embodiments, the purpose of adjusting the C1 / C3 or C2 / C3 ratio is achieved by adjusting the coating weight of the negative electrode coating in the first region, the second region and the middle region in the width direction of the negative electrode sheet or the specific gravity of the negative electrode active material in the negative electrode coating or the type of negative electrode active material in the negative electrode coating, or by adjusting two or three of the above three at the same time.

[0042] In some embodiments, the negative electrode plate includes a current collector and a negative electrode coating coated on the current collector, the weight of the negative electrode coating in the middle region is x, the weight of the negative electrode coating in the first region is y, and the weight of the negative electrode coating in the second region is z, x<y, and x<z. By adjusting the weight of the negative electrode coating in the middle region to be the smallest, the negative electrode capacity in the middle region is respectively smaller than the negative electrode capacity in the first region and the negative electrode capacity in the second region, which is highly feasible.

[0043] This situation is applicable to the case where the materials of the coatings in the first region, the second region and the middle region of the negative electrode plate are the same. In this way, by controlling the weight of different regions, such as the coating thickness, the negative electrode capacity in the middle region can be made smaller than the negative electrode capacity in the first region and the negative electrode capacity in the second region, respectively. This is highly feasible.

[0044] In some embodiments, the negative electrode plate includes a current collector and a negative electrode coating coated on the current collector, the mass proportion of the active material in the negative electrode coating in the middle region is a, the mass proportion of the active material in the negative electrode coating in the first region is b, and the mass proportion of the active material in the negative electrode coating in the second region is c, a<b, and a<c, reducing the proportion of the active material in the middle region, so that the negative electrode capacity in the middle region is smaller than the negative electrode capacity in the first region and the negative electrode capacity in the second region, respectively. The method is simple and easy to control.

[0045] It can be understood that the negative electrode plate includes a negative electrode current collector and a negative electrode coating on the negative electrode current collector, wherein the negative electrode coating includes a negative electrode active material.

[0046] This situation is applicable to the case where the materials of the coatings in the first region, the second region and the middle region of the negative electrode plate are the same but have different specific gravities. In this way, the specific gravities of the active materials in different regions can be controlled to achieve a negative electrode capacity in the middle region that is smaller than the negative electrode capacity in the first region and the negative electrode capacity in the second region. This is highly feasible and different optimizations can be achieved for lithium-ion battery performance by adjusting the type of negative electrode active material.

[0047] In some embodiments, the specific capacity of the active material in the middle region is m, the specific capacity of the active material in the first region is n, and the specific capacity of the active material in the second region is p, m<n, and m<p. Specifically, active materials with different specific capacities can be selected in different regions to achieve a negative electrode capacity in the middle region that is smaller than the negative electrode capacity in the first region and the negative electrode capacity in the second region, respectively. The method is simple and easy to operate.

[0048] This situation is applicable to the case where the materials of the coatings in the first region, the second region and the middle region of the negative electrode plate are all different. In this way, by controlling the types of active materials in different regions, the negative electrode capacity in the middle region can be made smaller than the negative electrode capacity in the first region and the negative electrode capacity in the second region, respectively. This is highly feasible.

[0049] In the selection of the type of negative electrode material, one or more negative electrode materials can be mixed. And they are different negative electrode active materials. If it is a carbon-based negative electrode material, a carbon-based negative electrode material with a specific capacity in the range of 250 to 500 mAh / g is used. If it is a silicon, silicon-carbon, silicon-oxygen negative electrode or a mixed negative electrode of a carbon-based negative electrode and a silicon, silicon-carbon, silicon-oxygen negative electrode, a carbon-based negative electrode material with a specific capacity in the range of 400 to 1500 mAh / g is used.

[0050] In the embodiment of the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode coating on the negative electrode current collector. The negative electrode coating includes a negative electrode active material, and the negative electrode active material is one or more of carbon-based negative electrode materials such as artificial graphite, natural graphite, soft carbon, hard carbon, mesophase carbon microspheres, graphene, silicon, silicon oxygen, and silicon carbon.

[0051] The negative electrode coating also includes a binder, which includes polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin or nylon, etc., which are not limited here.

[0052] The negative electrode coating may also include a conductive material, which includes carbon black, acetylene black, Ketjen black, carbon fiber, carbon nanotubes, metal powder, metal fiber, copper, nickel, aluminum, silver or polyphenylene derivatives, etc., which are not limited here.

[0053] The negative electrode current collector includes, but is not limited to: copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam or a polymer substrate coated with a conductive metal.

[0054] In a second aspect, the present application proposes a method for preparing the negative electrode sheet in the above embodiment, comprising the following steps:

[0055] Provide a current collector, wherein the current collector is divided into a first region, a middle region, and a second region arranged in sequence in a width direction thereof;

[0056] A first coating layer is prepared in the first region, an intermediate coating layer is prepared in the middle region, and a second coating layer is coated in the second region to obtain a negative electrode sheet, wherein the negative electrode capacity of the intermediate coating layer is smaller than the negative electrode capacity of the first coating layer and the negative electrode capacity of the second coating layer, respectively.

[0057] Specifically, the purpose of adjusting the C1 / C3 or C2 / C3 ratio can be achieved by adjusting the coating weight of the intermediate coating layer, the first coating layer, and the second coating layer, or the specific gravity of the negative electrode active material in the negative electrode coating, or the type of the negative electrode active material in the negative electrode coating, or by adjusting two or three of the above three at the same time.

[0058] An embodiment of the preparation of the negative electrode sheet: graphite, styrene-butadiene rubber (SBR for short), and sodium carboxymethyl cellulose (CMC for short) are fully stirred and mixed in deionized water at a certain specific gravity to form a uniform negative electrode slurry; different negative electrode slurries are applied to different areas of the negative electrode collector copper foil and dried, and the coated negative electrode is cold pressed, cut and welded using a roller press.

[0059] The method for preparing the negative electrode plate proposed in the embodiment of the present application adjusts the parameters such as the specific gravity of the negative electrode active material in the middle coating layer, the first coating layer and the second coating layer or the type of the negative electrode active material in the negative electrode coating, so that the negative electrode capacity of the middle area is smaller than the negative electrode capacity of the first area and the negative electrode capacity of the second area respectively. Compared with other methods, the method for preparing the negative electrode plate prepared in the present application is more convenient. In addition, the method for preparing the negative electrode plate prepared in the present application has all the beneficial effects of the negative electrode plate of the above-mentioned embodiment, which will not be repeated here one by one.

[0060] In a third aspect, the present application provides a secondary battery, comprising the negative electrode plate in the above embodiment.

[0061] Secondary battery cells, taking lithium-ion battery cells as an example, lithium-ion battery cells include the negative electrode plates as described in the above embodiments, and also include positive electrode plates, separators and electrolytes. The electrolyte that can be used in the present application can be an electrolyte known in the prior art, including organic solvents, lithium salts and additives; the separator that can be used in the present application can be a separator known in the prior art; the positive electrode of the present application can be a positive electrode known in the prior art. Lithium-ion battery cells mainly rely on the movement of lithium ions between the positive electrode plates and the negative electrode plates to work. The thin film structure of the three layers of materials in the cylindrical battery cell is wound into a cylindrical electrode assembly, while in the rectangular battery cell, the thin film structure is wound or stacked into an electrode assembly with a roughly rectangular shape.

[0062] In a common battery cell structure, the battery cell includes a shell, an electrode assembly and an electrolyte. The electrode assembly is contained in the shell of the battery cell, and the electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator. The shell includes a shell and an end cap. The shell includes a housing formed by a plurality of walls and an opening. The end cap is arranged at the opening to close the housing chamber. In addition to the electrode assembly, the housing chamber also contains an electrolyte. The positive electrode sheet and the negative electrode sheet in the electrode assembly include tabs. In order to ensure that a large current passes without melting, the number of positive tabs is multiple and stacked together, and the number of negative tabs is multiple and stacked together. The tabs are electrically connected to the electrode terminals located outside the battery cell through connecting members, and the electrode terminals generally include a positive electrode terminal and a negative electrode terminal. For a rectangular battery cell, the electrode terminal is generally arranged at the end cap portion. A plurality of battery cells are connected in series and / or in parallel via the electrode terminals for application in various applications.

[0063] The battery composed of cells formed by winding is called a wound battery. Wound batteries are also called cells, and battery industry insiders call them roll cores. Compared with flat batteries, wound batteries are made of plates with a thickness of only about 1mm and wound at high voltage. Through special process means, the battery has many characteristics: super high-rate discharge capability, with a maximum discharge rate of 18C to 30C; excellent high and low temperature performance, can work at -55℃ to 150℃; stable high output voltage, higher energy density; sturdy structure, with excellent seismic resistance; no free electrolyte (such as colloidal acid), can be placed in any direction for work; can be quickly charged, and can be charged with more than 95% of the power within 40 minutes (1C charging); super long life, the designed floating charge life can reach more than 8 years; extremely high resistance to low current deep discharge.

[0064] The lithium-ion battery proposed in this application has all the beneficial effects of the above-mentioned isolation membrane, which will not be described in detail here.

[0065] Secondary battery cells can form a battery module. A battery module is formed by electrically connecting a certain number of secondary batteries together and placing them in a frame in order to protect the battery cells from external impact, heat, vibration, etc. A commonly used battery module generally includes two end plates, between which a plurality of battery cells (lithium-ion batteries) are arranged. The end plate with the output pole of the battery module is also called the output pole end plate, and the end plate without the output pole of the battery module is also called the non-output pole end plate.

[0066] Battery modules can form battery packs. In some battery production and processing technologies, multiple battery cells are first integrated into battery modules, and then the battery modules are packaged in the battery box to form a battery pack. A battery pack can be packaged with multiple battery modules in one row or multiple rows. The arrangement of multiple rows of multiple battery modules can be double rows and multiple columns, multiple rows and double columns, multiple rows and multiple columns, etc. Taking a battery pack with double rows and multiple columns of battery modules as an example, the first end plate of each column is generally the head output extreme plate, the two adjacent end plates between the two rows of battery modules are the middle non-output extreme plates, and the last end plate of each column is the tail non-output extreme plate. The head output extreme plate and one of the middle non-output extreme plates belong to the first row of battery modules, and one of the middle non-output extreme plates and the tail output extreme plate belong to the second row of battery modules.

[0067] In a fourth aspect, the present application provides an electrical device, comprising the secondary battery in the above-mentioned embodiment.

[0068] The electrical devices proposed in the present application include but are not limited to: mobile phones, portable devices, laptop computers, electric vehicles, electric vehicles, ships, spacecraft, electric toys and electric tools, etc. For example, spacecraft include airplanes, rockets, space shuttles and spacecraft, etc. Electric toys include fixed or mobile electric toys, such as game consoles, electric vehicle toys, electric ship toys and electric airplane toys, etc. Electric tools include metal cutting electric tools, grinding electric tools, assembly electric tools and railway electric tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers.

[0069] The electrical device proposed in this application has all the beneficial effects of the above-mentioned negative electrode plate, which will not be described in detail here.

[0070] The technical solution of the present application is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present application and are not used to limit the present application.

[0071] The negative electrode plate parameters of Examples 1 to 9 and Comparative Examples 1 and 2 are shown in Table 1 below:

[0072] Table 1 Negative electrode sheet parameters of Examples 1 to 9 and Comparative Examples 1 and 2

[0073]

[0074]

[0075] Example 1

[0076] A current collector is provided, wherein the current collector is divided into a first region, a middle region, and a second region arranged in sequence in the width direction; a first coating layer is prepared in the first region, an intermediate coating layer is prepared in the middle region, a second coating layer is coated in the second region, and the coating is dried; a roller press is used to cold press, cut, and weld the coated negative electrode to obtain a negative electrode sheet, wherein the negative electrode capacity of the intermediate coating layer is respectively less than the negative electrode capacity of the first coating layer and the negative electrode capacity of the second coating layer. The weights of the negative electrode coatings of the intermediate coating layer, the first coating layer, and the second coating layer are different, refer to x, y, and z in Table 1.

[0077] Example 2

[0078] A current collector is provided, wherein the current collector is divided into a first region, a middle region, and a second region arranged in sequence in the width direction; a first coating layer is prepared in the first region, an intermediate coating layer is prepared in the middle region, a second coating layer is coated in the second region, and the coating is dried; a roller press is used to cold press, cut, and weld the coated negative electrode to obtain a negative electrode sheet, wherein the negative electrode capacity of the intermediate coating layer is respectively less than the negative electrode capacity of the first coating layer and the negative electrode capacity of the second coating layer. The weights of the negative electrode coatings of the intermediate coating layer, the first coating layer, and the second coating layer are different, refer to x, y, and z in Table 1.

[0079] Example 3

[0080] A current collector is provided, wherein the current collector is divided into a first region, a middle region, and a second region arranged in sequence in the width direction; a first coating layer is prepared in the first region, an middle coating layer is prepared in the middle region, a second coating layer is coated in the second region, and the coating is dried, and a roller press is used to cold press, cut, and weld the coated negative electrode to obtain a negative electrode sheet, wherein the negative electrode capacity of the middle coating layer is respectively less than the negative electrode capacity of the first coating layer and the negative electrode capacity of the second coating layer. The mass proportions of active materials in the middle coating layer, the first coating layer, and the second coating layer are different, refer to a, b, and c in Table 1.

[0081] Example 4

[0082] A current collector is provided, wherein the current collector is divided into a first region, a middle region, and a second region arranged in sequence in the width direction; a first coating layer is prepared in the first region, an middle coating layer is prepared in the middle region, a second coating layer is coated in the second region, and the coating is dried, and a roller press is used to cold press, cut, and weld the coated negative electrode to obtain a negative electrode sheet, wherein the negative electrode capacity of the middle coating layer is respectively less than the negative electrode capacity of the first coating layer and the negative electrode capacity of the second coating layer. The types of active materials, i.e., specific capacities, of the middle coating layer, the first coating layer, and the second coating layer are different, refer to m, n, and p in Table 1.

[0083] Example 5

[0084] Except for the different values ​​of H1 / H3 and H2 / H3, the rest of the preparation method is the same as Example 1.

[0085] Example 6

[0086] Except for the different values ​​of y and z, the rest of the preparation method is the same as Example 1.

[0087] Example 7

[0088] Except for the type of active substance and the values ​​of m, n and p, the rest of the preparation method is the same as Example 4.

[0089] Example 8

[0090] Except for the different values ​​of a, b and c, the rest of the preparation method is the same as Example 3.

[0091] Example 9

[0092] Except for the different values ​​of H1 / H3 and H2 / H3, the rest of the preparation method is the same as Example 1.

[0093] Comparative Example 1

[0094] Referring to the parameters in Table 1, a uniform coating layer was prepared on the base film to obtain a negative electrode sheet.

[0095] Comparative Example 2

[0096] Referring to the parameters in Table 1, a uniform coating layer was prepared on the base film to obtain a negative electrode sheet.

[0097] It should be noted that in the examples and comparative examples, styrene-butadiene rubber and sodium carboxymethyl cellulose are also added to the coating layer as a binder and a conductive agent.

[0098] Negative electrode capacity test: Take the first area, second area or middle area of ​​the negative electrode plates of Examples 1 to 9 and Comparative Examples 1 to 2, and assemble them into a button battery with a lithium metal negative electrode. First, place the button battery in a constant temperature environment of 25°C for 1 hour. Then discharge to 0.005V at 0.01C, discharge to 0.005V at 50μA, leave for 5 minutes, and charge to 2V at 0.1C. Take the discharge capacity as the negative electrode capacity C.

[0099] Battery lithium deposition test: The negative electrode sheets of Examples 1 to 9 and Comparative Examples 1 to 2 are assembled into laminated batteries, and the batteries are placed in a 25°C environment for 1 hour, and the battery cells are charged at a constant current rate of 2C. After charging to 3.65V, they are switched to constant voltage charging. Charging is stopped when the charging current is lower than 0.05C, and the battery is left for 5 minutes. Then, the battery is discharged at a constant current rate of 1C to 2.5V, and left for 5 minutes. After 50 charge and discharge cycles, the battery is disassembled to observe the lithium deposition on the surface of the negative electrode. Determination of the degree of lithium deposition in the first area, the second area, and the middle area of ​​the negative electrode sheet: Determine the state of the negative electrode sheet after the battery is fully charged and disassembled after the lithium deposition test. When the first area and the second area of ​​the negative electrode are golden yellow as a whole and the area of ​​gray displayed is less than 0.5%, it is determined that there is no lithium deposition at the edge. When most of the first area and the second area of ​​the negative electrode are yellow, but gray can be observed in some positions, and the gray area is greater than 0.5%, it is determined that there is lithium deposition at the edge.

[0100] Battery room temperature 2C cycle test: Take the lithium-ion batteries in the examples and comparative examples, and ensure that there are at least 2 parallel samples for each example. First, place the battery in a constant temperature environment of 25°C for 1 hour. Then charge the battery with a constant current at a charging rate of 2C, and switch to constant voltage charging after charging to 3.65V. Stop charging when the charging current is lower than 0.05C, and leave it for 5 minutes. Then use a discharge rate of 1C to discharge the battery with a constant current to 2.5V, and leave it for 5 minutes. The above process is cycled for a specific number of times, and the capacity retention rate is calculated as follows: Capacity retention rate of the nth cycle = discharge capacity of the nth cycle / discharge capacity of the second cycle*100%.

[0101] The test results are shown in Table 2:

[0102] Table 2 Performance measurement of Examples 1 to 9 and Comparative Examples 1 to 2

[0103]

[0104] It can be seen from Table 2 that the negative electrode plates of Examples 1 to 9 of the present application and the resulting lithium-ion batteries have a negative electrode capacity in the middle region that is smaller than the negative electrode capacity of the first region and the negative electrode capacity of the second region, respectively, thereby reducing the polarization potential of the first region and the second region, thereby optimizing the polarization potential of each part in the width direction of the negative electrode plate during lithium ion charging, improving the uniformity of lithium insertion, and further improving the problem of lithium plating at the edge of the plate, thereby improving the cycle performance of the lithium-ion battery.

[0105] Through Examples 1, 2, 3, 4, 5 and Comparative Examples 1 and 2, it can be found that by increasing the weight of the negative electrode coating in the first region and the second region of the negative electrode plate, or by increasing the specific gravity of the negative electrode active material in the negative electrode coating in the first region and the second region of the negative electrode plate, or by changing the type of negative electrode active material in the negative electrode coating in the first region and the second region of the negative electrode plate, the purpose of regulating C1 / C3 or C2 / C3 to meet 1.01≤C1 / C3≤1.1, 1.02≤C2 / C3≤1.1 can be achieved, and the cycle performance can be significantly improved; further, through Examples 6, 7, 8, it can be found that when C1 / C3 and C2 / C3 are in the optimal range of 1.02-1.05, the performance is better.

[0106] To sum up, the negative electrode pole piece proposed in the present application has a negative electrode capacity in the middle region that is smaller than the negative electrode capacity in the first region and the negative electrode capacity in the second region, respectively, thereby reducing the polarization potential in the first region and the second region, thereby optimizing the polarization potential of each part in the width direction of the negative electrode pole piece during lithium ion charging, improving the uniformity of lithium insertion, and further improving the problem of lithium plating at the edge of the pole piece, thereby improving the cycle performance of the lithium ion battery.

[0107] The above are only preferred embodiments of the present application, and do not limit the scope of the present application. For those skilled in the art, the present application may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the scope of the patent protection of the present application.

Claims

1. A negative electrode plate, characterized in that the negative electrode plate comprises a first region, a middle region and a second region arranged in sequence along the width direction thereof, wherein the negative electrode capacity of the middle region is smaller than the negative electrode capacity of the first region and the negative electrode capacity of the second region respectively; the negative electrode capacity of the first region is C1, the negative electrode capacity of the second region is C2, and the negative electrode capacity of the middle region is C3: 1.01≤C1 / C3≤1.1; 1.01≤C2 / C3≤1.1; In the width direction of the negative electrode sheet, the size of the first area is H1, the size of the second area is H2, and the size of the middle area is H3: 0.01≤H1 / H3≤0.2; 0.01≤H2 / H3≤0.

2.

2. The negative electrode sheet according to claim 1, characterized in that: The negative electrode capacity of the first region is C1, the negative electrode capacity of the second region is C2, and the negative electrode capacity of the middle region is C3: 1.02≤C1 / C3≤1.05; and / or, 1.02≤C2 / C3≤1.

05.

3. The negative electrode sheet according to claim 1, characterized in that: The negative electrode plate includes a current collector and a negative electrode coating coated on the current collector, the weight of the negative electrode coating in the middle region is x, the weight of the negative electrode coating in the first region is y, and the weight of the negative electrode coating in the second region is z, x<y, and x<z.

4. The negative electrode sheet according to claim 1, characterized in that: The negative electrode plate includes a current collector and a negative electrode coating coated on the current collector, the mass proportion of the active material in the negative electrode coating in the middle region is a, the mass proportion of the active material in the negative electrode coating in the first region is b, and the mass proportion of the active material in the negative electrode coating in the second region is c, a<b, and a<c.

5. The negative electrode sheet according to claim 1, characterized in that: The specific capacity of the active material in the middle region is m, the specific capacity of the active material in the first region is n, and the specific capacity of the active material in the second region is p, m<n, and m<p.

6. A method for preparing a negative electrode sheet according to any one of claims 1 to 5, characterized in that: The following steps are involved: Provide a current collector, wherein the current collector is divided into a first region, a middle region, and a second region arranged in sequence in a width direction thereof; A first coating layer is prepared in the first region, an intermediate coating layer is prepared in the middle region, and a second coating layer is coated in the second region to obtain a negative electrode sheet, wherein the negative electrode capacity of the intermediate coating layer is smaller than the negative electrode capacity of the first coating layer and the negative electrode capacity of the second coating layer, respectively.

7. A secondary battery, characterized in that: Comprising the negative electrode sheet as described in any one of claims 1 to 6.

8. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to claim 7.