Laminated lithium-ion battery
By setting a small-area adhesive layer on the separator and a barrier layer on the positive electrode current collector, the problem of the adhesive layer blocking the lithium ion channel is solved, the scope of lithium deposition on the negative electrode sheet is reduced, and the charging efficiency and stability of the battery are improved. sex.
Patent Information
- Application Number
- CN202111131673.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-09-26
AI Technical Summary
In existing stacked lithium-ion batteries, the glue layer blocks the lithium ion channel of the negative electrode piece, causing large-area lithium deposition on the negative electrode piece during the charging process.
An adhesive layer with an area smaller than the separator is provided on both sides of the separator, and a barrier layer is provided on the surface of the positive electrode current collector to block electron transmission, reduce the area occupied by the adhesive layer, and prevent clogging of the lithium ion channel.
It effectively alleviates the lithium precipitation of the negative electrode plate, improves the charging efficiency and stability of the battery, and prevents short circuits.
Smart Images

Figure CN115882079B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and more specifically, to a laminated lithium-ion battery. Background Art
[0002] In the prior art, laminated lithium-ion batteries usually have adhesive layers of the same shape as the diaphragm applied on both sides of the diaphragm, and the diaphragm is bonded to the positive and negative electrodes through the adhesive layers. However, the adhesive layer will block the lithium ion channels in the negative electrode to a certain extent, thus causing large-area lithium deposition on the negative electrode during charging. Summary of the invention
[0003] One purpose of the present application is to provide a new technical solution for stacked lithium-ion batteries, which can solve the technical problem of lithium plating in the negative electrode sheets of the prior art.
[0004] According to a first aspect of the present application, a laminated lithium-ion battery is provided, comprising: a positive electrode plate, the positive electrode plate comprising a positive electrode collector, a barrier layer and a positive electrode active material, the positive electrode collector having a first surface and a second surface arranged opposite to each other, the barrier layer and the positive electrode active material are respectively attached to a partial area of the first surface; the barrier layer is used to block electron transmission; a negative electrode plate; and a diaphragm, arranged between the positive electrode plate and the negative electrode plate, and adhesive layers are respectively provided on both side surfaces of the diaphragm; wherein the area of the adhesive layer is smaller than the area of the diaphragm, the positive electrode plate and the negative electrode plate are respectively connected to a part of the diaphragm through the adhesive layer, and the adhesive layer and the barrier layer are arranged opposite to each other.
[0005] According to one embodiment of the present application, the positive electrode active material covers at least a portion of the barrier layer.
[0006] According to one embodiment of the present application, the positive electrode sheet includes a positive electrode tab, which is electrically connected to the positive electrode collector and is arranged adjacent to the barrier layer, and the negative electrode sheet includes a negative electrode tab, the positive electrode tab and the negative electrode tab are located on the same side of the diaphragm, and a portion of the barrier layer extends to the surface of the positive electrode tab and is arranged opposite to the negative electrode tab.
[0007] According to an embodiment of the present application, in the direction from the positive electrode sheet to the negative electrode sheet, the orthographic projection of the negative electrode active material of the negative electrode sheet on the separator covers the orthographic projection of the positive electrode active material on the separator.
[0008] According to an embodiment of the present application, the barrier layer includes an adhesive, and the adhesive of the barrier layer is a hot-melt material.
[0009] According to an embodiment of the present application, the adhesive layer includes an adhesive, and the adhesive of the adhesive layer is a hot-melt material.
[0010] According to an embodiment of the present application, there are plural barrier layers and plural adhesive layers, respectively, and the plurality of barrier layers and the plurality of adhesive layers correspond one to one.
[0011] According to one embodiment of the present application, the diaphragm is in the shape of an elongated strip, the number of the adhesive layers is two, the two adhesive layers are spaced apart and distributed along the length direction of the diaphragm, and each adhesive layer is located on the wide side of the diaphragm and extends along the width direction of the diaphragm.
[0012] According to one embodiment of the present application, the area on the diaphragm where the adhesive layer is not provided is spaced apart from the positive electrode sheet and the negative electrode sheet, respectively, and the area on the diaphragm where the adhesive layer is provided is close to the edge of the diaphragm.
[0013] According to one embodiment of the present application, the area of the barrier layer is not less than the area of the adhesive layer.
[0014] According to one embodiment of the present disclosure, by providing an adhesive layer with a smaller area than the diaphragm on the diaphragm, the area occupied by the adhesive layer can be reduced, and the range of lithium deposition on the negative electrode plate can be reduced. By providing a barrier layer on the first surface of the positive electrode current collector, it can play a role in blocking electron transmission, effectively alleviating the situation of lithium deposition on the negative electrode plate corresponding to the adhesive layer.
[0015] Other features and advantages of the present application will become apparent from the following detailed description of exemplary embodiments of the present application with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the application and, together with the description, serve to explain the principles of the application.
[0017] Figure 1 is a schematic cross-sectional view of an assembly of a laminated lithium-ion battery provided by an embodiment of the present application;
[0018] Figure 2 is a schematic cross-sectional view of an assembly of a laminated lithium-ion battery provided in yet another embodiment of the present application;
[0019] Figure 3 It is a schematic diagram of the assembly process of the positive electrode sheet of a laminated lithium-ion battery provided by one embodiment of the present application;
[0020] Figure 4 It is a schematic cross-sectional assembly diagram of a positive electrode sheet of a laminated lithium-ion battery provided by an embodiment of the present application;
[0021] Figure 5 It is a schematic diagram of the assembly process of a diaphragm of a laminated lithium-ion battery provided by an embodiment of the present application;
[0022] Figure 6 is a schematic cross-sectional diagram of an assembly of a diaphragm of a laminated lithium-ion battery provided by an embodiment of the present application;
[0023] Figure 7 It is a schematic cross-sectional assembly diagram of a negative electrode sheet of a laminated lithium-ion battery provided by an embodiment of the present application;
[0024] Figure 8 It is a schematic diagram of the assembly of the positive electrode current collector and the barrier layer of a laminated lithium-ion battery provided in one embodiment of the present application.
[0025] Reference numerals
[0026] Laminated lithium-ion battery 100;
[0027] Positive electrode sheet 10;
[0028] Positive electrode current collector 11; first region 111; second region 112;
[0029] Positive electrode active material 12; first positive electrode active material 121; second positive electrode active material 122;
[0030] Positive electrode tab 13;
[0031] Diaphragm 20;
[0032] Negative electrode sheet 30; negative electrode current collector 31; negative electrode active material 32; negative electrode tab 33;
[0033] Barrier layer 40; first barrier layer 41; second barrier layer 42;
[0034] Adhesive layer 50 ; first adhesive layer 51 ; second adhesive layer 52 . DETAILED DESCRIPTION
[0035] Various exemplary embodiments of the present application will now be described in detail with reference to the accompanying drawings. It should be noted that unless otherwise specifically stated, the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present application.
[0036] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the present application, its application, or uses.
[0037] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0038] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0039] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0040] The laminated lithium-ion battery 100 according to the embodiment of the present application is described below with reference to the accompanying drawings.
[0041] like Figures 1 to 8 As shown, the laminated lithium-ion battery 100 according to the embodiment of the present application includes a positive electrode sheet 10, a separator 20 and a negative electrode sheet 30. The positive electrode sheet 10 includes a positive electrode current collector 11, a barrier layer 40 and a positive electrode active material 12.
[0042] Specifically, the positive electrode current collector 11 has a first surface and a second surface that are arranged opposite to each other, and the barrier layer 40 and the positive electrode active material 12 are respectively attached to a partial area of the first surface of the positive electrode current collector 11. The barrier layer 40 is used to block electron transmission. The diaphragm 20 is arranged between the positive electrode plate 10 and the negative electrode plate 30, and an adhesive layer 50 is respectively provided on both sides of the diaphragm 20. Among them, the area of the adhesive layer 50 is smaller than the area of the diaphragm 20, and the positive electrode plate 10 and the negative electrode plate 30 are respectively connected to a part of the diaphragm 20 through the adhesive layer 50, and the adhesive layer 50 is arranged opposite to the barrier layer 40.
[0043] In other words, the laminated lithium-ion battery 100 according to the embodiment of the present application is mainly composed of a positive electrode sheet 10, a separator 20 and a negative electrode sheet 30. The positive electrode sheet 10 of the embodiment of the present application is mainly composed of a positive current collector 11, a barrier layer 40, and a positive active material 12. The positive current collector 11 has a first surface and a second surface. When the positive current collector 11 is arranged in a horizontal direction, the first surface of the positive current collector 11 can be the upper surface of the positive current collector 11 or the lower surface of the positive current collector 11.
[0044] The positive electrode collector 11 has a first surface and a second surface at the same time, and the positive electrode active material 12, the separator 20 and the negative electrode plate 30 can be sequentially arranged on the first surface and the second surface of the positive electrode collector 11, respectively. That is, the positive electrode plate 10, the separator 20 and the negative electrode plate 30 can be stacked in an interlaced manner to form a laminated battery cell. A unit in the laminated battery cell may include a positive electrode plate 10, a separator 20 and a negative electrode plate 30. The positive electrode plate 10 and the negative electrode plate 30 are respectively located on both sides of the separator 20. The separator 20 may be located above the positive electrode collector 11 and / or below the positive electrode collector 11. When the first surface of the positive electrode plate 10 is defined as the upper surface of the positive electrode collector 11, the separator 20 may be located above the first surface of the positive electrode collector 11. When the first surface of the positive electrode collector 11 is defined as the lower surface of the positive electrode collector 11, the separator 20 may be located below the first surface of the positive electrode collector 11. By defining the positional relationship between the first surface of the positive current collector 11 and the separator 20 , it is not only convenient to assemble the laminated battery cell, but also convenient for the barrier layer 40 on the positive current collector 11 to cooperate with the adhesive layer 50 on the separator 20 .
[0045] Along the extension direction of the first surface of the positive electrode current collector 11, the barrier layer 40 and the positive electrode active material 12 are respectively provided on the positive electrode current collector 11. In other words, Figure 4 As shown, there are a first region 111 and a second region 112 on the first surface of the positive electrode current collector 11. The first region 111 and the second region 112 can be arranged adjacent to each other or spaced apart. A barrier layer 40 is arranged in the first region 111. During production and processing, the barrier layer 40 can be combined with the positive electrode current collector 11 corresponding to the first region 111 by coating, gluing, etc. The barrier layer 40 can be arranged entirely in the first region 111, or partially in the first region 111.
[0046] The positive electrode active material 12 is disposed in the second region 112. During production and processing, the positive electrode active material 12 can be disposed in the second region 112 by coating or the like. The positive electrode active material 12 can be disposed entirely in the second region 112 or partially in the second region 112.
[0047] The first surface of the separator 20 is connected to the positive electrode sheet 10. The second surface of the separator 20 is connected to the negative electrode sheet 30. The positive electrode sheet 10, the separator 20 and the negative electrode sheet 30 can be stacked in an interlaced manner to form a laminated battery cell. The laminated lithium-ion battery 100 of the present application also includes an electrolyte and a shell, which will not be described in detail here.
[0048] In addition, if Figure 1 and Figure 2 As shown, the separator 20 and the positive electrode sheet 10 and the negative electrode sheet 30 are connected by an adhesive layer 50. For example, Figure 5 and Figure 6 As shown, the adhesive layer 50 can be divided into a first adhesive layer 51 and a second adhesive layer 52, and the positive electrode sheet 10 and the separator 20 can be connected through the first adhesive layer 51. The negative electrode sheet 30 and the separator 20 are connected through the second adhesive layer 52. In order to improve the structural stability, simplify the processing technology and reduce the area of the barrier layer 40, the first adhesive layer 51 and the second adhesive layer 52 can be overlapped in the direction from the positive electrode sheet 10 to the negative electrode sheet 30.
[0049] The cooperation principle between the barrier layer 40 and the adhesive layer 50 will be described in detail below.
[0050] The barrier layer 40 is located on a portion of the first surface of the positive electrode collector 11. Since a portion of the separator 20 is connected to the positive electrode sheet 10 and the negative electrode sheet 30 respectively through the adhesive layer 50, and the area of the adhesive layer 50 is smaller than the area of the separator 20, the area occupied by the adhesive layer 50 can be reduced, thereby reducing the number of blockages of the lithium ion channel on the negative electrode sheet 30 caused by the provision of the adhesive layer 50. In other words, the separator 20 is defined as an area coated with the adhesive layer 50 and an area not coated with the adhesive layer 50. The area on the separator 20 where the adhesive layer 50 is not coated is in a state where the lithium ion channel is unobstructed.
[0051] In order to further avoid lithium deposition at the position of the negative electrode plate 30 corresponding to the adhesive layer 50, a first region 111 is provided on the positive electrode collector 11, and a barrier layer 40 is provided in the first region 111. During the battery charging process, due to the presence of the barrier layer 40, the electrons corresponding to the first region 111 will not be able to pass through the barrier layer 40 to be transported to the positive electrode collector 11, and will not be able to migrate to the negative electrode plate 30 through the external circuit. At the same time, the lithium ions corresponding to the first region 111 will not be able to pass through the diaphragm 20 in the electrolyte to reach the negative electrode collector 31, and there will be no problem that the lithium ions cannot be embedded in the lattice of the negative electrode plate 30, and thus lithium deposition on the surface of the negative electrode plate 30 will not be caused.
[0052] It should be noted that the first region 111 here includes the following two situations: Situation 1, there is a positive electrode active material 12 between the first region 111 and the separator 20, and the lithium ions corresponding to the first region 111 are the lithium ions in the positive electrode active material 12 between the first region 111 and the separator 20. Situation 2, there is no positive electrode active material 12 between the first region 111 and the separator 20, and at this time there are no lithium ions that can pass through the separator 20 in the electrolyte to reach the negative electrode current collector 31.
[0053] It can be seen that the laminated lithium-ion battery 100 of the present application can prevent the presence of lithium ions that can participate in the battery reaction in the first region 111 by providing the barrier layer 40, thereby preventing lithium deposition on the negative electrode sheet 30 corresponding to the first region 111. The region on the negative electrode sheet 30 corresponding to the first region 111 refers to the position on the negative electrode sheet 30 where the lithium ions corresponding to the first region 111 undergo a battery reaction.
[0054] In this embodiment, on the one hand, by providing an adhesive layer 50 having an area smaller than that of the diaphragm 20 on the diaphragm 20, not only can the area occupied by the adhesive layer 50 be reduced, and the range of the negative electrode plate 30 that is easy to precipitate lithium can be reduced, but also the diaphragm 20, the positive electrode plate 10 and the negative electrode plate 30 can be fixed to avoid misalignment between the diaphragm 20, the positive electrode plate 10 and the negative electrode plate 30, causing a short circuit. On the other hand, by providing a barrier layer 40 on the first surface of the positive electrode collector 11, it can play a role in blocking electron transmission, and can isolate the electrons corresponding to the first region 111 from migrating to the positive electrode collector 11. When the barrier layer 40 and the adhesive layer 50 are partially overlapped, the lithium ions in the positive active material 12 corresponding to the first region 111 can be prevented from participating in the battery reaction, thereby effectively alleviating the situation of lithium precipitation of the negative electrode plate 30 corresponding to the adhesive layer 50. When the barrier layer 40 and the adhesive layer 50 are completely overlapped, the lithium ions in the positive electrode active material 12 corresponding to the first region 111 can be prevented from participating in the battery reaction, thereby effectively preventing the negative electrode sheet 30 corresponding to the adhesive layer 50 from lithium deposition.
[0055] According to one embodiment of the present application, Figure 3 and Figure 4 As shown, the positive electrode active material 12 covers at least part of the barrier layer 40. That is, along the direction from the negative electrode plate 30 to the positive electrode plate 10, the positive electrode active material 12 covers the barrier layer 40. That is, the positive electrode active material 12 covers the barrier layer 40 and the second region 112 at the same time. In other words, the positive electrode active material 12 is arranged on the same side of the barrier layer 40 and the second region 112 at the same time. At this time, the positive electrode plate 10 is mainly composed of the positive current collector 11, the positive electrode active material 12 arranged on the first surface of the positive current collector 11, and the barrier layer 40 arranged between the positive current collector 11 and the positive electrode active material 12.
[0056] For ease of description, the positive electrode current collector 11 is arranged in the horizontal direction. In this case, a barrier layer 40 may be arranged in the first region 111 above the positive electrode current collector 11, and a positive electrode active material 12 may be arranged above the barrier layer 40 and above the second region 112. A barrier layer 40 may also be arranged in the first region 111 below the positive electrode current collector 11, and a positive electrode active material 12 may be arranged below the barrier layer 40 and below the second region 112.
[0057] When preparing, Figure 3 As shown, the positive electrode current collector 11 can be arranged to extend in the horizontal direction, and the first region 111 and the second region 112 are arranged side by side in the horizontal direction. Subsequently, the barrier layer 40 can be coated on the first region 111 of the upper surface of the positive electrode current collector 11. Then, the positive electrode active material 12 is coated on the positive electrode current collector 11, and the positive electrode active material 12 covers the barrier layer 40 and the exposed positive electrode current collector 11 in the second region 112.
[0058] For ease of description, Figure 4 As shown, the positive electrode active material 12 can be divided into a first positive electrode active material 121 and a second positive electrode active material 122. The first positive electrode active material 121 is located on the side of the barrier layer 40 away from the positive electrode current collector 11. The second positive electrode active material 122 is located in the second region 112 of the positive electrode current collector 11. That is, the first positive electrode active material 121 covers the barrier layer 40, and the second positive electrode active material 122 covers the positive electrode current collector 11 in the second region 112. In other words, the first positive electrode active material 121 and the second positive electrode active material 122 can be formed by coating at the same time, with good thickness consistency, good bonding effect after pressing or hot pressing, and avoiding deformation and falling of the edge of the pole core.
[0059] It should be noted that the lithium ions in the first positive electrode active material 121 above the barrier layer 40 cannot participate in the battery reaction. The lithium ions in the second positive electrode active material 122 on one side of the barrier layer 40 along the horizontal direction can participate in the battery reaction.
[0060] That is to say, in this embodiment, by simultaneously providing the positive electrode active material 12 in the barrier layer 40 and the second region 112, the lithium ions in the positive electrode active material 12 corresponding to the barrier layer 40 can be prevented from participating in the battery reaction, and at the same time, the lithium ions in the positive electrode active material 12 in the second region 112 are not hindered from participating in the battery reaction.
[0061] In some specific embodiments of the present application, Figure 2 As shown, the positive electrode sheet 10 includes a positive electrode tab 13, which is electrically connected to the positive electrode collector 11 and is arranged adjacent to the barrier layer 40. The negative electrode sheet 30 includes a negative electrode tab 33. The positive electrode tab 13 and the negative electrode tab 33 are located on the same side of the diaphragm 20, and a portion of the barrier layer 40 extends to the surface of the positive electrode tab 13 and is arranged opposite to the negative electrode tab 33.
[0062] Among them, the positive electrode collector 11 is electrically connected to the positive electrode tab 13. The physical connection relationship between the positive electrode collector 11 and the positive electrode tab 13 may include the following: First, the positive electrode tab 13 may be integrally formed with the positive electrode collector 11, that is, a part of the positive electrode collector 11 may be used as the positive electrode tab 13. For example, when a part of the positive electrode collector 11 is used as the positive electrode tab 13, a first blank area may be provided at one end of the positive electrode collector 11, and the first blank area is the positive electrode tab 13. Second, the positive electrode tab 13 may also be connected to the positive electrode collector 11 by welding or the like.
[0063] When the positive electrode collector 11 is arranged in the horizontal direction, the positive electrode tab 13 can be located outside the positive electrode collector 11 in the horizontal direction, for example, the positive electrode tab 13 is located on the left side, right side, front side or rear side of the positive electrode collector 11, which is not limited here.
[0064] like Figure 7 As shown, the negative electrode sheet 30 includes a negative electrode collector 31, a negative electrode active material 32 coated on the negative electrode collector 31, and a negative electrode tab 33. A second blank area not coated with the negative electrode active material 32 can be provided at the end of the negative electrode collector 31 as the negative electrode tab 33. The negative electrode tab 33 can also be connected to the negative electrode collector 31 by welding or the like. If an insulating barrier layer is provided between the negative electrode collector 31 and the negative electrode active material 32, the lithium ions of the positive electrode active material 12 can freely enter and exit at the bonding position between the positive electrode active material 12 and the separator 20. The insulating barrier layer at the bonding position between the negative electrode active material 32 and the separator 20 hinders the conduction of electrons, and the lithium ions cannot be embedded, which will form lithium precipitation in this area. In comparison, the present application can prevent the lithium ions in the positive electrode active material 12 in this area from participating in the battery reaction by providing a barrier layer 40 on the positive electrode collector 11, and lithium precipitation will not occur in the bonding area between the negative electrode active material 32 and the separator 20.
[0065] The negative electrode tab 33 of the embodiment of the present application can be located on the same side or different sides as the positive electrode tab 13. When the negative electrode tab 33 and the positive electrode tab 13 are located on the same side, by providing the second barrier layer 42 at a position close to the root of the positive electrode tab 13, the positive electrode tab 13 and the negative electrode tab 33 are effectively prevented from overlapping and short-circuiting during the use of the battery. Here, the root of the positive electrode tab 13 refers to the connection position between the positive electrode tab 13 and the positive current collector 11.
[0066] Specifically, Figure 2As shown, when the positive electrode tab 13 and the negative electrode tab 33 are arranged on the same side of the separator 20, the embodiment of the present application extends a portion of the barrier layer 40 to the surface of the positive electrode tab 13 and is arranged opposite to the negative electrode tab 33, that is, a barrier layer 40 is provided between the positive electrode tab 13 and the negative electrode tab 33. The barrier layer 40 has the characteristic of hindering electron transmission, that is, it has insulating properties, so the barrier layer 40 is provided to effectively avoid overlapping and short-circuiting the positive electrode tab 13 and the negative electrode tab 33.
[0067] In other words, a first region 111 and a second region 112 are defined on the upper surface of the positive electrode current collector 11. The first region 111 is disposed adjacent to the positive electrode tab 13, and the barrier layer 40 includes a first barrier layer 41 and a second barrier layer 42. The first barrier layer 41 is disposed in the first region 111. The second barrier layer 42 is connected to the first barrier layer 41, and the second barrier layer 42 is disposed in the positive electrode tab 13.
[0068] Alternatively, if Figure 4 As shown, the number of first regions 111 is two. The number of second regions 112 is one. The second region 112 and the first region 111 are simultaneously arranged on the first surface of the positive electrode current collector 11, and are arranged side by side. Specifically, one first region 111 is located on the left side of the second region 112 in the horizontal direction. Another first region 111 is located on the right side of the second region 112 in the horizontal direction, and is arranged adjacent to the positive electrode tab 13. A first barrier layer 41 is arranged in each first region 111. A second barrier layer 42 is arranged on the positive electrode tab 13. The second barrier layer 42 is connected to the adjacent first barrier layer 41. That is, the second barrier layer 42 is connected to the first barrier layer 41 of the first region 111 located on the right side of the second region 112. It should be noted that the first barrier layer 41 and the second barrier layer 42 can be an integrally formed structure or can be formed by multiple production connections.
[0069] During production and processing, the barrier layer 40 can be applied to the first region 111 and the first blank region of the positive electrode collector 11 at one time. The first blank region can be used as the positive electrode tab 13. The barrier layer 40 in the first region 111 is the first barrier layer 41. The second barrier layer 42 is provided on a portion of the positive electrode tab 13. Subsequently, the positive electrode active material 12 is covered with the first barrier layer 41, and the second barrier layer 42 is not covered. Along the extension direction of the first surface of the positive electrode collector 11, the second barrier layer 42 is staggered with the positive electrode active material 12.
[0070] Along the extension direction of the first surface of the positive current collector 11, the width of the barrier layer 40 is 2 mm to 12 mm. For example, the barrier layer 40 and the positive current collector 11 are respectively in the shape of long strips, the barrier layer 40 is arranged on the wide side of the first surface of the positive current collector 11, the long side of the barrier layer 40 coincides with the wide side of the positive current collector 11, the wide side of the barrier layer 40 extends along the long side of the positive current collector 11, and the width of the barrier layer 40 is 2 mm to 12 mm. For example, Figure 8 As shown, the long side of the positive electrode current collector 11 extends along the first direction, and the wide side of the positive electrode current collector 11 extends along the second direction. The long side of the barrier layer 40 extends along the second direction, and the wide side of the barrier layer 40 extends along the first direction.
[0071] Optionally, along the extension direction of the first surface of the positive current collector 11, the width of the first barrier layer 41 is 2 mm to 12 mm. For example, the first barrier layer 41 and the positive current collector 11 are respectively long strips, and the first region 111 is arranged near the wide side of the first surface of the positive current collector 11. The first barrier layer 41 is arranged on the wide side of the first surface of the positive current collector 11, the long side of the first barrier layer 41 coincides with the wide side of the positive current collector 11, the wide side of the first barrier layer 41 extends along the long side of the positive current collector 11, and the width of the first barrier layer 41 is 2 mm to 12 mm.
[0072] Optionally, along the extension direction of the first surface of the positive current collector 11, the thickness of the second barrier layer 42 is 2 mm to 10 mm. For example, the second barrier layer 42 and the positive current collector 11 are respectively in the shape of long strips, and the second region 112 is arranged near the wide side of the first surface of the positive current collector 11. The second barrier layer 42 is arranged outside the wide side of the first surface of the positive current collector 11, the long side of the second barrier layer 42 coincides with the wide side of the positive current collector 11, and the wide side of the second barrier layer 42 extends along the extension line direction of the long side of the positive current collector 11, and the width of the second barrier layer 42 is 2 mm to 10 mm.
[0073] In this embodiment, the first barrier layer 41 can block the electron conduction between the positive electrode active material 12 corresponding to the first region 111 and the positive electrode current collector 11, thereby preventing the positive electrode active material 12 corresponding to the first region 111 from having lithium ions participating in the battery reaction. The second barrier layer 42 can effectively prevent the positive electrode tab 13 and the negative electrode tab 33 from overlapping and short-circuiting during the use of the battery.
[0074] In some specific embodiments of the present application, the barrier layer 40 and the positive electrode active material 12 are bonded. That is, during assembly, the barrier layer 40 and the positive electrode active material 12 can be connected and fixed by bonding. During bonding, the barrier layer 40 and the positive electrode active material 12 can be directly bonded, or an adhesive coating can be provided between the barrier layer 40 and the positive electrode active material 12 to achieve indirect bonding between the barrier layer 40 and the positive electrode active material 12.
[0075] In this embodiment, the barrier layer 40 and the positive electrode active material 12 are bonded together, so that during the preparation of the positive electrode plate 10, as well as in subsequent processes and battery use, the barrier layer 40 and the positive electrode active material 12 can be well positioned to avoid misalignment between the barrier layer 40 and the positive electrode active material 12.
[0076] According to an embodiment of the present application, the barrier layer 40 includes an adhesive. The adhesive in the barrier layer 40 is a hot-melt material. In other words, the adhesive in the barrier layer 40 is a material that has adhesiveness only after hot pressing.
[0077] Optionally, the positive electrode active material 12 includes a positive electrode material, a conductive agent, and a binder.
[0078] Optionally, the positive electrode active material 12 includes 90 to 98 parts by weight of a positive electrode material, 0.5 to 3 parts by weight of a conductive agent, and 0.5 to 3 parts by weight of a binder.
[0079] Optionally, the binder in the positive electrode active material 12 is polytetrafluoroethylene.
[0080] Optionally, the barrier layer 40 includes inorganic particles and a binder.
[0081] Optionally, the barrier layer 40 includes 1 to 98 parts by weight of inorganic particles and 2 to 99 parts by weight of a binder.
[0082] Optionally, the inorganic particles in the barrier layer 40 are at least one of aluminum oxide, boehmite, and silicon dioxide.
[0083] Optionally, the binder in the barrier layer 40 is polyvinylidene fluoride.
[0084] Optionally, the width of the barrier layer 40 is 2 mm to 12 mm along the extension direction of the first surface of the positive current collector 11. For example, the barrier layer 40 and the positive current collector 11 are respectively in the shape of long strips, the barrier layer 40 is arranged on the wide side of the first surface of the positive current collector 11, the long side of the barrier layer 40 coincides with the wide side of the positive current collector 11, the wide side of the barrier layer 40 extends along the long side of the positive current collector 11, and the width of the barrier layer 40 is 2 mm to 12 mm.
[0085] In this embodiment, a binder is added to the barrier layer 40, and the binder in the barrier layer 40 is a hot-melt material. That is, the binder in the barrier layer 40 can be molten after being heated and become sticky. During assembly, the positive electrode active material 12 and the barrier layer 40 can be bonded and fixed together by hot pressing.
[0086] In this embodiment, by using a binder that becomes sticky only when heated, the positive current collector 11, the positive active material 12 and the barrier layer 40 can maintain freedom when they are not assembled, which makes it easy to adjust the placement angles of the positive current collector 11, the positive active material 12 and the barrier layer 40, and is beneficial to adjust the alignment degree of the positive current collector 11, the positive active material 12 and the barrier layer 40.
[0087] Optionally, the negative electrode active material 32 includes a negative electrode material, a conductive agent, and a binder.
[0088] Optionally, the negative electrode active material 32 includes 90 to 98 parts by weight of a negative electrode material, 0.5 to 3 parts by weight of a conductive agent, and 0.5 to 3 parts by weight of a binder.
[0089] Optionally, the binder in the negative electrode active material 32 is polystyrene-butadiene rubber.
[0090] In some specific embodiments of the present application, the adhesive layer 50 includes an adhesive, and the adhesive of the adhesive layer 50 is a hot-melt material.
[0091] According to one embodiment of the present application, Figure 1 and Figure 2 As shown, the number of barrier layers 40 and adhesive layers 50 is respectively multiple, and the multiple barrier layers 40 correspond to the multiple adhesive layers 50 one by one. That is to say, each barrier layer 40 corresponds to one adhesive layer 50. By providing multiple adhesive layers 50, the installation firmness between the diaphragm 20, the positive electrode sheet 10 and the negative electrode sheet 30 can be improved, and the diaphragm 20, the positive electrode sheet 10 and the negative electrode sheet 30 can be prevented from shaking left and right or even dislocating during the subsequent process and the use of the battery, resulting in a short circuit.
[0092] By providing a barrier layer 40 corresponding to each adhesive layer 50 , it is possible to prevent lithium from being easily deposited at the position corresponding to each adhesive layer 50 on the negative electrode sheet 30 .
[0093] In some specific embodiments of the present application, Figure 1 and Figure 2As shown, a plurality of adhesive layers 50 are spaced apart and distributed. In this embodiment, by spaced apart and distributed on the separator 20 , the installation firmness between the separator 20 , the positive electrode sheet 10 and the negative electrode sheet 30 can be further improved.
[0094] According to one embodiment of the present application, the shape of the diaphragm 20 is a long strip, the number of adhesive layers 50 is two, the two adhesive layers 50 are spaced apart and distributed along the length direction of the diaphragm 20, and each adhesive layer 50 is located on the wide side of the diaphragm 20 and extends along the width direction of the diaphragm 20.
[0095] That is to say, the shape of the diaphragm 20 is a long strip, and the long strip has a long side and a wide side, the long side extends in the length direction, and the wide side extends in the width direction. There are two adhesive layers 50, and the two adhesive layers 50 are spaced apart in the length direction. Each adhesive layer 50 can be in the shape of a long strip and extend in the width direction. In addition, by fixing the two relatively arranged sides of the diaphragm 20 with two adhesive layers 50, the diaphragm 20 can be prevented from shaking back and forth, thereby improving the stability of the diaphragm 20. Since the two long sides of the diaphragm 20 are not provided with the adhesive layer 50, it is convenient to inject the electrolyte. It should be noted that the width dimension is smaller than the length dimension. When the adhesive layer 50 is provided on the wide side, the area of the adhesive layer 50 can be further reduced.
[0096] In this embodiment, by arranging two adhesive layers 50 on the wide sides of the diaphragm 20, the area of the adhesive layer 50 can be further reduced. When the size of the diaphragm 20 is fixed, the ratio of the area of the adhesive layer 50 to the area of the diaphragm 20 is reduced, and the area on the negative electrode plate 30 connected to the adhesive layer 50 is reduced, thereby reducing the range on the negative electrode plate 30 that is easy to deposit lithium.
[0097] Furthermore, if Figure 1 and Figure 2 As shown, the shape and position of the barrier layer 40 correspond to the adhesive layer 50. For example, when the separator 20 is in the shape of a long strip, the number of adhesive layers 50 is two and they are located at the wide side of the long strip. The shape of the positive electrode collector 11 is in the shape of a long strip, the number of barrier layers 40 is two, and the two barrier layers 40 are spaced apart and distributed along the length direction of the positive electrode collector 11. Each barrier layer 40 is located at the wide side of the positive electrode collector 11 and extends along the width direction of the positive electrode collector 11.
[0098] In this embodiment, by making the shapes and positions of the barrier layer 40 and the adhesive layer 50 correspond to each other, it is helpful to adjust the barrier layer 40 and the adhesive layer 50 to partially overlap or fully overlap during the assembly process.
[0099] According to one embodiment of the present application, the area on the diaphragm 20 where the adhesive layer 50 is not provided is spaced apart from the positive electrode sheet 10 and the negative electrode sheet 30, respectively, and the area on the diaphragm 20 where the adhesive layer 50 is provided is close to the edge of the diaphragm 20. In other words, the surface of the diaphragm 20 is defined with an area where the adhesive layer 50 is provided and an area where the adhesive layer 50 is not provided. The edge position of the diaphragm 20 is connected and fixed to the positive electrode sheet 10 and the negative electrode sheet 30 through the adhesive layer 50, and the middle part of the diaphragm 20 is spaced apart from the positive electrode sheet 10 and the negative electrode sheet 30, respectively.
[0100] In this embodiment, if Figure 1 and Figure 2 As shown, disposing the adhesive layer 50 at the edge of the separator 20 can not only reduce the area ratio of the adhesive layer 50 on the separator 20 , but also realize the positioning of the separator 20 , the positive electrode sheet 10 and the negative electrode sheet 30 .
[0101] In addition, when the positive active material 12 is coated on the positive current collector 11, the thickness of the positive active material 12 in different regions will be different due to the slurry flowing to both sides. The thickness of the positive active material 12 at the edge of the positive current collector 11 will be lower than the thickness of the positive active material 12 in the middle of the positive current collector 11. There is a difference between the edge thickness and the middle thickness, and uneven coating is prone to occur when the adhesive layer 50 is coated on the edge of the separator 20, affecting the bonding effect during pressing. Moreover, during the pressing and fixing process, due to the thickness difference between the edge thickness and the middle thickness, it is easy to cause failure of the bonding after pressing.
[0102] Since the edge position of the adhesive layer 50 corresponds to the edge position of the positive electrode active material 12, the present application can make the sum of the thickness H1 of the positive electrode active material 12 in the edge area of the separator 20 and the thickness H2 of the adhesive layer 50 approach the same as the thickness H3 of the positive electrode active material 12 in the middle of the positive electrode current collector 11 by setting the adhesive layer 50 in the edge area of the separator 20. In addition, in the process of preparing the laminated battery cell, the situation that the thickness of the edge of the positive electrode active material 12 is lower than the thickness in the middle of the positive electrode active material 12 can be solved, and the bonding strength between the positive electrode active material 12 and the separator 20 can be ensured.
[0103] Similarly, when the negative electrode active material 32 is coated on the negative electrode current collector 31, the thickness of the negative electrode active material 32 in different regions will also be different. By making the adhesive layer 50 correspond to the edge position of the negative electrode current collector 31, the failure of the adhesive after pressing due to the difference between the edge thickness and the middle thickness can be avoided, which will not be described in detail here.
[0104] It should be noted that the thickness here refers to the thickness along the direction from the positive electrode sheet 10 to the negative electrode sheet 30 .
[0105] In some specific embodiments of the present application, in the direction from the positive electrode sheet 10 to the negative electrode sheet 30 , the orthographic projection of the negative electrode active material 32 on the separator 20 covers the orthographic projection of the positive electrode active material 12 on the separator 20 .
[0106] That is to say, Figure 4 and Figure 7 As shown, the area of the negative electrode active material 32 is not less than the area of the positive electrode active material 12, and the positive electrode active material 12 does not exceed the edge area of the negative electrode active material 32. The length L1 of the negative electrode active material 32 is greater than or equal to the length L2 of the positive electrode active material 12. If part of the positive electrode active material 12 exceeds the negative electrode active material 32, then after the lithium ions of the positive electrode active material 12 in the exceeding area come out, lithium deposition will be formed because there is no negative electrode active material 32 on the opposite side.
[0107] Optionally, the adhesive layer 50 is selected from one or more of polyvinylidene fluoride, carboxymethyl cellulose, acrylonitrile multipolymer LA133, styrene-butadiene rubber, and acrylic resin. The adhesive layer 50 does not show adhesive properties at room temperature and pressure, but shows adhesive properties when heated and pressurized. During the processing of the laminated lithium-ion battery 100, the separator 20 can be bonded and fixed to the positive electrode sheet 10 and the negative electrode sheet 30 by heating and pressurizing.
[0108] Optionally, along the direction from the positive electrode sheet 10 to the negative electrode sheet 30 , the thickness of the adhesive layer 50 is 0.3 μm to 3 μm.
[0109] Optionally, the width of the adhesive layer 50 is 3 mm to 14 mm along the extension direction of the diaphragm 20. For example, the diaphragm 20 and the adhesive layer 50 are respectively in the shape of long strips, the adhesive layer 50 is arranged on the wide side of the diaphragm 20, the long side of the adhesive layer 50 coincides with the wide side of the diaphragm 20, the wide side of the adhesive layer 50 extends along the long side of the diaphragm 20, and the width of the adhesive layer 50 is 3 mm to 14 mm.
[0110] According to one embodiment of the present application, the area of the barrier layer 40 is not less than the area of the adhesive layer 50. In other words, the area of the barrier layer 40 is greater than or equal to the area of the adhesive layer 50. The position on the negative electrode sheet 30 connected to the adhesive layer 50 is prone to lithium deposition. Therefore, by ensuring that the adhesive layer 50 is provided at the position corresponding to the adhesive layer 50, lithium deposition on the negative electrode sheet 30 can be avoided to a large extent.
[0111] The stacked lithium-ion battery 100 according to the embodiment of the present application is described in detail below in conjunction with specific embodiments.
[0112] Example 1
[0113] The laminated lithium-ion battery 100 comprises a laminated battery cell, which comprises a positive electrode sheet 10 , a separator 20 and a negative electrode sheet 30 .
[0114] The positive electrode sheet 10 includes a positive current collector 11, a positive active material 12 coated on both surfaces of the positive current collector 11, and a barrier layer 40 coated between the positive current collector 11 and the positive active material 12. The barrier layer 40 is located at the edge of the positive current collector 11. The width of the barrier layer 40 is 2 mm to 12 mm. The two surfaces of one end of the positive current collector 11 are provided with a first blank area as a positive electrode tab 13.
[0115] The separator 20 includes a region where the adhesive layer 50 is not coated and a region where the adhesive layer 50 is coated.
[0116] The negative electrode sheet 30 includes a negative electrode current collector 31 and a negative electrode active material 32 coated on both surfaces of the negative electrode current collector 31. Two surfaces of one end of the negative electrode current collector 31 are provided with second blank areas as negative electrode tabs 33.
[0117] The positive electrode current collector 11 is made of aluminum foil, and the negative electrode current collector 31 is made of copper foil.
[0118] In parts by weight, the positive electrode active material 12 includes 96 parts by weight of positive electrode material, 2 parts by weight of conductive agent, and 2 parts by weight of binder, wherein the binder in the positive electrode active material 12 is polytetrafluoroethylene.
[0119] The barrier layer 40 mainly comprises 1 to 98 parts by weight of inorganic particles and 2 to 99 parts by weight of a binder, wherein the inorganic particles are at least one of alumina, boehmite, and silicon dioxide, and the binder in the barrier layer 40 is polyvinylidene fluoride.
[0120] The adhesive layer 50 is one or more of polyvinylidene fluoride, carboxymethyl cellulose, acrylonitrile multipolymer LA133, styrene-butadiene rubber, and acrylic resin. The adhesive layer 50 does not show adhesive properties at room temperature and pressure, but shows adhesive properties when heated and pressurized. The adhesive layer 50 can be bonded and fixed to the positive electrode sheet 10 and the negative electrode sheet 30.
[0121] In parts by weight, the negative electrode active material 32 includes 96 parts by weight of negative electrode material, 2 parts by weight of conductive agent, and 2 parts by weight of binder. The binder of the negative electrode active material 32 is polystyrene-butadiene rubber.
[0122] When preparing a laminated battery cell, the positive electrode sheet 10, the separator 20, and the negative electrode sheet 30 are sequentially laminated. The first blank area of the positive electrode sheet 10 and the second blank area of the negative electrode sheet 30 are arranged in opposite directions during lamination.
[0123] Then, the barrier layer 40 and the adhesive layer 50 are completely or partially overlapped. After hot pressing, the edge area of the positive electrode active material 12, the adhesive layer 50, and the edge area of the negative electrode active material 32 are bonded and fixed.
[0124] Example 2
[0125] The laminated lithium-ion battery 100 comprises a laminated battery cell, which comprises a positive electrode sheet 10 , a separator 20 and a negative electrode sheet 30 .
[0126] The positive electrode sheet 10 includes a positive current collector 11, a positive active material 12 coated on both surfaces of the positive current collector 11, and a barrier layer 40 coated between the positive current collector 11 and the positive active material 12. The barrier layer 40 is located at the edge of the positive current collector 11. The width of the barrier layer 40 is 2 mm to 20 mm. The two surfaces of one end of the positive current collector 11 are provided with a first blank area as a positive electrode tab 13.
[0127] The separator 20 includes a region where the adhesive layer 50 is not coated and a region where the adhesive layer 50 is coated.
[0128] The negative electrode sheet 30 includes a negative electrode current collector 31 and a negative electrode active material 32 coated on both surfaces of the negative electrode current collector 31. Two surfaces of one end of the negative electrode current collector 31 are provided with second blank areas as negative electrode tabs 33.
[0129] The positive electrode current collector 11 is made of aluminum foil, and the negative electrode current collector 31 is made of copper foil.
[0130] In parts by weight, the positive electrode active material 12 includes 96 parts by weight of positive electrode material, 2 parts by weight of conductive agent, and 2 parts by weight of binder, wherein the binder in the positive electrode active material 12 is polytetrafluoroethylene.
[0131] The barrier layer 40 mainly comprises 1 to 98 parts by weight of inorganic particles and 2 to 99 parts by weight of a binder, wherein the inorganic particles are at least one of alumina, boehmite, and silica, and the binder in the barrier layer 40 is polyvinylidene fluoride.
[0132] The barrier layer 40 includes a first barrier layer 41 and a second barrier layer 42. The first barrier layer 41 has a width of 2 mm to 12 mm and is located between the positive electrode active material 12 and the positive electrode current collector 11, and can be used to block the electron conduction between the positive electrode active material 12 and the positive electrode current collector 11 in the region, thereby preventing the lithium ions in the positive electrode active material 12 in the region from participating in the battery reaction, and can effectively prevent lithium deposition in the region corresponding to the bonding layer 50 on the negative electrode sheet 30 in the region.
[0133] The second barrier layer 42 is disposed in the first blank area of the positive electrode current collector 11 and is close to the positive electrode active material 12. The width of the second barrier layer 42 is 2 mm to 10 mm. By providing the second barrier layer 42, the positive electrode tab 13 and the negative electrode tab 33 can be effectively prevented from overlapping and short-circuiting during the use of the battery.
[0134] The adhesive layer 50 is one or more of polyvinylidene fluoride, carboxymethyl cellulose, acrylonitrile multipolymer LA133, styrene-butadiene rubber, and acrylic resin. The adhesive layer 50 does not show adhesive properties at room temperature and pressure, but shows adhesive properties when heated and pressurized. The adhesive layer 50 can be bonded and fixed to the positive electrode sheet 10 and the negative electrode sheet 30.
[0135] In parts by weight, the negative electrode active material 32 includes 96 parts by weight of negative electrode material, 2 parts by weight of conductive agent, and 2 parts by weight of binder. The binder of the negative electrode active material 32 is polystyrene-butadiene rubber.
[0136] When preparing a laminated battery cell, the positive electrode sheet 10, the separator 20, and the negative electrode sheet 30 are sequentially laminated. The first blank area of the positive electrode sheet 10 and the second blank area of the negative electrode sheet 30 are arranged in opposite directions during lamination.
[0137] Then, the barrier layer 40 and the adhesive layer 50 are completely or partially overlapped. After hot pressing, the edge area of the positive electrode active material 12, the adhesive layer 50, and the edge area of the negative electrode active material 32 are bonded and fixed.
[0138] In summary, according to the laminated lithium-ion battery 100 of the embodiment of the present application, by setting a barrier layer 40 in the positive electrode plate 10 and setting an adhesive layer 50 at the edge of the diaphragm 20, not only can lithium deposition on the negative electrode plate 30 be avoided, but also the bonding strength between the positive electrode plate 10, the diaphragm 20, and the negative electrode plate 30 during hot pressing can be ensured.
[0139] Although some specific embodiments of the present application have been described in detail by way of example, it should be understood by those skilled in the art that the above examples are only for illustration, not for limiting the scope of the present application. It should be understood by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present application. The scope of the present application is defined by the appended claims.
Claims
1. A laminated lithium-ion battery, characterized in that: include: A positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector, a barrier layer and a positive electrode active material, the positive electrode current collector having a first surface and a second surface arranged opposite to each other, the barrier layer and the positive electrode active material are respectively attached to a partial area of the first surface; the barrier layer is used to block electron transmission; Negative electrode; and A diaphragm is arranged between the positive electrode sheet and the negative electrode sheet, and adhesive layers are respectively arranged on both sides of the diaphragm; Among them, the area of the bonding layer is smaller than the area of the diaphragm, the positive electrode sheet and the negative electrode sheet are respectively connected to a part of the diaphragm through the bonding layer, the bonding layer and the barrier layer are arranged opposite to each other, and the area of the barrier layer is not smaller than the area of the bonding layer.
2. The laminated lithium-ion battery according to claim 1, characterized in that: The positive electrode active material covers at least a portion of the barrier layer.
3. The laminated lithium-ion battery according to claim 1, characterized in that: The positive electrode sheet includes a positive electrode tab, which is electrically connected to the positive electrode collector and is arranged adjacent to the barrier layer. The negative electrode sheet includes a negative electrode tab, and the positive electrode tab and the negative electrode tab are located on the same side of the diaphragm. A portion of the barrier layer extends to the surface of the positive electrode tab and is arranged opposite to the negative electrode tab.
4. The laminated lithium-ion battery according to claim 1, characterized in that: In the direction from the positive electrode sheet to the negative electrode sheet, the orthographic projection of the negative electrode active material of the negative electrode sheet on the separator covers the orthographic projection of the positive electrode active material on the separator.
5. The laminated lithium-ion battery according to claim 1, characterized in that: The barrier layer includes an adhesive, and the adhesive of the barrier layer is a hot-melt material.
6. The laminated lithium-ion battery according to claim 1, characterized in that: The adhesive layer includes an adhesive, and the adhesive of the adhesive layer is a hot-melt material.
7. The laminated lithium-ion battery according to claim 1, characterized in that: The number of the barrier layer and the number of the adhesive layer are respectively plural, and the plurality of barrier layers and the plurality of adhesive layers correspond one to one.
8. The laminated lithium-ion battery according to claim 7, characterized in that: The diaphragm is in the shape of a long strip, and the number of the adhesive layers is two. The two adhesive layers are spaced apart and distributed along the length direction of the diaphragm, and each adhesive layer is located at the wide side of the diaphragm and extends along the width direction of the diaphragm.
9. The laminated lithium-ion battery according to claim 1, characterized in that: The area on the diaphragm where no adhesive layer is provided is spaced apart from the positive electrode sheet and the negative electrode sheet, respectively, and the area on the diaphragm where the adhesive layer is provided is close to the edge of the diaphragm.