A kind of polybutylene succinate / terephthalate based thermoplastic polyester elastomer and preparation method thereof
Through the design of polybutylene succinic acid/terephthalate-based thermoplastic polyester elastomer, the problems of non-biodegradability and poor mechanical properties of existing thermoplastic polyester elastomers are solved, achieving low cost and good mechanical properties. thermoplastic polyester elastomer, expanding the scope of applications and reducing environmental pollution through green processes.
Patent Information
- Application Number
- CN202211530567.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-01
AI Technical Summary
Existing thermoplastic polyester elastomers are non-biodegradable because they contain highly crystalline terephthalate polyester hard segments and polyether soft segments, leading to environmental pollution, high cost, and poor mechanical properties, which limits their application scope.
Using polybutylene succinate/terephthalate-based thermoplastic polyester elastomer, it is synthesized through the chain extender block synthesis of prepolymer A and prepolymer B, and the benzene ring structure is designed to reduce costs and improve mechanical properties. , and adopts green and environmentally friendly esterification and polycondensation reaction to prepare biodegradable polymer materials.
A thermoplastic polyester elastomer with low cost and good mechanical properties has been realized, expanding its application range, reducing environmental pollution through green processes, and the material is biodegradable.
Smart Images

Figure BDA0003975656160000261 
Figure BDA0003975656160000271
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a poly(butylene succinate / terephthalate)-based thermoplastic polyester elastomer and a preparation method thereof. Background Art
[0002] Thermoplastic polyester elastomer is a block copolymer material containing a polyester hard segment and a polyester or polyether soft segment, in which the hard segment is generally a crystallizable rigid polymer with excellent properties such as high strength, high hardness and high temperature resistance, thereby providing the thermoplastic polyester elastomer with excellent mechanical properties and heat resistance; while the soft segment is generally a polymer with flexibility and low-temperature properties, which can provide the thermoplastic polyester elastomer with excellent toughness and low-temperature performance.
[0003] At present, most thermoplastic polyester elastomers are non-biodegradable materials because they contain high-crystallinity terephthalic acid polyester hard segments and polyether soft segments, and their waste pollutes the environment. Patent CN104497318B discloses an aliphatic biodegradable thermoplastic polyester elastomer and a preparation method thereof, wherein a bio-based aliphatic dibasic acid or anhydride, a linear diol is used to synthesize a crystalline polyester prepolymer with a terminal carboxyl or hydroxyl group, and a bio-based aliphatic dibasic acid or anhydride, a branched diol is used to synthesize an amorphous polyester prepolymer with a terminal hydroxyl or carboxyl group, and then the two polyester prepolymers are mixed together for polycondensation to obtain an aliphatic biodegradable thermoplastic polyester elastomer. This method uses bio-based raw materials to synthesize all-aliphatic thermoplastic polyester elastomers, which has high costs, low product molecular weight, and poor mechanical properties, limiting the scope of application of thermoplastic polyester elastomers. Summary of the invention
[0004] The invention provides a thermoplastic polyester elastomer based on poly(succinic acid) / butylene terephthalate) copolymer as a hard segment and highly flexible aliphatic polyester as a soft segment, which has low raw material cost, good mechanical properties, simple preparation method, biodegradability and low requirements on production equipment, and a preparation method thereof.
[0005] In order to achieve the above-mentioned object of the invention, the technical solution of the present invention is as follows:
[0006] A polybutylene succinate / terephthalate-based thermoplastic polyester elastomer, wherein the thermoplastic polyester elastomer is an AbB type polybutylene succinate / terephthalate-polyester block copolymer synthesized by prepolymer A and prepolymer B through block reaction with a chain extender;
[0007] The prepolymer A is a dihydroxy or carboxyl terminated poly(succinic acid / butylene terephthalate) hard segment prepolymer prepared by polymerization of 1,4-butanediol, succinic acid and terephthalic acid;
[0008] The succinic acid may also be succinic anhydride, dimethyl succinate or succinyl chloride;
[0009] The terephthalic acid may also be dimethyl terephthalate;
[0010] The prepolymer B is a highly flexible aliphatic polyester soft segment prepolymer with dihydroxyl or carboxyl end-capping, which is prepared by melt polycondensation using a variety of aliphatic diols and dibasic acids, acid anhydrides and / or acid chlorides as monomers.
[0011] Furthermore, the mass ratio of the prepolymer A to the prepolymer B is 1:1-1:19.
[0012] Furthermore, the ratio of the molar number of functional groups in the chain extender to the molar number of hydroxyl or carboxyl groups in the prepolymer is 1:1-1.3:1; preferably, the ratio of the molar number of functional groups in the chain extender to the molar number of hydroxyl or carboxyl groups in the prepolymer is 1:1-1.25:1.
[0013] Furthermore, the number average molecular weight of the prepolymer A is 1000-20000.
[0014] Furthermore, the diol is one of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,10-decanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, PEG-200, PEG-400, PEG-600, PPG-200, PPG-400, PPG-600, or a mixture thereof in any proportion.
[0015] Furthermore, the number average molecular weight of the aliphatic polyester soft segment prepolymer B is in the range of 1000-20000; the glass transition temperature of the prepolymer B is lower than -40°C; and the molecular structure of the aliphatic polyester prepolymer B is composed of more than 4 aliphatic polyester repeating structural units.
[0016] Furthermore, the dibasic acid, acid anhydride and / or acid chloride is any one of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid, tridecanedioic acid, pentadecanedicarboxylic acid, itaconic acid, fumaric acid, succinic anhydride, glutaric anhydride, adipic anhydride, itaconic anhydride, maleic anhydride, succinic dichloride, glutaric dichloride, adipic dichloride, itaconic acid chloride, or a mixture thereof in any proportion.
[0017] Further, the chain extender is hexamethylene diisocyanate (HDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), isophorone diisocyanate (IPDI), lysine diisocyanate (LDI), 2,4-toluene diisocyanate (TDI), 2,6-toluene diisocyanate, naphthalene diisocyanate (NDI), bis((3,4-epoxycyclohexyl)methyl) adipate, 1,6-hexanedioic acid diglycidyl ether, resorcinol diglycidyl ether, 1,3-benzenediol diglycidyl ether, The invention can be selected from the group consisting of hydroquinone formaldehyde tetraglycidyl ether, p-aminophenol epoxy resin, tetrahydrophthalate epoxy resin, 1,2-epoxycyclohexane 4,5-dicarboxylic acid epoxy resin, o-phthalate epoxy resin, isophthalate epoxy resin, p-terephthalate epoxy resin, endomethyl tetrahydrophthalate epoxy resin, p-hydroxybenzoic acid epoxy resin, bis(2,3-epoxycyclopentyl) ether, ethylene glycol diglycidyl ether, 2,2-bis(2-oxazoline) (BOZ), and 2,2-(1,3-phenylene)-bisoxazoline (PBO), or a mixture thereof in any proportion.
[0018] On the other hand, the present invention provides a method for preparing the polybutylene succinate / terephthalate based thermoplastic polyester elastomer as described above, comprising the following steps:
[0019] (1) Preparation of prepolymer A
[0020] 1,4-butanediol and terephthalic acid are mixed in a molar ratio of 0.8-3:1, stirred and a catalyst and an antioxidant are added, and an esterification or transesterification reaction is carried out at a temperature above 240° C. under nitrogen protection for 10-30 minutes, then the temperature is lowered to 190° C., 1,4-butanediol and succinic acid are added in a molar ratio of 0.8:1-3:1, stirred and a catalyst and an antioxidant are added again, esterification is carried out at 190-220° C. for 1-3 hours, then the temperature is raised to 230° C., and the reaction is carried out in a pressure range below 2 kPa for 1-2 hours, and then the temperature is raised to above 240° C. and the reaction is continued for 0.5-3 hours to obtain a dihydroxy or carboxyl-terminated polysuccinic acid / terephthalate prepolymer A;
[0021] Wherein, the succinic acid may also be succinic anhydride, dimethyl succinate or succinyl chloride; the terephthalic acid may also be dimethyl terephthalate;
[0022] (2) Preparation of prepolymer B
[0023] A plurality of aliphatic diols and dibasic acids are mixed at an alcohol-acid ratio of 1:1.05-1.5 or 1.05-1.5:1, a catalyst and an antioxidant and a stabilizer are added in an amount of 0.01-0.5% by weight of the monomers, the mixture is stirred under an inert atmosphere and the temperature is raised in stages to 130-180°C, the esterification reaction is carried out for 1-6 hours, an antioxidant is then added, the mixture is stirred and the temperature is raised to 200-240°C under a pressure range below 2 kPa, and the reaction is continued for 2-8 hours to obtain a dihydroxy or carboxyl terminated aliphatic polyester soft segment prepolymer B;
[0024] (3) Preparation of polybutylene succinate / terephthalate based thermoplastic polyester elastomer
[0025] The prepolymer A and prepolymer B obtained in the above steps are mixed, heated to 140-180°C, melt-mixed for 20-60 minutes under nitrogen protection, and then a chain extender is added for block copolymerization, reacted for 10-60 minutes, and then continued to react for 0.5-2 hours in a pressure range of a vacuum degree below 2 kPa, thereby preparing a polybutylene succinate / terephthalate based thermoplastic polyester elastomer.
[0026] Further, the catalyst is selected from sulfuric acid, trifluoromethanesulfonic acid, methyl trifluoromethanesulfonate, titanium dioxide, ethylene glycol titanium, acetylacetonate titanium, n-butyl titanate, isopropyl titanate, ethylene glycol antimony, antimony trioxide, antimony acetate, stannous octoate, stannous oxalate, dibutyltin oxide, dibutyltin dilaurate, butylstannic acid, lithium acetate, potassium acetate, calcium acetate, magnesium acetate, barium acetate, zinc acetate, cobalt acetate, antimony acetate, lead acetate, manganese acetate, triisopropoxyaluminum, zinc acetate, zinc oxide, stannous chloride, concentrated sulfuric acid, p-toluenesulfonic acid, magnesium acetate, zinc acetate, zinc chloride, lithium chloride, germanium chloride, tin tetrachloride, potassium carbonate, triethylenediamine, triethylamine, zinc lactate or a mixture thereof in any proportion;
[0027] Further, the antioxidant is selected from antioxidant 168, antioxidant 240, antioxidant 245, antioxidant 264, antioxidant 300, antioxidant 330, antioxidant 445, antioxidant 1010, antioxidant 1024, antioxidant 1035, antioxidant 1520, antioxidant 1076, antioxidant 1098, antioxidant 1330, antioxidant 1790, antioxidant 2246, antioxidant 3114 or a mixture thereof in any proportion;
[0028] Furthermore, the stabilizer is selected from one or more mixtures of phosphoric acid, phosphorous acid, hypophosphorous acid, pyrophosphoric acid, ammonium phosphate, dimethyl phosphate, trimethyl phosphate, diphenyl phosphate, triphenyl phosphate, diphenyl phosphite, triphenyl phosphite, triethyl phosphate, ammonium phosphite, diammonium phosphate, p-hydroxyanisole, hydroquinone, o-methylhydroquinone, p-benzoquinone or benzoquinone triphenyl phosphite.
[0029] Compared with the prior art, the present invention has the following positive and beneficial effects:
[0030] (1) The polybutylene succinate / terephthalate-based thermoplastic polyester elastomer prepared by the present invention introduces a benzene ring structure in the structural design of the crystalline hard segment and uses part of terephthalic acid to replace aliphatic dibasic acid, thereby reducing costs, improving mechanical strength, and expanding its application range.
[0031] (2) The present invention adopts a chain extension method to synthesize a poly(butylene succinate / terephthalate)-based thermoplastic polyester elastomer, which has a low chain extension reaction temperature, a short reaction time, saves energy, and is easy for industrial production.
[0032] (3) The polybutylene succinate / terephthalate-based thermoplastic polyester elastomer prepared by the present invention is a biodegradable green polymer material.
[0033] (4) The synthesis method of polybutylene succinate / terephthalate-based thermoplastic polyester elastomer adopts a green and environmentally friendly esterification condensation reaction, which does not contain any organic solvents and does not produce any waste water, waste gas, waste residue or other three wastes, and is safe and environmentally friendly. DETAILED DESCRIPTION
[0034] The present invention will be further described in detail below in conjunction with specific examples. The following examples are not intended to limit the present invention, but are only intended to illustrate the present invention. The experimental methods used in the following examples are generally conventional, unless otherwise specified, and the materials, reagents, etc. used in the following examples are commercially available, unless otherwise specified.
[0035] When the embodiment gives a numerical range, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs.
[0036] It is worth noting that the raw materials used in the present invention are all common commercially available products, so their sources are not specifically limited.
[0037] Example 1
[0038] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0039] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0040] 3. Add 2.00g of prepolymer A and 18.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add the chain extender hexamethylene diisocyanate (HDI), wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1 kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.9×10 4 .
[0041] Comparative Example 1
[0042] 1. Add 51.96g (0.4400mol) of succinic acid and 36.05g (0.4000mol) of 1,4-butanediol into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer, esterify at 160℃ for 2h, heat to 180℃, and when the water output reaches more than 90%, add 0.1760g (0.20%wt) of stannous chloride and 0.0880g (0.10%wt) of antioxidant 168, heat to 220℃ in 2h, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, continue the reaction for 3.5h, and finally obtain a carboxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography is 4.0×10 3 .
[0043] 2. Add 70.08 g (0.3500 mol) of sebacic acid, 19.21 g (0.1500 mol) of itaconic acid, and 41.86 g (0.5500 mol) of 1,2-propylene glycol into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. After the materials are completely melted at 130°C, add 0.3935 g (0.30% wt) of p-benzoquinone and esterify at 150°C for 3 h. Raise the temperature to 180℃, when the water output reaches more than 90%, 0.2623g (0.20%wt) of tetrabutyl titanate, 0.1314g (0.10%wt) of antioxidant 168 and 0.1314g (0.10%wt) of antioxidant 1010 are added, and the temperature is gradually raised to 220℃ within 2h. The pressure in the reactor gradually drops from one atmospheric pressure to 1kPa, and the reaction is continued for 4h to finally obtain hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography is 9.6×10 3 .
[0044] 3. 2.00 g of prepolymer A, 18.00 g of prepolymer B, 0.1000 g (0.50% wt) of p-toluenesulfonic acid, and 0.02 g (0.10% wt) of antioxidant 240 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and reacted at 180°C for 0.5 h. The temperature was gradually raised to 220°C within 2 h, and the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa. The reaction was continued for 1 h to obtain a polybutylene succinate-based thermoplastic polyester elastomer. The number average molecular weight was measured by gel permeation chromatography to be 4.8×10 4 .
[0045] Comparative Example 2
[0046] 1. 14.62 g (0.0880 mol) of terephthalic acid, 7.21 g (0.0800 mol) of 1,4-butanediol, 0.0218 g (0.10% wt) of stannous oxalate, 0.0109 g (0.05% wt) of antioxidant 168, and 0.0109 g (0.05% wt) of antioxidant 1010 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The reaction temperature was raised to 245°C and the reaction was carried out for 10 min under stirring and nitrogen atmosphere. The reaction temperature was quickly reduced to 190°C and the reaction temperature was increased. 93.53 g (0.7920 mol) of succinic acid, 64.89 g (0.7200 mol) of 1,4-butanediol, 0.1584 g (0.10% wt) of stannous oxalate, 0.0792 g (0.05% wt) of antioxidant 168 and 0.0792 g (0.05% wt) of antioxidant 1010 were added, and esterification was carried out at 190°C for 2 h. The temperature was gradually raised to 220°C within 2 h. The pressure in the reactor gradually dropped from one atmospheric pressure to below 1 kPa. The reaction was continued for 3.5 h, and finally a carboxyl-terminated prepolymer A was obtained. The number average molecular weight measured by gel permeation chromatography was 4.1×10 3 .
[0047] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. The reaction temperature was raised to 190°C in a reactor equipped with a device and a thermometer. The esterification reaction was carried out for 3 hours under stirring and nitrogen atmosphere. When the water output reached more than 90%, 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added. The reaction temperature was gradually raised to 220°C. The pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa. The reaction was continued for 4 hours to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 .
[0048] 3. 2.00 g of prepolymer A, 18.00 g of prepolymer B, 0.1000 g (0.50% wt) of p-toluenesulfonic acid, and 0.02 g (0.10% wt) of antioxidant 240 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and reacted at 180°C for 0.5 h. The temperature was gradually raised to 220°C within 2 h, and the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa. The reaction was continued for 1 h to obtain a polybutylene succinate / terephthalate-based thermoplastic polyester elastomer. The number average molecular weight was measured by gel permeation chromatography to be 5.6×10 4 .
[0049] Example 2
[0050] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0051] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0052] 3. Add 3.00g of prepolymer A and 17.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.8×10 4 .
[0053] Example 3
[0054] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0055] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0056] 3. Add 4.00g of prepolymer A and 16.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.6×10 4 .
[0057] Comparative Example 3
[0058] 1. Add 51.96g (0.4400mol) of succinic acid and 36.05g (0.4000mol) of 1,4-butanediol into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer, esterify at 160℃ for 2h, heat to 180℃, and when the water output reaches more than 90%, add 0.1760g (0.20%wt) of stannous chloride and 0.0880g (0.10%wt) of antioxidant 168, heat to 220℃ in 2h, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, continue the reaction for 3.5h, and finally obtain a carboxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography is 4.0×10 3 .
[0059] 2. Add 70.08 g (0.3500 mol) of sebacic acid, 19.21 g (0.1500 mol) of itaconic acid, and 41.86 g (0.5500 mol) of 1,2-propylene glycol into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. After the materials are completely melted at 130°C, add 0.3935 g (0.30% wt) of p-benzoquinone and esterify at 150°C for 3 h. Raise the temperature to 180℃, when the water output reaches more than 90%, 0.2623g (0.20%wt) of tetrabutyl titanate, 0.1314g (0.10%wt) of antioxidant 168 and 0.1314g (0.10%wt) of antioxidant 1010 are added, and the temperature is gradually raised to 220℃ within 2h. The pressure in the reactor gradually drops from one atmospheric pressure to 1kPa, and the reaction is continued for 4h to finally obtain hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography is 9.6×10 3 .
[0060] 3. 4.00 g of prepolymer A, 16.00 g of prepolymer B, 0.1000 g (0.50% wt) of p-toluenesulfonic acid, and 0.02 g (0.10% wt) of antioxidant 240 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and reacted at 180°C for 0.5 h. The temperature was gradually raised to 220°C within 2 h, and the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa. The reaction was continued for 1 h to obtain a polybutylene succinate-based thermoplastic polyester elastomer. The number average molecular weight was measured by gel permeation chromatography to be 4.6×10 4 .
[0061] Comparative Example 4
[0062] 1. 14.62 g (0.0880 mol) of terephthalic acid, 7.21 g (0.0800 mol) of 1,4-butanediol, 0.0218 g (0.10% wt) of stannous oxalate, 0.0109 g (0.05% wt) of antioxidant 168, and 0.0109 g (0.05% wt) of antioxidant 1010 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The reaction temperature was raised to 245°C and the reaction was carried out for 10 min under stirring and nitrogen atmosphere. The reaction temperature was quickly reduced to 190°C and the reaction temperature was increased. 93.53 g (0.7920 mol) of succinic acid, 64.89 g (0.7200 mol) of 1,4-butanediol, 0.1584 g (0.10% wt) of stannous oxalate, 0.0792 g (0.05% wt) of antioxidant 168 and 0.0792 g (0.05% wt) of antioxidant 1010 were added, and esterification was carried out at 190°C for 2 h. The temperature was gradually raised to 220°C within 2 h. The pressure in the reactor gradually dropped from one atmospheric pressure to below 1 kPa. The reaction was continued for 3.5 h, and finally a carboxyl-terminated prepolymer A was obtained. The number average molecular weight measured by gel permeation chromatography was 4.1×10 3 .
[0063] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. The reaction temperature was raised to 190°C in a reactor equipped with a device and a thermometer. The esterification reaction was carried out for 3 hours under stirring and nitrogen atmosphere. When the water output reached more than 90%, 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added. The reaction temperature was gradually raised to 220°C. The pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa. The reaction was continued for 4 hours to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 .
[0064] 3. 4.00 g of prepolymer A, 16.00 g of prepolymer B, 0.1000 g (0.50% wt) of p-toluenesulfonic acid, and 0.02 g (0.10% wt) of antioxidant 240 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and reacted at 180°C for 0.5 h. The temperature was gradually raised to 220°C within 2 h, and the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa. The reaction was continued for 1 h to obtain a polybutylene succinate / terephthalate-based thermoplastic polyester elastomer. The number average molecular weight was measured by gel permeation chromatography to be 5.3×10 4 .
[0065] Example 4
[0066] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0067] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0068] 3. Add 5.00g of prepolymer A and 15.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.4×10 4 .
[0069] Example 5
[0070] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0071] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0072] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.5×10 4 .
[0073] Comparative Example 5
[0074] 1. Add 51.96g (0.4400mol) of succinic acid and 36.05g (0.4000mol) of 1,4-butanediol into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer, esterify at 160℃ for 2h, heat to 180℃, and when the water output reaches more than 90%, add 0.1760g (0.20%wt) of stannous chloride and 0.0880g (0.10%wt) of antioxidant 168, heat to 220℃ in 2h, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, continue the reaction for 3.5h, and finally obtain a carboxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography is 4.0×10 3 .
[0075] 2. Add 70.08 g (0.3500 mol) of sebacic acid, 19.21 g (0.1500 mol) of itaconic acid, and 41.86 g (0.5500 mol) of 1,2-propylene glycol into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. After the materials are completely melted at 130°C, add 0.3935 g (0.30% wt) of p-benzoquinone and esterify at 150°C for 3 h. Raise the temperature to 180℃, when the water output reaches more than 90%, 0.2623g (0.20%wt) of tetrabutyl titanate, 0.1314g (0.10%wt) of antioxidant 168 and 0.1314g (0.10%wt) of antioxidant 1010 are added, and the temperature is gradually raised to 220℃ within 2h. The pressure in the reactor gradually drops from one atmospheric pressure to 1kPa, and the reaction is continued for 4h to finally obtain hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography is 9.6×10 3 .
[0076] 3. 6.00 g of prepolymer A, 14.00 g of prepolymer B, 0.1000 g (0.50% wt) of p-toluenesulfonic acid, and 0.02 g (0.10% wt) of antioxidant 240 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and reacted at 180°C for 0.5 h. The temperature was gradually raised to 220°C within 2 h, and the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa. The reaction was continued for 1 h to obtain a polybutylene succinate-based thermoplastic polyester elastomer. The number average molecular weight was measured by gel permeation chromatography to be 4.3×10 4 .
[0077] Comparative Example 6
[0078] 1. 14.62 g (0.0880 mol) of terephthalic acid, 7.21 g (0.0800 mol) of 1,4-butanediol, 0.0218 g (0.10% wt) of stannous oxalate, 0.0109 g (0.05% wt) of antioxidant 168, and 0.0109 g (0.05% wt) of antioxidant 1010 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The reaction temperature was raised to 245°C and the reaction was carried out for 10 min under stirring and nitrogen atmosphere. The reaction temperature was quickly reduced to 190°C and the reaction temperature was increased. 93.53 g (0.7920 mol) of succinic acid, 64.89 g (0.7200 mol) of 1,4-butanediol, 0.1584 g (0.10% wt) of stannous oxalate, 0.0792 g (0.05% wt) of antioxidant 168 and 0.0792 g (0.05% wt) of antioxidant 1010 were added, and esterification was carried out at 190°C for 2 h. The temperature was gradually raised to 220°C within 2 h. The pressure in the reactor gradually dropped from one atmospheric pressure to below 1 kPa. The reaction was continued for 3.5 h, and finally a carboxyl-terminated prepolymer A was obtained. The number average molecular weight measured by gel permeation chromatography was 4.1×10 3 .
[0079] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. The reaction temperature was raised to 190°C in a reactor equipped with a device and a thermometer. The esterification reaction was carried out for 3 hours under stirring and nitrogen atmosphere. When the water output reached more than 90%, 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added. The reaction temperature was gradually raised to 220°C. The pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa. The reaction was continued for 4 hours to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 .
[0080] 3. 6.00 g of prepolymer A, 14.00 g of prepolymer B, 0.1000 g (0.50% wt) of p-toluenesulfonic acid, and 0.02 g (0.10% wt) of antioxidant 240 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and reacted at 180°C for 0.5 h. The temperature was gradually raised to 220°C within 2 h, and the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa. The reaction was continued for 1 h to obtain a polybutylene succinate / terephthalate-based thermoplastic polyester elastomer. The number average molecular weight was measured by gel permeation chromatography to be 5.1×10 4 .
[0081] Example 6
[0082] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0083] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0084] 3. 7.00 g of prepolymer A and 13.00 g of prepolymer B were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt-mixed by mechanical stirring at a temperature of 160°C. When the two prepolymers were completely melted, a chain extender HDI was added, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers was 1.25:1. After 30 minutes of reaction, the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa, and the reaction was continued for 30 minutes to obtain a polybutylene succinate / terephthalate-based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography was 8.4×10 4 .
[0085] Example 7
[0086] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0087] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0088] 3. 8.00 g of prepolymer A and 12.00 g of prepolymer B were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt-mixed by mechanical stirring at a temperature of 160°C. When the two prepolymers were completely melted, a chain extender HDI was added, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers was 1.25:1. After 30 minutes of reaction, the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa, and the reaction was continued for 30 minutes to obtain a polybutylene succinate / terephthalate-based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography was 8.2×10 4 .
[0089] Comparative Example 7
[0090] 1. Add 51.96g (0.4400mol) of succinic acid and 36.05g (0.4000mol) of 1,4-butanediol into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer, esterify at 160℃ for 2h, heat to 180℃, and when the water output reaches more than 90%, add 0.1760g (0.20%wt) of stannous chloride and 0.0880g (0.10%wt) of antioxidant 168, heat to 220℃ in 2h, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, continue the reaction for 3.5h, and finally obtain a carboxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography is 4.0×10 3 .
[0091] 2. Add 70.08 g (0.3500 mol) of sebacic acid, 19.21 g (0.1500 mol) of itaconic acid, and 41.86 g (0.5500 mol) of 1,2-propylene glycol into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. After the materials are completely melted at 130°C, add 0.3935 g (0.30% wt) of p-benzoquinone and esterify at 150°C for 3 h. Raise the temperature to 180℃, when the water output reaches more than 90%, 0.2623g (0.20%wt) of tetrabutyl titanate, 0.1314g (0.10%wt) of antioxidant 168 and 0.1314g (0.10%wt) of antioxidant 1010 are added, and the temperature is gradually raised to 220℃ within 2h. The pressure in the reactor gradually drops from one atmospheric pressure to 1kPa, and the reaction is continued for 4h to finally obtain hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography is 9.6×10 3 .
[0092] 3. 8.00 g of prepolymer A, 12.00 g of prepolymer B, 0.1000 g (0.50% wt) of p-toluenesulfonic acid, and 0.02 g (0.10% wt) of antioxidant 240 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and reacted at 180°C for 0.5 h. The temperature was gradually raised to 220°C within 2 h, and the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa. The reaction was continued for 1 h to obtain a polybutylene succinate-based thermoplastic polyester elastomer. The number average molecular weight was measured by gel permeation chromatography to be 4.1×10 4 .
[0093] Comparative Example 8
[0094] 1. 14.62 g (0.0880 mol) of terephthalic acid, 7.21 g (0.0800 mol) of 1,4-butanediol, 0.0218 g (0.10% wt) of stannous oxalate, 0.0109 g (0.05% wt) of antioxidant 168, and 0.0109 g (0.05% wt) of antioxidant 1010 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The reaction temperature was raised to 245°C and the reaction was carried out for 10 min under stirring and nitrogen atmosphere. The reaction temperature was quickly reduced to 190°C and the reaction temperature was increased. 93.53 g (0.7920 mol) of succinic acid, 64.89 g (0.7200 mol) of 1,4-butanediol, 0.1584 g (0.10% wt) of stannous oxalate, 0.0792 g (0.05% wt) of antioxidant 168 and 0.0792 g (0.05% wt) of antioxidant 1010 were added, and esterification was carried out at 190°C for 2 h. The temperature was gradually raised to 220°C within 2 h. The pressure in the reactor gradually dropped from one atmospheric pressure to below 1 kPa. The reaction was continued for 3.5 h, and finally a carboxyl-terminated prepolymer A was obtained. The number average molecular weight measured by gel permeation chromatography was 4.1×10 3 .
[0095] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. The reaction temperature was raised to 190°C in a reactor equipped with a device and a thermometer. The esterification reaction was carried out for 3 hours under stirring and nitrogen atmosphere. When the water output reached more than 90%, 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added. The reaction temperature was gradually raised to 220°C. The pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa. The reaction was continued for 4 hours to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 .
[0096] 3. 8.00 g of prepolymer A, 12.00 g of prepolymer B, 0.1000 g (0.50% wt) of p-toluenesulfonic acid, and 0.02 g (0.10% wt) of antioxidant 240 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device, and reacted at 180°C for 0.5 h. The temperature was gradually raised to 220°C within 2 h, and the pressure in the reactor was gradually reduced from one atmosphere to 1 kPa. The reaction was continued for 1 h to obtain a polybutylene succinate / terephthalate-based thermoplastic polyester elastomer. The number average molecular weight was measured by gel permeation chromatography to be 4.9×10 4 .
[0097] Example 8
[0098] 1. 29.13 g (0.1500 mol) of dimethyl terephthalate, 14.87 g (0.1650 mol) of 1,4-butanediol, 0.0440 g (0.10% wt) of stannous oxalate, 0.0220 g (0.05% wt) of antioxidant 168, and 0.0220 g (0.05% wt) of antioxidant 1010 were added to a reactor filled with nitrogen and containing a mechanical stirring device and a thermometer. The reaction temperature was raised to 245°C and the reaction was carried out for 10 min under stirring and nitrogen atmosphere. The reaction temperature was quickly reduced to 190°C, and 70.85 g (0.600 0mol of succinic acid, 59.48g (0.6600mol) of 1,4-butanediol, 0.1303g (0.10%wt) of stannous oxalate, 0.0652g (0.05%wt) of antioxidant 168 and 0.0652g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain a hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.0×10 3 .
[0099] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0100] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.4×10 4 .
[0101] Example 9
[0102] 1. 43.69 g (0.2250 mol) of dimethyl terephthalate, 22.30 g (0.2475 mol) of 1,4-butanediol, 0.0660 g (0.10% wt) of stannous oxalate, 0.0330 g (0.05% wt) of antioxidant 168, and 0.0330 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 62 0.00g (0.5250mol) of succinic acid, 52.04g (0.5775mol) of 1,4-butanediol, 0.1140g (0.10%wt) of stannous oxalate, 0.0570g (0.05%wt) of antioxidant 168 and 0.0570g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 3.9×10 3 .
[0103] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0104] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.2×10 4 .
[0105] Example 10
[0106] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0107] 2. 48.75 g (0.4200 mol) of fumaric acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1551 g (0.05% wt) of antioxidant 168 and 0.1551 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3103g (0.10%wt) of stannous oxalate, 0.4654g (0.15%wt) of antioxidant 168 and 0.4654g (0.15%wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.6×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -57.2°C.
[0108] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.6×10 4 .
[0109] Embodiment 11
[0110] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0111] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 73.16 g (0.4200 mol) of suberic acid, 84.95 g (0.4200 mol) of sebacic acid, 46.88 g (0.6160 mol) of 1,3-propylene glycol, 55.51 g (0.6160 mol) of 1,4-butanediol, 72.80 g (0.6160 mol) of 1,6-hexanediol, 0.2221 g (0.05% wt) of antioxidant 168 and 0.2221 g (0.05% wt) of wt) of antioxidant 1010 was added to a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer, and the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was carried out for 3 hours under stirring and nitrogen atmosphere; then 0.4443g (0.10%wt) of stannous oxalate, 0.6664g (0.15%wt) of antioxidant 168 and 0.6664g (0.15%wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1kPa, and the reaction was carried out for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.5°C.
[0112] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.8×10 4 .
[0113] Example 12
[0114] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 2h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 6.6×10 3 .
[0115] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0116] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 9.5×10 4 .
[0117] Embodiment 13
[0118] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0119] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 6 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 1.4×10 4 The glass transition temperature of the product was measured by differential scanning calorimetry to be -54.7°C.
[0120] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 1.1×10 5 .
[0121] Embodiment 14
[0122] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 2h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 6.6×10 3 .
[0123] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 6 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 1.4×10 4 The glass transition temperature of the product was measured by differential scanning calorimetry to be -54.7°C.
[0124] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add chain extender HDI, wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 1.6×10 5 .
[0125] Embodiment 15
[0126] 1. 14.56 g (0.0750 mol) of dimethyl terephthalate, 7.43 g (0.0825 mol) of 1,4-butanediol, 0.0220 g (0.10% wt) of stannous oxalate, 0.0110 g (0.05% wt) of antioxidant 168, and 0.0110 g (0.05% wt) of antioxidant 1010 were added into a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was continued for 10 min under stirring and nitrogen atmosphere. The reaction temperature was rapidly reduced to 190°C and 79. 71g (0.6750mol) of succinic acid, 66.91g (0.7425mol) of 1,4-butanediol, 0.1466g (0.10%wt) of stannous oxalate, 0.0733g (0.05%wt) of antioxidant 168 and 0.0733g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain hydroxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.2×10 3 .
[0127] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 52.74 g (0.6930 mol) of 1,3-propylene glycol, 62.45 g (0.6930 mol) of 1,4-butanediol, 0.1556 g (0.05% wt) of antioxidant 168 and 0.1556 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, mechanically stirred flask. In a reactor equipped with a stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.3111 g (0.10% wt) of stannous oxalate, 0.4667 g (0.15% wt) of antioxidant 168 and 0.4667 g (0.15% wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a hydroxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.7×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -56.8°C.
[0128] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add the chain extender diphenylmethane diisocyanate (MDI), wherein the ratio of the molar number of isocyanate in the chain extender to the molar number of hydroxyl in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 9.0×10 4 .
[0129] Example 16
[0130] 1. 14.62 g (0.0880 mol) of terephthalic acid, 7.21 g (0.0800 mol) of 1,4-butanediol, 0.0218 g (0.10% wt) of stannous oxalate, 0.0109 g (0.05% wt) of antioxidant 168, and 0.0109 g (0.05% wt) of antioxidant 1010 were added to a reactor filled with nitrogen and equipped with a mechanical stirring device and a thermometer. The temperature was raised to 245°C and the reaction was carried out for 10 min under stirring and nitrogen atmosphere. The reaction temperature was quickly reduced to 190°C and 93.5 3g (0.7920mol) of succinic acid, 64.89g (0.7200mol) of 1,4-butanediol, 0.1584g (0.10%wt) of stannous oxalate, 0.0792g (0.05%wt) of antioxidant 168 and 0.0792g (0.05%wt) of antioxidant 1010 were reacted at 190-220°C for 3h; the reaction temperature was raised to 230°C, and the pressure in the reactor gradually dropped from one atmospheric pressure to below 1kPa for 2h; the temperature was raised to 245°C and reacted for 1h to finally obtain a carboxyl-terminated prepolymer A. The number average molecular weight measured by gel permeation chromatography was 4.1×10 3 .
[0131] 2. 49.60 g (0.4200 mol) of succinic acid, 61.38 g (0.4200 mol) of adipic acid, 84.95 g (0.4200 mol) of sebacic acid, 43.1487 g (0.5670 mol) of 1,3-propylene glycol, 51.0980 g (0.5670 mol) of 1,4-butanediol, 0.1451 g (0.05% wt) of antioxidant 168 and 0.1451 g (0.05% wt) of antioxidant 1010 were added to a nitrogen-filled, organic In a reactor equipped with a mechanical stirring device and a thermometer, the reaction temperature was gradually increased from 140°C to 190°C, and the reaction was continued for 3 hours under stirring and nitrogen atmosphere; then 0.2902g (0.1%wt) of stannous oxalate, 0.4353g (0.15%wt) of antioxidant 168 and 0.4353g (0.15%wt) of antioxidant 1010 were added, the reaction temperature was gradually increased to 220°C, the pressure in the reactor was gradually reduced from one atmospheric pressure to 1 kPa, and the reaction was continued for 4 hours under stirring conditions to finally obtain a carboxyl-terminated prepolymer B. The number average molecular weight measured by gel permeation chromatography was 9.4×10 3 The glass transition temperature of the product was measured by differential scanning calorimetry to be -58.1°C.
[0132] 3. Add 6.00g of prepolymer A and 14.00g of prepolymer B into a reactor filled with nitrogen and equipped with a mechanical stirring device, and melt mix them by mechanical stirring at a temperature of 160°C. When the two prepolymers are completely melted, add the chain extender di((3,4-epoxycyclohexyl)methyl) adipate, wherein the ratio of the molar number of epoxy groups in the chain extender to the molar number of carboxyl groups in the two prepolymers is 1.25:1. After reacting for 30 minutes, gradually reduce the pressure in the reactor from one atmosphere to 1kPa, and continue to react for 30 minutes to obtain a polybutylene succinate / terephthalate based thermoplastic polyester elastomer. The number average molecular weight measured by gel permeation chromatography is 8.6×10 4 .
[0133] Performance test: Molecular weight characterization by gel permeation chromatography (GPC)
[0134] The mechanical properties are tested according to GB / T528-2009 standard.
[0135] The biodegradability test was performed as follows: the sample was degraded in a lipase solution at 37°C for 15 days and the sample mass loss rate (degradation rate, %) was calculated. The lipase solution was prepared by dissolving a certain mass of lipase (200,000 U / g) in 250 ml of a mixed phosphate solution (0.025 M) with a pH value of 6.86 to prepare a lipase solution with a concentration of 5 mg / ml.
[0136] The specific test results are shown in Table 1 below.
[0137] Table 1. Properties of polybutylene succinate / terephthalate based thermoplastic polyester elastomers
[0138]
[0139]
[0140] It can be concluded from Examples 1 to 7 that different tensile strengths, elongations at break, hardness and degradation performance of polybutylene succinate-based thermoplastic polyester elastomers can be obtained by adjusting the ratio of soft and hard segments. It can be concluded from Examples 5, 8 and 9 that different types of polybutylene succinate-based thermoplastic polyester elastomers can be obtained by changing the ratio of reactive monomers in prepolymer A, and then different types of polybutylene succinate-based thermoplastic polyester elastomers can be synthesized. It can be concluded from Examples 10 and 11 that different molecular structures of prepolymers B can be obtained by changing the types of monomers, and then different types of polybutylene succinate-based thermoplastic polyester elastomers can be synthesized. It can be concluded from Examples 5, 12, 13, and 14 that by changing the reaction time of the soft and hard segments, different molecular weight soft and hard segments and different molecular weight polybutylene succinate / terephthalate based thermoplastic polyester elastomers can be obtained, thereby affecting the tensile strength, elongation at break, hardness, and degradation performance of the polybutylene succinate / terephthalate based thermoplastic polyester elastomers. It can be concluded from Examples 5, 15, and 16 that by changing the component ratio, hydroxyl or carboxyl terminated hard and soft segment prepolymers can be designed, and the corresponding polybutylene succinate / terephthalate based thermoplastic polyester elastomers can be obtained by using hydroxyl chain extenders or carboxyl chain extenders. It can be concluded from Examples 1 to 16 and Comparative Examples 1 to 8 that for the same soft and hard segment ratio, the polybutylene succinate / terephthalate based thermoplastic polyester elastomer prepared by the present invention has a higher molecular weight and more excellent mechanical properties. The various properties of the polysuccinic acid / butylene terephthalate based thermoplastic polyester elastomer prepared by the invention can be adjusted, and the tensile strength thereof is 8.5-34.7 MPa, the elongation at break is 723-1972%, the hardness is 65.1-92.5 HA, and the degradation rate in 15 days is 51.4-86.5%. In addition, the polysuccinic acid / butylene terephthalate based thermoplastic polyester elastomer also has excellent resilience, and the 100% tensile recovery rate is 90.5-96.2%.
[0141] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A polybutylene succinate / terephthalate based thermoplastic polyester elastomer, characterized in that: The thermoplastic polyester elastomer is an AbB type polybutylene succinate / terephthalate-polyester block copolymer synthesized by prepolymer A and prepolymer B via chain extender block reaction; The prepolymer A is a dihydroxy or carboxyl terminated poly(succinic acid / terephthalic acid) hard segment prepolymer prepared by polymerization of 1,4-butanediol, succinic acid and terephthalic acid; The succinic acid may also be succinic anhydride, dimethyl succinate or succinyl chloride; The terephthalic acid may also be dimethyl terephthalate; The prepolymer B is a highly flexible aliphatic polyester soft segment prepolymer terminated with dihydroxyl or carboxyl groups, which is prepared by melt polycondensation using a variety of aliphatic diols and dibasic acids, acid anhydrides and / or acid chlorides as monomers; The number average molecular weight of the highly flexible aliphatic polyester soft segment prepolymer B is in the range of 1000-20000; the glass transition temperature of the prepolymer B is lower than -40°C; the molecular structure of the prepolymer B is composed of more than 4 aliphatic polyester repeating structural units; The method for preparing the polybutylene succinate / terephthalate-based thermoplastic polyester elastomer specifically comprises the following steps: (1) Preparation of prepolymer A Mix 1,4-butanediol and terephthalic acid in a molar ratio of 0.8-3:1, stir and add a catalyst and an antioxidant, perform esterification or transesterification reaction at a temperature above 240° C. under nitrogen protection for 10-30 minutes, then cool to 190° C., add 1,4-butanediol and succinic acid in a molar ratio of 0.8-3:1, stir and add a catalyst and an antioxidant again, perform esterification at 190-220° C. for 1-3 hours, then heat to 230° C., react for 1-2 hours within a pressure range below 2 kPa, then heat to above 240° C., continue to react for 0.5-3 hours, and obtain a dihydroxy or carboxyl terminated polysuccinic acid / terephthalate prepolymer A; Wherein, the succinic acid may also be succinic anhydride, dimethyl succinate or succinyl chloride; the terephthalic acid may also be dimethyl terephthalate; (2) Preparation of prepolymer B A plurality of aliphatic diols and dibasic acids are mixed at an alcohol-acid ratio of 1:1.05-1.5 or 1.05-1.5:1, a catalyst and an antioxidant and a stabilizer are added in an amount of 0.01-0.5% by weight of the monomers, the mixture is stirred under an inert atmosphere and the temperature is raised in stages to 130-180°C, the esterification reaction is carried out for 1-6 hours, and then an antioxidant is added, the mixture is stirred and the temperature is raised to 200-240°C under a pressure range below 2 kPa, and the reaction is continued for 2-8 hours to obtain a dihydroxy or carboxyl terminated aliphatic polyester soft segment prepolymer B; (3) Preparation of polybutylene succinate / terephthalate based thermoplastic polyester elastomer The prepolymer A and prepolymer B obtained in the above step are mixed, heated to 140-180° C., melt-mixed for 20-60 min under nitrogen protection, and then a chain extender is added for block copolymerization, reacted for 10-60 min, and then continued to react for 0.5-2 h in a pressure range of a vacuum degree of less than 2 kPa, thereby preparing a polybutylene succinate / terephthalate-based thermoplastic polyester elastomer; The mass ratio of the prepolymer A to the prepolymer B is 1:1-1:19; The ratio of the molar number of the functional groups in the chain extender to the molar number of the hydroxyl groups or carboxyl groups in the two prepolymers is 1:1-1.3:
1.
2. The thermoplastic polyester elastomer according to claim 1, characterized in that The number average molecular weight of the prepolymer A is 1000-20000.
3. The thermoplastic polyester elastomer according to claim 1, characterized in that The diol is one of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,10-decanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, PEG-200, PEG-400, PEG-600, PPG-200, PPG-400, PPG-600 or a mixture thereof in any proportion.
4. The thermoplastic polyester elastomer according to claim 1, characterized in that The dibasic acid, acid anhydride and / or acid chloride is any one of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid, tridecanedioic acid, pentadecanedicarboxylic acid, itaconic acid, fumaric acid, succinic anhydride, glutaric anhydride, adipic anhydride, itaconic anhydride, maleic anhydride, succinic dichloride, glutaric dichloride, adipic dichloride, itaconic acid chloride, or a mixture thereof in any proportion.
5. The thermoplastic polyester elastomer according to claim 1, characterized in that The chain extender is hexamethylene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, isophorone diisocyanate, lysine diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, naphthalene diisocyanate, bis((3,4-epoxycyclohexyl)methyl) adipate, 1,6-adipic acid diglycidyl ether, resorcinol diglycidyl ether, resorcinol formaldehyde tetraglycidyl ether, p-aminophenol epoxy resin, tetra Hydrogenated phthalate epoxy resin, 1,2-epoxycyclohexane 4,5-dicarboxylic acid epoxy resin, phthalate epoxy resin, isophthalate epoxy resin, terephthalate epoxy resin, endomethylene tetrahydrophthalate epoxy resin, p-hydroxybenzoic acid epoxy resin, bis(2,3-epoxycyclopentyl) ether, ethylene glycol diglycidyl ether, 2,2-bis(2-oxazoline), 2,2-(1,3-phenylene)-bisoxazoline or a mixture thereof in any proportion.
6. The thermoplastic polyester elastomer according to claim 1, characterized in that The catalyst is selected from trifluoromethanesulfonic acid, methyl trifluoromethanesulfonate, titanium dioxide, titanium glycolate, titanium acetylacetonate, n-butyl titanate, isopropyl titanate, antimony glycolate, antimony trioxide, stannous octoate, stannous oxalate, dibutyltin oxide, dibutyltin dilaurate, butylstannic acid, lithium acetate, potassium acetate, calcium acetate, magnesium acetate, barium acetate, zinc acetate, cobalt acetate, antimony acetate, lead acetate, manganese acetate, triisopropoxyaluminum, zinc oxide, stannous chloride, concentrated sulfuric acid, p-toluenesulfonic acid, zinc chloride, lithium chloride, germanium chloride, tin tetrachloride, potassium carbonate, triethylenediamine, triethylamine, zinc lactate or a mixture thereof in any proportion; The antioxidant is selected from the group consisting of antioxidant 168, antioxidant 240, antioxidant 245, antioxidant 264, antioxidant 300, antioxidant 330, antioxidant 445, antioxidant 1010, antioxidant 1024, antioxidant 1035, antioxidant 1520, antioxidant 1076, antioxidant 1098, antioxidant 1330, antioxidant 1790, antioxidant 2246, and antioxidant 3114, or a mixture thereof in any proportion; The stabilizer is selected from one or more mixtures of phosphoric acid, phosphorous acid, hypophosphorous acid, pyrophosphoric acid, ammonium phosphate, dimethyl phosphate, trimethyl phosphate, diphenyl phosphate, triphenyl phosphate, diphenyl phosphite, triphenyl phosphite, triethyl phosphate, ammonium phosphite, diammonium phosphate, p-hydroxyanisole, hydroquinone, o-methylhydroquinone, p-benzoquinone or benzoquinone triphenyl phosphite.