A bone repair composition and its preparation method and application

By using exosomes derived from adipose mesenchymal stem cells and polydopamine and gelatin sponge composite materials, the problem of poor bioactivity and biocompatibility of existing bone graft materials is solved, effective repair of bone defects is achieved, and seed cells are avoided. risk, significantly improving bone tissue formation and biocompatibility.

CN115957378BActive Publication Date: 2024-10-22RUIJIN HOSPITAL AFFILIATED TO SHANGHAI JIAO TONG UNIV SCHOOL OF MEDICINE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310083650.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-08
Publication Date
2024-10-22
Estimated Expiration
2043-02-08

AI Technical Summary

Technical Problem

Existing bone graft replacement materials have poor bioactivity and biocompatibility, and the use of seed cells has low survival rate, immune rejection and tumor formation risks, which limits their application and fails to effectively utilize the potential of exosomes in the field of bone repair.

Method used

Develop a bone repair composition that utilizes the biological functions of exosomes to promote bone repair through adipose mesenchymal stem cell-derived exosomes and polydopamine and gelatin sponge composites (GS-PDA-Exos), avoiding direct use risk of seeding cells and growth factors, and improving the adhesion and biocompatibility of the material through a polydopamine coating.

Benefits of technology

The composition significantly improves cell survival rate and bone tissue formation in bone defect repair, avoids the risk of seed cells, has the advantages of good biocompatibility and easy storage and transportation, and promotes the bone healing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115957378B_ABST
    Figure CN115957378B_ABST
Patent Text Reader

Abstract

The present invention provides a bone repair composition and a preparation method and application thereof, wherein the preparation method comprises soaking GS in a weak alkaline dopamine solution until it turns dark brown, then taking out the material, repeatedly soaking and rinsing it in deionized water, and vacuum drying it to obtain GS-PDA, then soaking GS-PDA in an ADSCs-Exos solution, and repeatedly soaking and rinsing it in deionized water to obtain GS-PDA-Exos. The present invention can react secondary with carboxyl groups carried by various biomolecules, drugs, etc., so as to achieve the purpose of modifying the surface of the material again, and has the advantages of good biocompatibility, easy storage, transportation, and preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of medical bone repair and relates to a bone repair composition and a preparation method thereof. Background Art

[0002] Bone defects are structurally incomplete diseases of the bone caused by various diseases such as trauma, which seriously endanger the life and health of patients. Bone transplantation is still the preferred method for clinical treatment of bone defects. Due to various limitations of autologous bone transplantation and allogeneic bone transplantation, it is very important to develop new artificial bone transplantation materials.

[0003] There are still many shortcomings in the existing bone transplant substitute materials, including poor bioactivity and biocompatibility of repair materials. Mesenchymal stem cells (MSCs) play an important role in the field of bone tissue engineering and regenerative medicine because they have the ability to promote the repair and regeneration of damaged tissues. Although bone tissue engineering materials using "seed cells" have many advantages, with the deepening of research, materials using "seed cells" also show many disadvantages, such as low cell survival rate, decreased cell autoreplication and differentiation ability, prolonged time, the possibility of immune rejection reaction in the body, and the potential risk of tumor formation of MSCs. In addition, technical problems such as seed cell processing, storage, and transportation also limit the application of seed cells. With the deepening of research, researchers have found that the paracrine effect of mesenchymal stem cells plays an important role in tissue repair. Among them, exosomes (Exos) have become the focus of research as an important component of cell paracrine. Exos is a lipid-encapsulated vesicle released to the outside of the cell after binding to the cell membrane by multivesicular bodies (MVBs). It has rich contents, including lipids, proteins, mRNAs, microRNAs, etc. Various cells in the body can secrete exosomes, and the contents of Exos are not completely consistent depending on the cell source and microenvironment. It has been found that Exos have many biological functions, including participating in intercellular signal transmission, material transport, metabolism, etc. Exos secreted outside the cell can locally regulate surrounding cells or enter the blood to reach other parts of the body to participate in long-distance regulation. If Exos can be used in the field of bone repair, the various risks brought by the direct use of seed cells, cells and growth factors can be avoided.

[0004] However, there is no technology in the prior art that can apply exosomes to bone repair. The poor bioactivity and biocompatibility of current artificial materials for bone repair need to be addressed urgently. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a bone repair composition and its preparation method and application, and constructs a new exosome / polydopamine / gelatin sponge composite material (GS-PDA-Exos) derived from adipose mesenchymal stem cells, which provides a new option for the treatment of bone defects. Exosomes (Exos) are easier to store, transport, and prepare than existing artificial bone repair materials; gelatin sponge (GS) prepared by hydrolysis of animal collagen provides good biocompatibility and biodegradability for bone repair materials; the strong adhesion of the polydopamine (PDA) coating can adhere to the surface of a variety of materials, and the surface of the material can be modified secondary.

[0006] Specifically, on the one hand, the present invention provides a method for preparing a bone repair composition, the preparation method being: GS (gelatin sponge) is soaked in a weakly alkaline solution of dopamine (DA) until it becomes dark brown, then the material is taken out, repeatedly soaked and rinsed with deionized water, and vacuum dried to obtain GS-PDA (gelatin sponge / polydopamine), then the GS-PDA is soaked in an ADSCs-Exos solution, and repeatedly soaked and rinsed with deionized water to obtain GS-PDA-Exos (exosomes / polydopamine / gelatin sponge composite material).

[0007] Specifically, the GS of the present invention has a porous structure with a pore size of 100 μm-300 μm and a smooth fiber surface.

[0008] Preferably, the method for preparing the ADSCs-Exos solution of the present invention is as follows: taking out capillaries from the lipoaspirate, washing and mincing with a phosphate buffer solution, digesting with collagenase at low temperature, filtering the digested material, centrifuging the mixture at room temperature, and discarding the supernatant; washing the collected cells with PBS, resuspending them in a DMEM / F12 medium containing fetal bovine serum and penicillin-streptomycin after centrifugation, and culturing them in a CO2 atmosphere; after the cells have been passaged for 3 generations, obtaining the required serum-free cell culture medium containing adipose mesenchymal stem cells;

[0009] Exosomes derived from ADSCs were purified from serum-free cell culture medium by serial centrifugation and filtration steps.

[0010] Furthermore, the present invention centrifuges the collected serum-free cell culture medium supernatant containing adipose-derived mesenchymal stem cells at 300 g for 10 minutes to remove dead cells and at 5000 g for 10 minutes to remove cell debris, then filters the supernatant through a 0.22 μm filter and centrifuges at 120,000 g for 90 minutes, and resuspends the final pellet in 1 mL of PBS and stores at -80°C for future use.

[0011] Specifically, the gelatin sponge of the present invention is immersed in a 2 mg / mL dopamine solution with a pH of 8.5, and incubated at 37° C. for 24 hours with shaking to form a polydopamine-coated GS-PDA. The GS-PDA is gently shaken 5 times in an ultrasonic cleaner filled with distilled water, dried and sterilized with ethylene oxide, and then the GS-PDA is placed in a 5 mg / mL lecithin, 1 mg / mL phospholipid and 10 mg / L coral powder solution and incubated overnight. The obtained product is then placed in an ADSCs-Exos solution and shaken at 37° C. for 12 hours to obtain a GS-PDA-Exos scaffold. The GS-PDA-Exos scaffold is gently shaken 5 times in an ultrasonic cleaner filled with distilled water to obtain the bone repair composition.

[0012] More specifically, the dopamine solution of the present invention is prepared by dissolving dopamine in 10 ml of Tris-HCl to obtain a buffer solution with a pH of 8.5.

[0013] On the other hand, the present invention also provides a bone repair composition, wherein the scaffold of the bone repair composition is a gelatin sponge, a polydopamine coating is provided on the gelatin sponge, and exosomes derived from adipose mesenchymal stem cells are provided on the polydopamine coating.

[0014] Specifically, each bone repair composition of the present invention contains 10 10 Adipose-derived mesenchymal stem cells-derived exosomes.

[0015] In a third aspect, the bone repair composition of the present invention can promote bone repair in combination with other drugs.

[0016] A fourth aspect is the use of the bone repair composition in the preparation of bone repair devices.

[0017] Beneficial effects of the present invention:

[0018] The mesenchymal stem cell-derived Exos used in the present invention play an important role in the repair of various tissues such as bones, lungs, liver, kidneys, and skin. Exos can promote the osteogenic differentiation of human BMSCs. Exos derived from MSCs repair bone defects by promoting the formation of blood vessels and bone tissue, and Exos derived from BMSCs play an important role in the healing process of fractures.

[0019] The use of Exos in the present invention avoids various risks caused by directly using seed cells, cells and growth factors, and Exos also has the advantages of easy storage, transportation, preparation and the like.

[0020] The present invention uses 10 10 During the attachment and aggregation of exosome particles, exosomes of this magnitude can effectively promote bone tissue repair.

[0021] The polydopamine coating PDA of the present invention can be modified on the surface of almost all organic and inorganic substrates, and has very good biocompatibility. It can also be modified again. A large number of amino groups will remain in the formation process of the PDA coating. These amino groups can undergo secondary reactions with carboxyl groups carried by various biological molecules, drugs, etc., thereby achieving the purpose of modifying the material surface again.

[0022] The filling material of the invention has good biocompatibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a morphological diagram of the GS-PDA-Exos composition of the present invention;

[0024] Figure 2 This is a surface morphology diagram of the material observed by scanning electron microscope of the present invention;

[0025] Figure 3 Micro-CT2D reconstruction of the present invention shows the healing status of bone defects in each group;

[0026] Figure 4 Micro-CT3D reconstruction of the present invention shows the healing status of bone defects in each group;

[0027] Figure 5 The BMD amount in the ROI area of ​​each group of 3D models in Example 6 of the present invention;

[0028] Figure 6 The BV / TV content in the ROI area of ​​each group of 3D models in Example 6 of the present invention;

[0029] Figure 7 The amount of Tb.Th in the ROI area of ​​each group of 3D models in Example 6 of the present invention;

[0030] Figure 8 The Tb and Sp values ​​in the ROI area of ​​each group of 3D models in the sixth embodiment of the present invention;

[0031] Fig. 9 Hematoxylin-eosin (HE) staining was used to observe the tissue healing of the bone defect site in Example 6 of the present invention;

[0032] Fig.10 This is the release of Exos from the GS-PDA-EXO material in Example 3 of the present invention;

[0033] Fig.11 This is the observation of P0 and P3 generation ADSCs under an optical microscope in Example 5 of the present invention;

[0034] Fig.12 This is the observation of ADSCsExos by NTA instrument in Example 5 of the present invention.

[0035] Figure 2 In the figure, A and B are the surface morphology images of the material observed by GS scanning electron microscope, C and D are the surface morphology images of the material observed by GS-PDA scanning electron microscope, and E and F are the surface morphology images of the material observed by GS-PDA-Exos scanning electron microscope;

[0036] Figure 3 In the figure, A, B, C, and D show the healing of the bone defect at two weeks, and E, F, G, and H show the healing of the bone defect at four weeks;

[0037] Figure 4 In the figure, A, B, C, and D show the healing status of the bone defect site after two weeks, and E, F, G, and H show the healing status of the bone defect site after four weeks. DETAILED DESCRIPTION

[0038] Below, the present application is further described in conjunction with the accompanying drawings and specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.

[0039] Unless otherwise specified, the materials, instruments and methods used in the following embodiments are conventional materials, instruments and methods in the art and can be obtained through commercial channels.

[0040] Example 1: Preparation of adipose-derived mesenchymal stem cell-derived exosomes / polydopamine / gelatin sponge (GS-PDA-Exos)

[0041] As the instruction manual Figure 1 As shown:

[0042] GS has a milky white porous structure. After being soaked in a weak alkaline dopamine solution for 24 hours, GS gradually changes from milky white to dark brown in the solution, and the dark brown gradually deepens as the soaking time increases. Until the material completely turns dark brown, the material is taken out, rinsed with deionized water repeatedly for 5 times, and vacuum dried to obtain GS-PDA. Then it is soaked in an ADSCs-Exos solution, and GS-PDA-Exos is obtained after being soaked and rinsed with deionized water repeatedly for 5 times.

[0043] Example 2: Construction of exosome / polydopamine / gelatin sponge composition derived from adipose-derived mesenchymal stem cells

[0044] The gelatin sponge was soaked in 10 ml of 2 mg / mL, pH 8.5 dopamine (DA) solution prepared with Tris-HCl buffer solution and incubated at 37°C for 24 hours with shaking to form a polydopamine (PDA) coating. The gelatin sponge / polydopamine (GS-PDA) scaffold was gently shaken 5 times in an ultrasonic cleaner filled with distilled water. The GS-PDA scaffold was dried and sterilized with ethylene oxide. The GS-PDA scaffold was then placed in an ADSCs-Exos solution (10 10 The GS-PDA-Exos scaffold was gently shaken 5 times in an ultrasonic cleaner filled with distilled water to obtain the composition of the present invention.

[0045] Example 3: Construction of exosome / polydopamine / gelatin sponge composition derived from adipose-derived mesenchymal stem cells

[0046] The difference from Example 2 is that each GS-PDA bracket is placed in a 8 Each GS-PDA scaffold was placed in an ADSCs-Exos solution containing exosome particles or in a solution containing 10 11 Exosome particles in ADSCs-Exos solution. 10 8 Combined with the decrease in the number of exosomes, there is no effect on promoting bone formation. 11 The above may lead to excessive results and complications.

[0047] As the instruction manual Fig.10 As shown, the number of Exos particles in the infiltration solution at different times was calculated by ELISA. The results showed that the release of Exos gradually increased within 12 hours at a high rate. After 72 hours, the GS-PDA-Exos material continued to release Exos particles until 168 hours, when Exos continued to be released, but the rate slowed down.

[0048] Example 4: Construction of exosome / polydopamine / gelatin sponge composition derived from adipose-derived mesenchymal stem cells

[0049] The sterilized GS-PDA from Example 2 was placed in a solution of 5 mg / mL lecithin, 1 mg / mL phospholipids and 10 mg / L coral powder and incubated overnight. The obtained product was then placed in ADSCs-Exos (10 10 The GS-PDA-Exos scaffold was gently shaken 5 times in an ultrasonic cleaner filled with distilled water to obtain the bone repair composition.

[0050] Through the detection of the grafting rate of dopamine, the grafting rate of dopamine in Example 4 of the present invention was 81%, and the grafting rate of dopamine that was not incubated overnight in the 5 mg / mL lecithin, 1 mg / mL phospholipid and 10 mg / L coral powder solution was 35%. For the dopamine that was not treated with the 5 mg / mL lecithin, 1 mg / mL phospholipid and 10 mg / L coral powder solution, each GS-PDA scaffold was placed in a 10 11 The grafting rate of exosome particles in ADSCs-Exos solution was 37%. Each GS-PDA scaffold was placed on a 10 8 The grafting rate of exosome particles in the ADSCs-Exos solution was 25%.

[0051] Example 5: Extraction of exosomes from adipose-derived mesenchymal stem cells of the present invention

[0052] Adipose mesenchymal stem cells (ADSCs) extraction: Capillaries were removed from lipoaspirates, rinsed and minced with phosphate buffered solution, and digested with 1% collagenase at 37°C for 1 hour. After filtration, the mixture was centrifuged at room temperature (1000rpm, 10 minutes), and the supernatant was discarded. The collected cells were washed with PBS, centrifuged (1000rpm, 5 minutes), and then resuspended in DMEM / F12 medium (PS) containing 10% fetal bovine serum and 1% penicillin-streptomycin and cultured at 37°C, 5% CO2; when the cells were passed through 3 generations, they were identified and used for subsequent use.

[0053] Extraction of exosomes from adipose-derived mesenchymal stem cells: Exosomes derived from ADSCs were purified from serum-free cell culture media by a series of centrifugation and filtration steps. Specifically, the collected supernatant was centrifuged at 300g for 10 minutes to remove dead cells and at 5000g for 10 minutes to remove cell debris. The supernatant was then filtered through a 0.22μm filter and centrifuged at 120,000g for 90 minutes, and the final pellet was resuspended in 1mL PBS and stored at -80°C.

[0054] As the instruction manual Fig.12 As shown, according to the nanoparticle tracking analysis of Exos, A: the diameter of ADSCs-Exos is mainly distributed between 80-180nm, with a peak value of 122.1nm; B: Visual observation of Exos particles shows ADSCs-Exos particles in the liquid.

[0055] Example 6: Animal Experiment

[0056] Surgical modeling process:

[0057] After the experimental animals were weighed, 2.5% sodium pentobarbital (40 mg / kg) was injected intraperitoneally. After anesthesia, they were fixed in a supine position, and the left hind limb knee joint was dehaired and disinfected. A longitudinal incision was made on the medial side of the knee joint, and the distal femur was exposed. A 3.0 mm diameter drill was used to slowly drill along the central level of the medial condyle of the knee joint, in a direction perpendicular to the longitudinal axis of the femur, to create a 3.0 mm diameter bone defect tunnel that penetrated the medial and lateral condyles. During the drilling process, ice saline was used to continuously rinse and cool. Subsequently, a large amount of saline was repeatedly rinsed with bone defect tunnels, and GS materials, GSPDA materials, and GS-PDA-Exos materials were implanted according to the grouping. No material was implanted in the control group. The incision was closed layer by layer using a 3-0 absorbable front. After the operation, the experimental animals in each group were housed in separate cages, given normal feed and drinking water every day, and the growth, activity, and incision of the animals were observed. At 2 weeks and 4 weeks after surgery, three experimental animals were randomly selected from each group and killed under anesthesia to observe whether the surgical incision had healed and whether there were any signs of infection such as redness, swelling, and ulceration. Subsequently, the femur specimens of the left hind limb were collected, the soft tissue was peeled off, and the growth of the bone defect area was observed.

[0058] Micro-CT detection of bone defect healing:

[0059] The distal 1 / 2 of the femoral specimen was cut off and fixed in 4% paraformaldehyde for 48 hours, and then the specimen was taken out.

[0060] Placed in a Micro-CT detection tube, fixed with cotton balls around. Scan the specimen area with Micro-CT at a resolution of 12μm. Mimics17.0 was used for data analysis, 3D reconstruction and selection of a 3mm diameter bone defect area as the region of interest (ROI). Parameters such as bone mineral density (BMD), trabecular thickness (Tb.Th), trabecular separation / spacing (Tb,Sp), and bone volume fraction (BV / TV) were counted and analyzed.

[0061] Hematoxylin-eosin (HE) staining of specimens was used to observe the tissue healing at the bone defect site:

[0062] (1) Rinse the distal 1 / 2 femur specimen fixed in 4% paraformaldehyde for 48 hours with running water.

[0063] (2) The cells were then placed in 10% EDTA decalcification solution for 2 weeks, and the decalcification solution was replaced every other day.

[0064] (3) Place the specimen in running water and rinse overnight to wash away any residual EDTA.

[0065] (4) Dehydration with gradient alcohol, clearing with xylene, and then embedding in paraffin.

[0066] (5) Serial sections were made along the sagittal plane of the femur with a thickness of 5 μm.

[0067] (6) Dewax the paraffin wax by immersing it in xylene for 5 times for 10 min each.

[0068] (7) Place in absolute ethanol I and II for 5 min each, 95% ethanol I and II for 5 min each, 80% ethanol for 5 min, 70% ethanol for 5 min, and distilled water for 3 min for hydration.

[0069] (8) For hematoxylin staining, place the sections in Harris hematoxylin solution for 5 min, wash with water, and use 0.5% hydrochloric acid alcohol solution for color separation for 3-5 s. Observe under a microscope and wash with water for 5-10 min until fully blued.

[0070] (9) For eosin staining, the sections were placed in 95% ethanol eosin solution for 3–30 seconds, then immersed in 95% ethanol I and II, and anhydrous ethanol I and II for 5 minutes each, and then transparentized in xylene twice for 1 minute each.

[0071] (10) Seal the slides with neutral gum.

[0072] Result analysis:

[0073] A rat femoral bone defect model was constructed and the scaffolds were implanted into the defect to compare the effects of different materials on local repair of bone defects. Samples were collected at 2 weeks and 4 weeks and Micro-CT scans were performed. The area with a bone defect diameter of 3 mm was set as the ROI, and the new bone in the ROI was observed through 2D and 3D reconstruction. Figure 3 and attached Figure 4 As shown in the figure, only a small amount of new bone appeared in the peripheral area of ​​the ROI in the CON group at 2 weeks, while some new bone appeared in the peripheral area of ​​the ROI in the GS and GS-PDA groups. A small amount of new bone tissue appeared in the central area of ​​the ROI in the GS-PDA-Exos group, and some new bone appeared in the periphery of the defect. At 4 weeks, some new bone appeared in the periphery of the ROI in the CON group, but there was still an obvious defect in the ROI area, which indicates that the size of the constructed femoral defect exceeded the self-healing ability of the bone tissue itself. Figure 3 and attached Figure 4 As can be seen from F and G, a small amount of loose new bone tissue was seen inside the ROI of the GS and GS-PDA groups, and only some areas were defective. A large amount of new bone was seen inside the ROI of the GS-PDA-Exos group, with a large amount of bone and a relatively compact structure.

[0074] like Figure 5-8 As shown, in this embodiment, by calculating the BMD, BV / TV, Tb.Th, Tb,Sp in each group of 3D model ROI area, it can be seen that the CON group has the smallest BMD, BV / TV, and Tb.Th at 2w and 4w, while Tb,Sp is the largest. The BMD, BV / TV, and Tb.Th of the GS, GS-PDA, and GS-PDA-Exos groups are significantly higher than those of the CON group at the same time point, and Tb,Sp is lower than that of the CON group. Among them, the BMD, BV / TV, and Tb.Th of the GS-PDA-Exos group at each time point are the highest, and Tb,Sp is the lowest. This shows that the filling of GS and GS-PDA materials contributes to the repair of bone defects, and the GS-PDA-Exos material connected to ADSCs-Exos can significantly promote the repair of bone defects.

[0075] like Fig. 9 As shown in Figure 2, the experimental animals were killed 4 weeks after surgery, and the samples were taken for HE staining. The results showed that some new bone appeared outside the defect area in the CON group, but there was no obvious bone inside, only a small amount of fibrous tissue, which indicated that the size of the bone defect exceeded its normal repair capacity and the bone defect could not heal on its own (e.g. Fig. 9 In the defect area of ​​both GS and GS-PDA groups, some new bone was observed, the bone structure was relatively loose, the bone mass was small, and some residual material fibers were observed (e.g. Fig. 9 In the B and C of the GS-PDA-Exos group, a large amount of new bone was observed in the defect area, and the new bone was tightly surrounded by a small amount of residual GS-PDA-Exos material inside, indicating that GS-PDA-Exos material has a significant ability to promote new bone formation.

[0076] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a bone repair composition, characterized in that: The preparation method comprises the following steps: GS is soaked in a weak alkaline dopamine solution until it turns dark brown, then the material is taken out, repeatedly soaked and rinsed in deionized water, and vacuum dried to obtain GS-PDA, then the GS-PDA is soaked in an ADSCs-Exos solution, and repeatedly soaked and rinsed in deionized water to obtain GS-PDA-Exos; The gelatin sponge is immersed in a 2 mg / mL dopamine solution with a pH of 8.5, and incubated at 37° C. for 24 hours with shaking to form GS-PDA. The GS-PDA is gently shaken 5 times in an ultrasonic cleaner filled with distilled water, dried and sterilized with ethylene oxide, and then the GS-PDA is placed in a 5 mg / mL lecithin, 1 mg / mL phospholipid and 10 mg / L coral powder solution and incubated overnight. The obtained product is then placed in an ADSCs-Exos solution and shaken at 37° C. for 12 hours to obtain a GS-PDA-Exos scaffold. The GS-PDA-Exos scaffold is gently shaken 5 times in an ultrasonic cleaner filled with distilled water to obtain the bone repair composition. The ADSCs-Exos solution preparation method is as follows: taking out capillaries from fat aspirates, washing and mincing them with a phosphate buffer solution, digesting them with collagenase at low temperature, filtering the digested substances, centrifuging the mixture at room temperature, and discarding the supernatant; washing the collected cells with PBS, resuspending them in a DMEM / F12 culture medium containing fetal bovine serum and penicillin-streptomycin after centrifugation, and culturing them in a CO2 atmosphere; when the cells are passed through three generations, the required serum-free cell culture medium containing adipose mesenchymal stem cells is obtained; Exosomes derived from ADSCs were purified from serum-free cell culture medium by serial centrifugation and filtration steps.

2. The method for preparing the bone repair composition according to claim 1, characterized in that: The GS has a porous structure with a pore size of 100 μm-300 μm and a smooth fiber surface.

3. The method for preparing the bone repair composition according to claim 1, characterized in that: The collected serum-free cell culture medium supernatant containing adipose-derived mesenchymal stem cells was centrifuged at 300 g for 10 minutes to remove dead cells and at 5000 g for 10 minutes to remove cell debris, and then the supernatant was filtered through a 0.22 μm filter and centrifuged at 120,000 g for 90 minutes, and the final pellet was resuspended in 1 mL of PBS and stored at -80°C for future use.

4. The method for preparing the bone repair composition according to claim 1, characterized in that: The dopamine solution is prepared by dissolving dopamine in 10 ml of Tris-HCl to obtain a buffer solution with a pH of 8.

5.

5. A bone repair composition prepared by the method for preparing a bone repair composition according to any one of claims 1 to 4, wherein the bone repair composition scaffold is a gelatin sponge, a polydopamine coating is provided on the gelatin sponge, and exosomes derived from adipose mesenchymal stem cells are provided on the polydopamine coating.

6. The bone repair composition according to claim 5, characterized in that: Each bone repair composition contains 10 10 Adipose-derived mesenchymal stem cells-derived exosomes.

7. Use of the bone repair composition prepared by the method for preparing a bone repair composition according to any one of claims 1 to 4 in preparing bone repair drugs.

8. Use of the bone repair composition prepared by the method for preparing a bone repair composition according to any one of claims 1 to 4 in preparing a bone repair device.