Worm-like expanded graphite and preparation method thereof, sodium ion battery negative electrode, sodium ion battery and electrical equipment

The preparation method of worm-shaped expanded graphite solves the problem of limited electrochemical performance of graphite materials in sodium-ion batteries and achieves efficient and stable sodium-ion battery performance, which is suitable for large-scale development.

CN115974073BActive Publication Date: 2024-10-18GUANGZHOU GREAT POWER ENERGY & TECH CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211599456.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-10-18
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

In existing sodium-ion batteries, graphite as an anode material has limited electrochemical properties and is difficult to meet the needs of high specific capacity, high first efficiency and high stability. The preparation process is complex, making it difficult to achieve large-scale production.

Method used

The preparation method of worm-like expanded graphite is adopted, through vacuum heat treatment and oxidation treatment of strong oxidant and strong acid solution, combined with heating reaction and hydrogen peroxide reaction, followed by pickling and high-temperature heat treatment, to form worm-like expanded graphite with a three-dimensional network cross-linked structure , as anode material for sodium-ion batteries.

Benefits of technology

It achieves efficient and stable cycle performance and excellent rate performance in sodium-ion batteries. It has high first Coulombic efficiency, high specific capacity and high stability, and is suitable for large-scale development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115974073B_ABST
    Figure CN115974073B_ABST
Patent Text Reader

Abstract

The present application provides a worm-like expanded graphite and a preparation method thereof, a sodium ion battery negative electrode, a sodium ion battery and electrical equipment, and relates to the field of sodium ion batteries. The preparation method of worm-like expanded graphite comprises: subjecting natural graphite to vacuum heat treatment, and then mixing it with a strong oxidant strong acid solution for oxidation treatment; mixing the mixed solution obtained by oxidation treatment with water, and then heating the reaction; mixing the system with hydrogen peroxide for reaction; subjecting the reaction system to solid-liquid separation, acid washing and drying of the solid, and then subjecting the solid to high-temperature heat treatment under a protective atmosphere to obtain worm-like expanded graphite. The worm-like expanded graphite is prepared using the above-mentioned preparation method. The sodium ion battery negative electrode, the raw material of which includes worm-like expanded graphite. The sodium ion battery includes a sodium ion battery negative electrode. Electrical equipment includes a sodium ion battery. The worm-like expanded graphite provided in the present application can achieve efficient and stable circulation in a sodium ion battery, and exhibits excellent rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of sodium ion batteries, and in particular to a worm-like expanded graphite and a preparation method thereof, a sodium ion battery negative electrode, a sodium ion battery and electrical equipment. Background Art

[0002] As one of the alternatives to lithium-ion batteries, sodium-ion batteries have attracted much attention due to their abundant sources, low cost, and similar performance to lithium-ion batteries. However, due to the large radius of sodium ions, their slow kinetics and huge barriers make it very difficult for sodium ions to be embedded in electrodes. Therefore, it is a challenge to find a suitable regulator to achieve a reversible sodium-deoxygenation process. Carbonaceous materials have attracted great attention due to their stability, accessibility, and abundance. As a typical negative electrode material for lithium-ion batteries, graphite has extremely limited electrochemical performance in sodium ion storage. Therefore, scientists have tried to obtain other carbonaceous materials with large interlayers or amorphous structures, including soft carbon, hard carbon, graphene, etc. However, among electrode materials, how to develop negative electrode materials with high specific capacity, high initial efficiency, and high stability on a large scale is still a key scientific issue facing sodium-ion batteries. Among all carbonaceous materials, expanded graphite has attracted much attention because it has a large carbon interlayer interlayer, which is conducive to the insertion and deinsertion of sodium ions. According to previous reports, there have been some studies in the field of sodium ions based on expanded negative electrodes. Despite these works, the storage performance of sodium ions still cannot meet current needs. In addition, the corresponding technical conditions are complex, and large-scale production cannot be achieved in the large-scale sodium-ion battery industry.

[0003] Therefore, it is very necessary to further develop expanded graphite for high-performance sodium-ion batteries with simple and feasible preparation scheme, high first coulombic efficiency, high and stable electrochemical performance. Summary of the invention

[0004] The purpose of the present application is to provide a worm-like expanded graphite and a preparation method thereof, a sodium ion battery negative electrode, a sodium ion battery and electrical equipment to solve the above-mentioned problems.

[0005] To achieve the above objectives, this application adopts the following technical solutions:

[0006] A method for preparing worm-like expanded graphite, comprising:

[0007] The natural graphite is subjected to vacuum heat treatment and then mixed with a strong oxidant strong acid solution for oxidation treatment;

[0008] The mixed solution obtained by the oxidation treatment is mixed with water, and then heated for reaction; after the heating reaction is completed, the system is mixed with hydrogen peroxide for reaction;

[0009] The reaction system is subjected to solid-liquid separation, the solid is acid-washed and dried, and then subjected to high-temperature heat treatment under a protective atmosphere to obtain the worm-like expanded graphite.

[0010] Preferably, the vacuum heat treatment is performed at a temperature of 100-200°C and for a time of 5-24 hours;

[0011] Preferably, the vacuum heat treatment is carried out at a temperature of 150° C. and for a time of 12 hours.

[0012] Preferably, the solute in the strong oxidant strong acid solution includes one or more of potassium permanganate, potassium dichromate, potassium perchlorate, sodium perchlorate, potassium persulfate, potassium nitrate, and sodium nitrate;

[0013] Preferably, the solutes in the strong oxidant strong acid solution are potassium permanganate and sodium nitrate, and the mass ratio of the potassium permanganate to the sodium nitrate is 1:(0.5-2);

[0014] Preferably, the solution in the strong oxidant strong acid solution includes concentrated sulfuric acid and / or concentrated nitric acid, and the mass ratio of the solute to the solution in the strong oxidant strong acid solution is 1:(15-25);

[0015] Preferably, the solution in the strong oxidant strong acid solution is concentrated sulfuric acid, and the mass ratio of the solute to the solution in the strong oxidant strong acid solution is 1:20.

[0016] Preferably, the mass ratio of the natural graphite to the solute in the strong oxidant strong acid solution is 1:(0.5-3), preferably 1:1;

[0017] Preferably, during the process of mixing the natural graphite after vacuum heat treatment with the strong oxidant strong acid solution, the system temperature does not exceed 20°C;

[0018] Preferably, the oxidation treatment temperature is 30-50°C and the time is 1-10h;

[0019] Preferably, the oxidation treatment is carried out at a temperature of 35° C. and for a time of 4 hours.

[0020] Preferably, during the mixing process of the mixed solution and water, the system temperature does not exceed 40°C;

[0021] Preferably, the mass ratio of the mixed solution to water is 1:(3-8), and during the mixing process, the rate of adding water is 2-20 mL / min;

[0022] Preferably, the mass ratio of the mixed solution to water is 1:4, and the rate of adding water is 5 mL / min;

[0023] Preferably, the heating reaction temperature is 80-100°C and the time is 0.5-5h;

[0024] Preferably, the heating reaction is carried out at a temperature of 90° C. and for a time of 1 hour.

[0025] Preferably, the acid solution used for pickling includes at least one of hydrochloric acid, sulfuric acid, nitric acid and acetic acid, and the concentration of the acid solution is 0.5-3 mol / L;

[0026] Preferably, the acid solution used in the pickling is hydrochloric acid with a concentration of 1 mol / L;

[0027] Preferably, the drying temperature is 60-150°C and the drying time is 5-24h;

[0028] Preferably, the gas in the protective atmosphere includes one or more of nitrogen, argon, carbon dioxide, and hydrogen, and the gas flow rate is 50-200 mL / min;

[0029] Preferably, the temperature of the high temperature heat treatment is 600-1200°C, and the heating rate is 5-20°C / min;

[0030] Preferably, the gas in the protective atmosphere is nitrogen, the gas flow rate is 100 mL / min, the temperature of the high-temperature heat treatment is 800° C., and the heating rate is 10° C. / min.

[0031] The present application also provides a worm-like expanded graphite, which is prepared using the preparation method of the worm-like expanded graphite.

[0032] The present application also provides a sodium ion battery negative electrode, the raw materials of which include the worm-like expanded graphite and a binder;

[0033] Preferably, the binder includes one or more of polyvinylidene fluoride, sodium carboxymethyl cellulose, sodium alginate, and polystyrene rubber;

[0034] Preferably, the mass ratio of the worm-like expanded graphite to the binder is (2-10):100, preferably 10:100;

[0035] Preferably, the current collector material of the negative electrode of the sodium ion battery is selected from any one of pure copper foil, carbon-coated copper foil, pure aluminum foil, carbon-coated aluminum foil and stainless steel foil.

[0036] The present application also provides a sodium ion battery, comprising the sodium ion battery negative electrode;

[0037] Preferably, the method for preparing the sodium ion battery comprises:

[0038] The worm-like expanded graphite and the binder are mixed to obtain a slurry, which is then coated on a current collector and dried to obtain a negative electrode of a lithium-ion battery, and then assembled under an argon atmosphere using a sodium-ion electrolyte to obtain a sodium-ion battery;

[0039] Preferably, in the argon atmosphere, the oxygen content is less than 1 ppm and the water content is less than 1 ppm;

[0040] Preferably, the sodium salt in the sodium electrolyte includes one or more of sodium hexafluorophosphate, sodium perchlorate, and sodium trifluoromethanesulfonate;

[0041] Preferably, the concentration of sodium salt in the sodium-electrolyte electrolyte is 0.5-2 mol / L.

[0042] The present application also provides an electrical device, including the sodium ion battery.

[0043] Compared with the prior art, the beneficial effects of this application include:

[0044] The preparation method of worm-like expanded graphite provided in the present application comprises the following steps: using a strong oxidant and an auxiliary strong acid to oxidize natural graphite, and then performing a heating reaction and a reaction with hydrogen peroxide after oxidation, and then performing a high-temperature thermal reduction treatment under an inert atmosphere after acid washing and drying; utilizing the oxygen escape process during the oxidation of natural graphite and the pyrolysis process to cause the interlayer spacing of graphite to expand, thereby realizing the rapid preparation of three-dimensional worm-like expanded graphite.

[0045] The worm-like expanded graphite provided in the present application is three-dimensional worm-like and has a network cross-linked structure. The flakes of the expanded graphite material directly constitute a large number of electron conduction networks, thereby achieving efficient and stable circulation in sodium ion batteries and exhibiting excellent rate performance. The worm-like expanded graphite has high first coulombic efficiency, high specific capacity, high stability and has prospects for large-scale development.

[0046] The sodium ion battery negative electrode, sodium ion battery and electrical equipment provided in this application have excellent electrical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0048] Figure 1 This is a scanning electron microscope schematic diagram of expanded graphite in Example 1;

[0049] Figure 2 This is a transmission electron microscope schematic diagram of expanded graphite in Example 1;

[0050] Figure 3is the cycle curve of the expanded graphite in Example 1 at a current density of 100 mA / g;

[0051] Figure 4 is the long cycle curve of expanded graphite in Example 1 at a current density of 1 A / g-1;

[0052] Figure 5 is the cycle curve of the expanded graphite in Example 2 at a current density of 100 mA / g;

[0053] Figure 6 is the long cycle curve of expanded graphite in Example 2 at a current density of 1 A / g;

[0054] Figure 7 is the cycle curve of the expanded graphite in Example 3 at a current density of 100 mA / g;

[0055] Figure 8 This is the cycle curve of the expanded graphite in Example 4 at a current density of 100 mA / g. DETAILED DESCRIPTION

[0056] As used herein:

[0057] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0058] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0059] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0060] In these examples, parts and percentages are by mass unless otherwise indicated.

[0061] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.

[0062] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0063] A method for preparing worm-like expanded graphite, comprising:

[0064] The natural graphite is subjected to vacuum heat treatment and then mixed with a strong oxidant strong acid solution for oxidation treatment;

[0065] The mixed solution obtained by the oxidation treatment is mixed with water, and then heated for reaction; after the heating reaction is completed, the system is mixed with hydrogen peroxide for reaction;

[0066] The reaction system is subjected to solid-liquid separation, the solid is acid-washed and dried, and then subjected to high-temperature heat treatment under a protective atmosphere to obtain the worm-like expanded graphite.

[0067] In an optional embodiment, the vacuum heat treatment is performed at a temperature of 100-200° C. for a time of 5-24 hours;

[0068] In an optional embodiment, the vacuum heat treatment is carried out at a temperature of 150° C. and for a time of 12 hours.

[0069] Optionally, the temperature of the vacuum heat treatment can be 100°C, 150°C, 200°C or any value between 100-200°C, and the time can be 5h, 6h, 12h, 18h, 24h or any value between 5-24h.

[0070] In an optional embodiment, the solute in the strong oxidant strong acid solution includes one or more of potassium permanganate, potassium dichromate, potassium perchlorate, sodium perchlorate, potassium persulfate, potassium nitrate, and sodium nitrate;

[0071] In an optional embodiment, the solutes in the strong oxidant strong acid solution are potassium permanganate and sodium nitrate, and the mass ratio of the potassium permanganate to the sodium nitrate is 1:(0.5-2);

[0072] Optionally, the mass ratio of the potassium permanganate to the sodium nitrate may be 1:0.5, 1:1, 1:1.5, 1:2 or any value between 1:(0.5-2).

[0073] In an optional embodiment, the solution in the strong oxidant strong acid solution includes concentrated sulfuric acid and / or concentrated nitric acid, and the mass ratio of the solute to the solution in the strong oxidant strong acid solution is 1:(15-25);

[0074] Optionally, the mass ratio of solute to solution in the strong oxidant strong acid solution can be 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, 1:21, 1:22, 1:23, 1:24, 1:25 or any value between 1:(15-25).

[0075] In an optional embodiment, the solution in the strong oxidant strong acid solution is concentrated sulfuric acid, and the mass ratio of the solute to the solution in the strong oxidant strong acid solution is 1:20.

[0076] In an optional embodiment, the mass ratio of the natural graphite to the solute in the strong oxidant strong acid solution is 1:(0.5-3), preferably 1:1;

[0077] The optional mass ratio of the natural graphite to the solute in the strong oxidant strong acid solution can be 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3 or any value between 1:(0.5-3).

[0078] In an optional embodiment, during the process of mixing the natural graphite after vacuum heat treatment with the strong oxidant strong acid solution, the system temperature does not exceed 20°C;

[0079] In an optional embodiment, the oxidation treatment temperature is 30-50°C and the time is 1-10h;

[0080] Optionally, the temperature of the oxidation treatment can be 30°C, 40°C, 50°C or any value between 30-50°C, and the time can be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h or any value between 1-10h.

[0081] In an optional embodiment, the oxidation treatment is carried out at a temperature of 35° C. and for a time of 4 hours.

[0082] In an optional embodiment, during the mixing of the mixed solution and water, the system temperature does not exceed 40°C;

[0083] In an optional embodiment, the mass ratio of the mixed solution to water is 1:(3-8), and during the mixing process, the rate of adding water is 2-20 mL / min;

[0084] Optionally, the mass ratio of the mixed solution to water can be 1:3, 1:4, 1:5, 1:6, 1:7, 1:8 or any value between 1:(3-8), and the rate of adding water can be 2 mL / min, 5 mL / min, 10 mL / min, 15 mL / min, 20 mL / min or any value between 2-20 mL / min.

[0085] In an optional embodiment, the mass ratio of the mixed solution to water is 1:4, and the rate of adding water is 5 mL / min;

[0086] In an optional embodiment, the heating reaction temperature is 80-100°C and the time is 0.5-5h;

[0087] Optionally, the temperature of the heating reaction can be 80°C, 90°C, 100°C or any value between 80-100°C, and the time can be 0.5h, 1h, 2h, 3h, 4h, 5h or any value between 0.5-5h.

[0088] In an optional embodiment, the heating reaction temperature is 90° C. and the time is 1 hour.

[0089] In an optional embodiment, the acid solution used for pickling includes at least one of hydrochloric acid, sulfuric acid, nitric acid, and acetic acid, and the concentration of the acid solution is 0.5-3 mol / L;

[0090] Optionally, the concentration of the acid solution may be 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L or any value between 0.5-3 mol / L.

[0091] In an optional embodiment, the acid solution used for pickling is hydrochloric acid with a concentration of 1 mol / L.

[0092] In an optional embodiment, the drying temperature is 60-150° C. and the drying time is 5-24 h;

[0093] Optionally, the drying temperature can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C or any value between 60-150°C, and the drying time can be 5h, 6h, 12h, 18h, 24h or any value between 5-24h.

[0094] In an optional embodiment, the gas in the protective atmosphere includes one or more of nitrogen, argon, carbon dioxide, and hydrogen, and the gas flow rate is 50-200 mL / min;

[0095] Optionally, the gas flow rate may be 50 mL / min, 100 mL / min, 150 mL / min, 200 mL / min, or any value between 50-200 mL / min.

[0096] In an optional embodiment, the high temperature heat treatment is performed at a temperature of 600-1200° C. and a heating rate of 5-20° C. / min.

[0097] Optionally, the temperature of the high-temperature heat treatment can be 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C or any value between 600-1200°C, and the heating rate can be 5°C / min, 10°C / min, 15°C / min, 20°C / min or any value between 5-20°C / min.

[0098] In an optional embodiment, the gas in the protective atmosphere is nitrogen, the gas flow rate is 100 mL / min, the temperature of the high-temperature heat treatment is 800° C., and the heating rate is 10° C. / min.

[0099] The present application also provides a worm-like expanded graphite, which is prepared using the preparation method of the worm-like expanded graphite.

[0100] The present application also provides a sodium ion battery negative electrode, the raw materials of which include the worm-like expanded graphite and a binder;

[0101] In an optional embodiment, the binder includes one or more of polyvinylidene fluoride, sodium carboxymethyl cellulose, sodium alginate, and polystyrene rubber;

[0102] In an optional embodiment, the mass ratio of the worm-like expanded graphite to the binder is (2-10):100, preferably 10:100;

[0103] Optionally, the mass ratio of the worm-like expanded graphite to the binder may be 2:100, 5:100, 10:100 or any value between (2-10):100.

[0104] In an optional embodiment, the current collector material of the negative electrode of the sodium ion battery is selected from any one of pure copper foil, carbon-coated copper foil, pure aluminum foil, carbon-coated aluminum foil, and stainless steel foil.

[0105] The present application also provides a sodium ion battery, comprising the sodium ion battery negative electrode;

[0106] In an optional embodiment, the method for preparing the sodium ion battery comprises:

[0107] The worm-like expanded graphite and the binder are mixed to obtain a slurry, which is then coated on a current collector and dried to obtain a negative electrode of a lithium-ion battery, and then assembled under an argon atmosphere using a sodium-ion electrolyte to obtain a sodium-ion battery;

[0108] In an optional embodiment, in the argon atmosphere, the oxygen content is less than 1 ppm and the water content is less than 1 ppm;

[0109] In an optional embodiment, the sodium salt in the sodium electrolyte includes one or more of sodium hexafluorophosphate, sodium perchlorate, and sodium trifluoromethanesulfonate;

[0110] In an optional embodiment, the concentration of sodium salt in the sodium-electrolyte electrolyte is 0.5-2 mol / L.

[0111] Optionally, the concentration of the sodium salt in the sodium-electrolyte electrolyte may be 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L or any value between 0.5-2 mol / L.

[0112] The present application also provides an electrical device, including the sodium ion battery.

[0113] It should be noted that the electrical equipment referred to in this application not only includes equipment that is itself equipped with the above-mentioned sodium ion batteries, such as electric vehicles, electric bicycles, mobile phones, electronic watches, etc.; it also includes equipment or energy storage equipment powered by the above-mentioned sodium ion batteries, such as power banks, energy storage power stations and their systems, etc.

[0114] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0115] Example 1

[0116] This embodiment provides a worm-like expanded graphite, and the preparation method thereof is as follows:

[0117] After natural graphite is dried at 150° C. in a vacuum drying oven for 12 hours, the graphite is mixed with a potassium permanganate-sodium nitrate-concentrated sulfuric acid solvent in an ice bath, wherein the mass ratio of potassium permanganate-sodium nitrate-concentrated sulfuric acid is 1:1:40, and the mass of graphite to the mass of the solute in the mixed solution is 1:1.

[0118] After the appropriate amount of strong oxidant solvent solution is mixed, the addition process is carried out under ice bath conditions, and the solvent temperature is ensured not to exceed 20°C during the addition process. After the addition is completed, the mixed solution is oxidized at an appropriate temperature. After uniform mixing, the mixed solvent is oxidized at 35°C for 4 hours. After the reaction is completed, stir under ice bath conditions until the solution temperature drops below 20°C, and slowly add water under ice bath conditions for stirring. The rate of adding water is 5mL / min, and the mass of water added is 4 times that of the mixed solution. During the water addition process, it is necessary to ensure that the solution temperature does not exceed 40°C. Then the mixed solution added with water is added again to 90°C for reaction for 1 hour, and an appropriate amount of hydrogen peroxide solution is added until the solution has no bubbles. The obtained sample is washed and dried with a 1mol / L hydrochloric acid solution. After the obtained sample is dried, it is placed in nitrogen for high-temperature heat treatment, and the gas flow rate is 100mL / min. The heat treatment temperature is 800°C, and the heating rate is 10°C / min.

[0119] Figure 1 The scanning electron microscope image of the synthesized worm-like expanded graphite is shown in Figure 2. Figure 2 This is a transmission electron microscope image of the synthesized worm-like expanded graphite.

[0120] Based on the synthesized expanded graphite, it is mixed with sodium carboxymethyl cellulose in a mass ratio of 9:1, and the obtained slurry is evenly coated on the copper current collector by blade coating or spraying. After drying, the electrode is obtained, and the battery is assembled under an argon atmosphere, in which O2<1ppm and H2O<1ppm. The electrolyte is a mixed solution of 1 mol / L sodium perchlorate dissolved in ethylene carbonate / propylene carbonate (mass ratio of 1:1). In a sodium ion battery, the obtained worm-like expanded graphite has an initial reversible specific capacity of 245 mAh / g at a current density of 100 mA / g, and a specific capacity of 232 mAh / g after 50 cycles ( Figure 3 ), the capacity retention rate after 50 cycles is greater than 90%. After 3000 cycles at a high current density of 1A / g, its specific capacity is 122mAh / g ( Figure 4 ).

[0121] Example 2

[0122] This embodiment provides a worm-like expanded graphite, and the preparation method thereof is as follows:

[0123] After natural graphite is dried in a vacuum drying oven at 150° C. for 12 hours, the graphite is mixed with a potassium permanganate-sodium nitrate-concentrated sulfuric acid solvent in an ice bath, wherein the mass ratio of potassium permanganate-sodium nitrate-concentrated sulfuric acid is 1:1:40, and the mass of graphite to the mass of the solute in the mixed solution is 1:0.5.

[0124] After the appropriate amount of strong oxidant solvent solution is mixed, the addition process is carried out under ice bath conditions, and the solvent temperature is ensured not to exceed 20°C during the addition process. After the addition is completed, the mixed solution is oxidized at an appropriate temperature. After mixing evenly, the mixed solvent is oxidized at 50°C for 6 hours. After the reaction is completed, stir under ice bath conditions until the solution temperature drops below 20°C, and slowly add water under ice bath conditions for stirring. The rate of adding water is 5mL / min, and the mass of water added is 4 times that of the mixed solution. During the water addition process, it is necessary to ensure that the solution temperature does not exceed 40°C. Then the mixed solution with water is added again to 90°C for reaction for 4 hours, and an appropriate amount of hydrogen peroxide solution is added until the solution has no bubbles. The obtained sample is cleaned and dried with a 1mol / L hydrochloric acid solution. After the obtained sample is dried, it is placed in nitrogen for high-temperature heat treatment, and the gas flow rate is 100mL / min. The heat treatment temperature is 800°C, and the heating rate is 10°C / min.

[0125] Based on the synthesized expanded graphite, it is mixed with sodium carboxymethyl cellulose in a mass ratio of 9:1, and the obtained slurry is evenly coated on the copper current collector by blade coating or spraying. After drying, the electrode is obtained, and the battery is assembled under an argon atmosphere. In the argon atmosphere, O2<1ppm and H2O<1ppm. The electrolyte is a mixed solution of 1 mol / L sodium perchlorate dissolved in ethylene carbonate / propylene carbonate (mass ratio of 1:1). In a sodium ion battery, the obtained worm-like expanded graphite has an initial reversible specific capacity of 208 mAh / g at a current density of 100 mA / g, and a specific capacity of 198 mAh / g after 50 cycles ( Figure 5 ), the capacity retention rate after 50 cycles is greater than 90%. After 3000 cycles at a high current density of 1A / g, its specific capacity is 89mAh / g ( Figure 6 ).

[0126] Example 3

[0127] This embodiment provides a worm-like expanded graphite, and the preparation method thereof is as follows:

[0128] After natural graphite is dried at 150° C. in a vacuum drying oven for 12 hours, the graphite is mixed with a potassium permanganate-potassium nitrate-concentrated nitric acid solvent in an ice bath, wherein the mass ratio of potassium permanganate-potassium nitrate-concentrated nitric acid is 1:1:40, and the mass of graphite to the mass of the solute in the mixed solution is 1:1.5.

[0129] After the appropriate amount of strong oxidant solvent solution is mixed, the addition process is carried out under ice bath conditions, and the solvent temperature is ensured not to exceed 20°C during the addition process. After the addition is completed, the mixed solution is oxidized at an appropriate temperature. After mixing evenly, the mixed solvent is oxidized at 35°C for 2 hours. After the reaction is completed, stir under ice bath conditions until the solution temperature drops below 20°C, and slowly add water under ice bath conditions for stirring. The rate of adding water is 2mL / min, and the mass of water added is 4 times that of the mixed solution. During the water addition process, it is necessary to ensure that the solution temperature does not exceed 40°C. Then the mixed solution added with water is added again to 90°C for reaction for 4 hours, and an appropriate amount of hydrogen peroxide solution is added until the solution has no bubbles. The obtained sample is cleaned and dried with a 1mol / L hydrochloric acid solution. After the obtained sample is dried, it is placed in nitrogen for high-temperature heat treatment, and the gas flow rate is 100mL / min. The heat treatment temperature is 1000°C, and the heating rate is 10°C / min.

[0130] Based on the synthesized expanded graphite, it is mixed with sodium carboxymethyl cellulose in a mass ratio of 9:1, and the obtained slurry is evenly coated on the copper current collector by blade coating or spraying. After drying, the electrode is obtained, and the battery is assembled in an argon atmosphere. In the argon atmosphere, O2<1ppm and H2O<1ppm. The electrolyte is a mixed solution of 1 mol / L sodium perchlorate dissolved in ethylene carbonate / propylene carbonate (mass ratio of 1:1). In the sodium ion battery, the obtained worm-like expanded graphite has a specific capacity of 189 mAh / g after 50 cycles at a current density of 100 mA / g, and the capacity retention rate after 50 cycles is greater than 90% ( Figure 7 ).

[0131] Example 4

[0132] This embodiment provides a worm-like expanded graphite, and the preparation method thereof is as follows:

[0133] After natural graphite is dried at 200° C. in a vacuum drying oven for 5 hours, the graphite is mixed with a potassium perchlorate-potassium nitrate-concentrated sulfuric acid solvent in an ice bath, wherein the mass ratio of potassium perchlorate-potassium nitrate-concentrated sulfuric acid is 1:1:50, and the mass of graphite to the mass of the solute in the mixed solution is 1:1.

[0134] After the appropriate amount of strong oxidant solvent solution is mixed, the addition process is carried out under ice bath conditions, and the solvent temperature is ensured not to exceed 20°C during the addition process. After the addition is completed, the mixed solution is oxidized at an appropriate temperature. After mixing evenly, the mixed solvent is oxidized at 35°C for 2 hours. After the reaction is completed, stir under ice bath conditions until the solution temperature drops below 20°C, and slowly add water under ice bath conditions for stirring. The rate of adding water is 2mL / min, and the mass of water added is 4 times that of the mixed solution. During the water addition process, it is necessary to ensure that the solution temperature does not exceed 40°C. Then the mixed solution added with water is added again to 90°C for reaction for 4 hours, and an appropriate amount of hydrogen peroxide solution is added until the solution has no bubbles. The obtained sample is cleaned and dried with a 1mol / L hydrochloric acid solution. After the obtained sample is dried, it is placed in nitrogen for high-temperature heat treatment, and the gas flow rate is 100mL / min. The heat treatment temperature is 1000°C, and the heating rate is 10°C / min.

[0135] Based on the synthesized expanded graphite, it is mixed with sodium carboxymethyl cellulose in a mass ratio of 9:1, and the obtained slurry is evenly coated on the copper current collector by blade coating or spraying. After drying, the electrode is obtained, and the battery is assembled in an argon atmosphere. In the argon atmosphere, O2<1ppm and H2O<1ppm. The electrolyte is a mixed solution of 1 mol / L sodium perchlorate dissolved in ethylene carbonate / propylene carbonate (mass ratio of 1:1). In a sodium ion battery, the obtained worm-like expanded graphite has a specific capacity of 185 mAh / g after 50 cycles at a current density of 100 mA / g, and the capacity retention rate after 50 cycles is greater than 90% ( Figure 8 ).

[0136] Comparative Example 1

[0137] Natural graphite is directly used for the negative electrode of sodium ion battery without any related expansion treatment. Natural graphite and sodium carboxymethyl cellulose are mixed in a mass ratio of 9:1, and the obtained slurry is evenly coated on the copper current collector by blade coating or spraying. After drying, the electrode is obtained, and the battery is assembled under argon atmosphere, in which O2<1ppm and H2O<1ppm. The electrolyte is a mixed solution of 1mol / L sodium perchlorate dissolved in ethylene carbonate / propylene carbonate (mass ratio of 1:1). In sodium ion batteries, the first reversible specific capacity of natural graphite is 18mAh / g at a current density of 100mA / g, and the specific capacity is 5mAh / g after 50 cycles.

[0138] Comparative Example 2

[0139] Mixing graphite with potassium permanganate-sodium nitrate-concentrated sulfuric acid solvent directly under ice bath conditions without thorough drying is prone to a sharp rise in temperature. In the comparative experiment, the mass ratio of potassium permanganate-sodium nitrate-concentrated sulfuric acid was 1:1:40, and the mass of graphite to the mass of solute in the mixed solution was 1:0.5. The mixed solution was then oxidized at an appropriate temperature. After uniform mixing, the mixed solvent was oxidized at 50°C for 6 hours. After the reaction was completed, it was stirred under ice bath conditions until the solution temperature dropped below 20°C, and water was slowly added under ice bath conditions for stirring. The rate of adding water was 5mL / min, and the mass of water added was 4 times that of the mixed solution. During the water addition process, it was necessary to ensure that the solution temperature did not exceed 40°C. Then the mixed solution with water was added again to 90°C for reaction for 4 hours, and an appropriate amount of hydrogen peroxide solution was added until no bubbles emerged from the solution. The obtained sample was washed and dried with a 1mol / L hydrochloric acid solution. After drying, the obtained sample was placed in nitrogen for high temperature heat treatment, with a gas flow rate of 100 mL / min. The heat treatment temperature was 800° C. and the heating rate was 10° C. / min.

[0140] Based on the synthesized comparative expanded graphite, it is mixed with sodium carboxymethyl cellulose in a mass ratio of 9:1, and the obtained slurry is evenly coated on the copper current collector by blade coating or spraying, and the electrode is obtained after drying. The battery is assembled in an argon atmosphere, and O2<1ppm and H2O<1ppm in the argon atmosphere. The electrolyte is a mixed solution of 1mol / L sodium perchlorate dissolved in ethylene carbonate / propylene carbonate (mass ratio of 1:1). In a sodium ion battery, the obtained worm-like expanded graphite has an initial reversible specific capacity of 138mAh / g at a current density of 100mA / g, and a specific capacity of 115mAh / g after 50 cycles.

[0141] Comparative Example 3

[0142] After drying natural graphite at 150°C in a vacuum drying oven for 12 hours, the graphite is mixed with potassium permanganate-sodium nitrate-concentrated sulfuric acid solvent under ice bath conditions, wherein the mass ratio of potassium permanganate-sodium nitrate-concentrated sulfuric acid is 1:1:40, and the mass of graphite and the mass of solute in the mixed solution are 1:1. After mixing an appropriate amount of strong oxidant solvent solution, the addition process is carried out under ice bath conditions, and the solvent temperature is ensured not to exceed 20°C during the addition process. After the addition is completed, the mixed solution is oxidized at an appropriate temperature. After mixing evenly, the mixed solvent is oxidized at 35°C for 4 hours. After the reaction is completed, stir under ice bath conditions until the solution temperature drops below 20°C, and slowly add water under ice bath conditions for stirring, the rate of adding water is 5mL / min, and the mass of water added is 4 times that of the mixed solution. During the water addition process, it is necessary to ensure that the solution temperature does not exceed 40°C. Then the mixed solution with water is added again to 90°C for reaction for 1 hour, and an appropriate amount of hydrogen peroxide solution is added until no bubbles emerge from the solution. The obtained sample was washed with 1 mol / L hydrochloric acid solution and dried. After drying, the obtained sample was placed in nitrogen for high temperature heat treatment, with a gas flow rate of 100 mL / min. The heat treatment temperature was 400°C and 1400°C, and the heating rate was 10°C / min.

[0143] Based on the synthesized expanded graphite, it is mixed with sodium carboxymethyl cellulose in a mass ratio of 9:1, and the obtained slurry is uniformly coated on the copper current collector by a doctor blade method or a spraying method. After drying, the electrode is obtained, and the battery is assembled in an argon atmosphere, in which O2<1ppm and H2O<1ppm. The electrolyte is a mixed solution of 1mol / L sodium perchlorate dissolved in ethylene carbonate / propylene carbonate (mass ratio of 1:1). In a sodium ion battery, the obtained expanded graphite (heat treated at 400℃) has a first reversible specific capacity of 76mAh / g at a current density of 100mA / g, and a specific capacity of 65mAh / g after 50 cycles. The obtained expanded graphite (heat treated at 1400℃) has a first reversible specific capacity of 112mAh / g at a current density of 100mA / g, and a specific capacity of 108mAh / g after 50 cycles.

[0144] Comparative Example 4

[0145] After natural graphite is dried at 150° C. in a vacuum drying oven for 12 hours, the graphite is mixed with a potassium permanganate-sodium nitrate-concentrated sulfuric acid solvent in an ice bath, wherein the mass ratio of potassium permanganate-sodium nitrate-concentrated sulfuric acid is 1:1:40, and the mass of graphite to the mass of the solute in the mixed solution is 1:1.

[0146] After the appropriate amount of strong oxidant solvent solution is mixed, the addition process is carried out under ice bath conditions, and the solvent temperature is ensured not to exceed 20°C during the addition process. After the addition is completed, the mixed solution is oxidized at an appropriate temperature. After uniform mixing, the mixed solvent is oxidized at 35°C for 4 hours. After the reaction is completed, stir under ice bath conditions until the solution temperature drops below 20°C, and slowly add water under ice bath conditions for stirring. The rate of adding water is 5mL / min, and the mass of water added is 4 times that of the mixed solution. During the water addition process, it is necessary to ensure that the solution temperature does not exceed 40°C. Then the mixed solution added with water is added again to 90°C for reaction for 1 hour, and an appropriate amount of hydrogen peroxide solution is added until the solution has no bubbles. The obtained sample is washed and dried with a 1mol / L hydrochloric acid solution. After the obtained sample is dried, it is placed in nitrogen for high-temperature heat treatment, and the gas flow rate is 100mL / min. The heat treatment temperature is 800°C, and the heating rate is 10°C / min.

[0147] Based on the synthesized expanded graphite, it is mixed with sodium carboxymethyl cellulose in a ratio of 9:1, and the obtained slurry is evenly coated on the copper current collector by blade coating or spraying, and the electrode is obtained after drying. The battery is assembled in an argon atmosphere, in which O2<1ppm and H2O<1ppm. The electrolyte is 1mol / L sodium perchlorate dissolved in ethylene glycol dimethyl ether solution. In a sodium ion battery, the obtained worm-like expanded graphite has an initial reversible specific capacity of 238mAh / g at a current density of 100mA / g, and a specific capacity of 121mAh / g after 50 cycles.

[0148] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0149] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for preparing worm-like expanded graphite, characterized in that: include: The natural graphite is subjected to vacuum heat treatment, and then mixed with a strong oxidant strong acid solution for oxidation treatment; the temperature of the vacuum heat treatment is 100-200°C, and the time is 5-24h; the solute in the strong oxidant strong acid solution includes one or more of potassium permanganate, potassium dichromate, potassium perchlorate, sodium perchlorate, potassium persulfate, potassium nitrate, and sodium nitrate; during the process of mixing the natural graphite after vacuum heat treatment with the strong oxidant strong acid solution, the system temperature does not exceed 20°C; the temperature of the oxidation treatment is 30-50°C, and the time is 1-10h; the mass ratio of the natural graphite to the solute in the strong oxidant strong acid solution is 1:(0.5-3); The mixed solution obtained by the oxidation treatment is mixed with water, and then heated for reaction; after the heating reaction is completed, the system is mixed with hydrogen peroxide for reaction; during the mixing process of the mixed solution and water, the system temperature does not exceed 40°C; the mass ratio of the mixed solution to water is 1: (3-8), and during the mixing process, the rate of adding water is 2-20mL / min; the temperature of the heating reaction is 80-100°C, and the time is 0.5-5h; The reaction system is subjected to solid-liquid separation, the solid is pickled and dried, and then subjected to high-temperature heat treatment under a protective atmosphere to obtain the worm-like expanded graphite; the acid solution used for the pickling includes at least one of hydrochloric acid, sulfuric acid, nitric acid, and acetic acid, and the concentration of the acid solution is 0.5-3 mol / L; the drying temperature is 60-150° C., and the time is 5-24 h; the gas in the protective atmosphere includes one or more of nitrogen, argon, carbon dioxide, and hydrogen, and the gas flow rate is 50-200 mL / min; the temperature of the high-temperature heat treatment is 600-1200° C., and the heating rate is 5-20° C. / min.

2. The preparation method according to claim 1, characterized in that: The temperature of the vacuum heat treatment is 150° C. and the time is 12 hours.

3. The preparation method according to claim 1, characterized in that: The solutes in the strong oxidant strong acid solution are potassium permanganate and sodium nitrate, and the mass ratio of the potassium permanganate to the sodium nitrate is 1:(0.5-2).

4. The preparation method according to claim 1, characterized in that: The solution in the strong oxidant strong acid solution includes concentrated sulfuric acid and / or concentrated nitric acid, and the mass ratio of the solute to the solution in the strong oxidant strong acid solution is 1:(15-25).

5. The preparation method according to claim 1, characterized in that: The solution in the strong oxidant strong acid solution is concentrated sulfuric acid, and the mass ratio of the solute to the solution in the strong oxidant strong acid solution is 1:

20.

6. The preparation method according to claim 3, characterized in that: The mass ratio of the natural graphite to the solute in the strong oxidant strong acid solution is 1:

1.

7. The preparation method according to claim 1, characterized in that: The temperature of the oxidation treatment is 35° C. and the time is 4 hours.

8. The preparation method according to claim 1, characterized in that: The mass ratio of the mixed solution to water is 1:4, and the rate of adding water is 5 mL / min.

9. The preparation method according to claim 1, characterized in that: The heating reaction was carried out at a temperature of 90° C. and for a time of 1 h.

10. The preparation method according to any one of claims 1 to 9, characterized in that: The acid solution used in the pickling is hydrochloric acid with a concentration of 1 mol / L.

11. The preparation method according to any one of claims 1 to 9, characterized in that: The gas in the protective atmosphere is nitrogen, the gas flow rate is 100 mL / min, the temperature of the high-temperature heat treatment is 800° C., and the heating rate is 10° C. / min.

12. A worm-like expanded graphite, characterized in that: The method for preparing worm-like expanded graphite according to any one of claims 1 to 11 is used to prepare the worm-like expanded graphite.

13. A sodium ion battery negative electrode, characterized in that: The raw materials include the worm-like expanded graphite as claimed in claim 12 and a binder.

14. The sodium ion battery negative electrode according to claim 13, characterized in that: The binder includes one or more of polyvinylidene fluoride, sodium carboxymethyl cellulose, sodium alginate, and polystyrene rubber.

15. The sodium ion battery negative electrode according to claim 14, characterized in that: The mass ratio of the worm-like expanded graphite to the binder is (2-10):

100.

16. The sodium ion battery negative electrode according to claim 15, characterized in that: The mass ratio of the worm-like expanded graphite to the binder is 10:

100.

17. The sodium ion battery negative electrode according to claim 13, characterized in that: The current collector material of the negative electrode of the sodium ion battery is selected from any one of pure copper foil, carbon-coated copper foil, pure aluminum foil, carbon-coated aluminum foil and stainless steel foil.

18. A sodium ion battery, characterized in that: A sodium ion battery negative electrode comprising any one of claims 13 to 17; The preparation method of the sodium ion battery comprises: The worm-like expanded graphite and the binder are mixed to obtain a slurry, which is then coated on a current collector and dried to obtain a negative electrode of a lithium-ion battery, and then assembled under an argon atmosphere using a sodium-ion electrolyte to obtain a sodium-ion battery; The solvent of the sodium-carbonate electrolyte is a mixed solution of ethylene carbonate / propylene carbonate.

19. The sodium ion battery according to claim 18, characterized in that: In the argon atmosphere, the oxygen content is less than 1 ppm and the water content is less than 1 ppm.

20. The sodium ion battery according to claim 18, characterized in that: The sodium salt in the sodium electrolyte includes one or more of sodium hexafluorophosphate, sodium perchlorate, and sodium trifluoromethanesulfonate.

21. The sodium ion battery according to claim 20, characterized in that: The concentration of sodium salt in the sodium electrolyte is 0.5-2 mol / L.

22. An electrical equipment, characterized in that: A sodium ion battery comprising any one of claims 18 to 21.

Citation Information

Patent Citations

  • Method for preparing sulfur-free expanded graphite from natural fine flakes

    CN111377442A