A solar cell and a method for preparing the same

By using the combination of transition layer and anti-reflection layer in the preparation of solar cells, the problem of low short-circuit current of heterojunction cells is solved, the preparation process is simplified, the cell efficiency is improved, and efficient current and voltage performance are achieved.

CN116014022BActive Publication Date: 2024-10-01TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211105438.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-10-01
Estimated Expiration
2042-09-09

AI Technical Summary

Technical Problem

The short-circuit current of heterojunction solar cells is low, resulting in low efficiency, and the existing laser anti-reflection film removal method has a negative impact on cell efficiency.

Method used

During the preparation process of the solar cell, a transition layer is prepared on the first transparent conductive layer, and a corresponding gate metal layer is formed on the anti-reflection layer, and the molten transition layer is used to destroy the anti-reflection layer and make the gate metal The layer is conductively connected to the transparent conductive layer, simplifying the preparation process and improving battery efficiency.

Benefits of technology

This method does not require etching the anti-reflection layer, but only requires the preparation of a transition layer, which improves the preparation effect and efficiency of the solar cell, and increases the short-circuit current and open-circuit voltage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116014022B_ABST
    Figure CN116014022B_ABST
Patent Text Reader

Abstract

The present application provides a solar cell and a preparation method thereof, the preparation method comprising the following steps: preparing a transition layer on a first transparent conductive layer; preparing an anti-reflection layer, the anti-reflection layer partially covers the first transparent conductive layer and partially covers the transition layer; forming a gate metal layer corresponding to the first transparent conductive layer on the anti-reflection layer; the melting temperature of the transition layer is lower than the solidification temperature of the gate metal layer; solidifying the gate metal layer and destroying the anti-reflection layer through the melted transition layer; the gate metal layer passes through the anti-reflection layer and is conductively connected to the first transparent conductive layer. In the above technical solution, the transition layer melts in the anti-reflection layer to form a gap when solidifying the gate metal layer, so that the gate metal layer can be conductively connected to the first transparent conductive layer. During preparation, only one transition layer needs to be prepared, and there is no need to etch the anti-reflection layer as in the prior art, thereby improving the preparation process of the solar cell and improving the effect of the prepared solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular to a solar cell and a method for preparing the same. Background Art

[0002] With the continuous development of solar cell technology, high-efficiency cell technology has become one of the main means to reduce production costs. Compared with PREC cells, heterojunction cell efficiency has obvious advantages in open circuit voltage Voc and fill factor FF, but the short-circuit current gap is quite obvious. On the one hand, the thickness of silicon wafers used for PERC solar cells is 150-180μm, while the thickness of silicon wafers used for heterojunction solar cells is 100-130μm. Since crystalline silicon is an indirect band material with a small light absorption coefficient, when the thickness of the solar cell decreases, the loss caused by the transmitted light increases with the decrease in thickness. Therefore, thin-film cells are more likely to cause insufficient and wasteful use of light, making the current of heterojunction cells significantly lower than that of PERC cells. On the other hand, the anti-reflection film of PREC cells is SIN, which has a better anti-reflection effect. The anti-reflection film of heterojunction cells is ITO, and it is also a conductive film. It is necessary to find a balance between sheet resistance and transmittance, which limits the effect of ITO as an anti-reflection film to be inferior to silicon nitride. Therefore, how to optimize the emission reduction film of heterojunction solar cells and increase the short-circuit current has become an important direction for improving the efficiency of heterojunction cells.

[0003] When using laser to remove the anti-reflection film, the temperature at the laser ablation site is high. On the one hand, oxides are formed on the surface of the gate metal layer, affecting welding. On the other hand, the laser will also affect the battery, further reducing battery efficiency. Summary of the invention

[0004] The present application provides a solar cell and a method for preparing the same, so as to reduce the difficulty of preparing the solar cell.

[0005] In a first aspect, a method for preparing a solar cell is provided, the method comprising the following steps:

[0006] preparing a transition layer on the first transparent conductive layer;

[0007] preparing an anti-reflection layer, wherein the anti-reflection layer partially covers the first transparent conductive layer and partially covers the transition layer;

[0008] forming a gate metal layer corresponding to the first transparent conductive layer on the anti-reflection layer; wherein the melting temperature of the transition layer is lower than the solidification temperature of the gate metal layer;

[0009] The gate metal layer is solidified, and the anti-reflection layer is destroyed by the melted transition layer; the gate metal layer passes through the anti-reflection layer to be conductively connected to the first transparent conductive layer.

[0010] In the above technical solution, the transition layer melts in the anti-reflection layer to form a gap when the gate metal layer is solidified, so that the gate metal layer can be conductively connected to the first transparent conductive layer. During preparation, only one transition layer needs to be prepared, and there is no need to etch the anti-reflection layer as in the prior art, which improves the preparation process of solar cells and improves the effect of the prepared solar cells.

[0011] In a specific embodiment, the transition layer is prepared on the first transparent conductive layer, specifically:

[0012] The transition layer is printed or sprayed on the first transparent conductive layer by screen printing or spraying, and the transition layer is cured.

[0013] In a specific possible implementation manner, the preparation of the anti-reflection layer is specifically: depositing the anti-reflection layer on the first transparent conductive layer and the transition layer by using a PVD or CVD method.

[0014] In a specific embodiment, the anti-reflection layer is one or a stacked film of at least two of SiNx, SiOx, SiOxNy, AlOx, MgF2 and TiO2; wherein x and y are natural numbers.

[0015] In a specific possible implementation manner, a gate metal layer corresponding to the first transparent conductive layer is formed on the anti-reflection layer; specifically:

[0016] The gate metal layer slurry is printed on the anti-reflection layer by a screen printing method, and the gate metal layer slurry is dried; wherein the drying temperature is lower than the melting temperature of the transition layer.

[0017] In a specific implementation manner, the gate metal layer is solidified, and the anti-reflection layer is destroyed by a melted transition layer; the gate metal layer is conductively connected to the first transparent conductive layer, specifically:

[0018] destroying the anti-reflection layer by a melted transition layer;

[0019] The gate metal layer passes through the anti-reflection layer and is conductively connected to the first transparent conductive layer through the transition layer or directly.

[0020] In a specific implementation manner, the gate metal layer passes through the anti-reflection layer and is conductively connected to the first transparent conductive layer through the transition layer or directly, specifically:

[0021] The transition layer is a layer structure made of a conductive material, and the gate metal layer is conductively connected to the first transparent conductive layer through the transition layer; or,

[0022] The transition layer is a layer structure made of an insulating material, and the gate metal layer is mixed with the transition layer and is conductively connected to the first transparent conductive layer.

[0023] In a specific embodiment, the curing temperature is 180-240° C., and the curing time is 5-30 min.

[0024] In a specific implementation scheme, the following steps are also included:

[0025] forming a first intrinsic amorphous silicon layer and a second intrinsic amorphous silicon layer on two opposite surfaces of the silicon wafer;

[0026] forming a first doped amorphous silicon layer on a side of the first intrinsic amorphous silicon layer away from the silicon wafer; forming a second doped amorphous silicon layer on a side of the second intrinsic amorphous silicon layer away from the silicon wafer;

[0027] forming the first transparent conductive layer on a side of the first doped amorphous silicon layer away from the silicon wafer;

[0028] A second transparent conductive layer is formed on a side of the second doped amorphous silicon layer facing away from the silicon wafer.

[0029] In a specific implementation scheme, the following steps are also included:

[0030] The surface of the silicon wafer is etched to form a pyramid structure velvet surface.

[0031] In a specific possible implementation manner, the transition layer is a layer structure made of indium tin alloy or bismuth lead tin alloy and low-temperature resin.

[0032] In a specific implementation manner, the gate metal layer and the transition layer are doped, and the doped gate metal layer is conductively connected to the first transparent conductive layer, specifically:

[0033] The material of the transition layer and the gate metal layer are doped with a doping amount less than 20%.

[0034] In a second aspect, a solar cell is provided, the solar cell comprising a first transparent conductive layer, a transition layer located on the first transparent conductive layer, and an anti-reflection layer covering the first transparent conductive layer and the transition layer;

[0035] It also includes a gate metal layer; the gate metal layer passes through the anti-reflection layer and is conductively connected to the first transparent conductive layer; the transition layer is a layer structure made of conductive material, and the gate metal layer is conductively connected to the first transparent conductive layer through the transition layer; or,

[0036] The transition layer is a layer structure made of an insulating material, and the gate metal layer is doped with the transition layer and is conductively connected to the first transparent conductive layer.

[0037] In the above technical solution, the transition layer melts in the anti-reflection layer to form a gap when the gate metal layer is solidified, so that the gate metal layer can be conductively connected to the first transparent conductive layer. During preparation, only one transition layer needs to be prepared, and there is no need to etch the anti-reflection layer as in the prior art, which improves the preparation process of solar cells and improves the effect of the prepared solar cells.

[0038] In a specific implementation manner, the transition layer is a layer structure made of a conductive material, and the gate metal layer is conductively connected to the first transparent conductive layer through the transition layer; or,

[0039] The transition layer is a layer structure made of an insulating material, and the gate metal layer is mixed with the transition layer and is conductively connected to the first transparent conductive layer.

[0040] In a specific embodiment, the melting temperature of the transition layer is lower than the solidification temperature of the gate metal layer.

[0041] In a specific embodiment, the thickness of the anti-reflection layer located above the transition layer is smaller than the thickness of the transition layer.

[0042] In a specific possible implementation manner, the transition layer is a layer structure made of indium tin alloy or bismuth lead tin alloy and low-temperature resin.

[0043] In a specific embodiment, the shape of the transition layer is substantially the same as that of the gate metal layer.

[0044] In a specific possible implementation manner, when the transition layer is a layer structure made of an insulating material, the volume ratio of the material of the transition layer to the portion of the gate metal layer passing through the anti-reflection layer is 1:4.

[0045] In a specific embodiment, the anti-reflection layer is one or a stacked film of at least two of SiNx, SiOx, SiOxNy, AlOx, MgF2 and TiO2; wherein x and y are natural numbers.

[0046] In a specific embodiment, the thickness of the anti-reflection layer is between 1 and 200 nm.

[0047] In a specific embodiment, the anti-reflection layer covers the transition layer by deposition.

[0048] In a specific embodiment, the invention further comprises a silicon wafer, a first intrinsic amorphous silicon layer and a second intrinsic amorphous silicon layer stacked with the silicon wafer; wherein the silicon wafer is located between the first intrinsic amorphous silicon layer and the second intrinsic amorphous silicon layer; and further comprises:

[0049] a first doped amorphous silicon layer disposed on a side of the first intrinsic amorphous silicon layer away from the silicon wafer; and a first transparent conductive layer disposed on a side of the first intrinsic amorphous silicon layer away from the silicon wafer;

[0050] a second doped amorphous silicon layer disposed on a side of the second intrinsic amorphous silicon layer away from the silicon wafer; and a second transparent conductive layer disposed on a side of the second doped amorphous silicon layer away from the silicon wafer.

[0051] In a specific embodiment, it also includes a silicon wafer supporting the first transparent conductive layer, and the surface of the silicon wafer has a pyramid structure velvet surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 A schematic diagram of the structure of a solar cell provided in an embodiment of the present application;

[0053] Figure 2 A flow chart of a method for preparing a solar cell provided in an embodiment of the present application;

[0054] Figure 3 A process flow chart of curing the gate metal layer provided in an embodiment of the present application;

[0055] Figure 4 A process flow chart of curing the gate metal layer provided in an embodiment of the present application;

[0056] Figure 5 A partial flow chart of a method for preparing a solar cell provided in an embodiment of the present application. DETAILED DESCRIPTION

[0057] The present application is further described in detail below through the accompanying drawings and embodiments. Through these descriptions, the characteristics and advantages of the present application will become clearer and more specific.

[0058] The word "exemplary" is used exclusively herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as preferred or advantageous over other embodiments. Although various aspects of the embodiments are shown in the drawings, the drawings are not necessarily drawn to scale unless otherwise noted.

[0059] In addition, the technical features involved in different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.

[0060] To facilitate understanding of the method for preparing a solar cell provided in an embodiment of the present application, the structure of the solar cell is first described. The solar cell provided in an embodiment of the present application includes a plurality of layer structures, and the layer structures are stacked to form a heterojunction cell. When an existing heterojunction cell is used to prepare an anti-reflection film, the structure of the cell is affected. For this reason, an embodiment of the present application provides a solar cell to improve the performance of the cell. The following is a detailed description of the method in conjunction with specific drawings and embodiments.

[0061] To facilitate understanding of the method for preparing the solar cell provided in the embodiment of the present application, the main structure of the solar cell provided in the embodiment of the present application is first introduced. Figure 1 As shown, Figure 1 A schematic diagram of the structure of a solar cell provided in an embodiment of the present application. The main structure of the solar cell provided in an embodiment of the present application includes a plurality of stacked structures, which form a heterojunction structure. Exemplarily, the main structure of the solar cell includes: a silicon wafer 1, a first intrinsic amorphous silicon layer 2, a first doped amorphous silicon layer 4, a first transparent conductive layer 6, an anti-reflection layer 8, and a first gate metal layer 10 formed on one surface of the silicon wafer 1; and a second intrinsic amorphous silicon layer 3, a second doped amorphous silicon layer 5, a second transparent conductive layer 7, and a second gate metal layer 11 formed in sequence on the other side of the silicon wafer 1. The above-mentioned sequentially refers to the order of stacking in sequence in the direction away from the silicon wafer 1.

[0062] In the above structure, the first doped amorphous silicon layer 4, the first intrinsic amorphous silicon layer 2, the silicon wafer 1, the second intrinsic amorphous silicon layer 3, and the second doped amorphous silicon layer 5 form a heterojunction structure.

[0063] In the embodiment of the present application, the silicon wafer 1 may be an N-type silicon wafer 1 or a P-type silicon wafer 1. In the embodiment of the present application, an N-type silicon wafer is taken as an example for description.

[0064] The first doped amorphous silicon layer 4 and the second doped amorphous silicon layer 5 can be made of different amorphous silicon materials to form different types of heterojunctions. Exemplarily, the amorphous silicon material can be an N-type amorphous silicon material or a P-type amorphous silicon material to form a pN junction. Specifically, the first doped amorphous silicon layer 4 can be an amorphous silicon material layer doped with P-type impurities, and the second doped amorphous silicon layer 5 can be an amorphous silicon material layer doped with N-type impurities. Alternatively, the first doped amorphous silicon layer 4 can be an amorphous silicon material layer doped with N-type impurities, and the second doped amorphous silicon layer 5 can be an amorphous silicon material layer doped with P-type impurities. The specific setting can be based on actual conditions and is not specifically limited in the embodiments of the present application.

[0065] The n-type impurity elements include Group VA elements, including but not limited to phosphorus, arsenic, and antimony. The p-type impurity elements include Group IIIA elements, including but not limited to boron, aluminum, gallium, indium, and thallium.

[0066] refer to Figure 2 , Figure 2 The process of the method for preparing a solar cell provided in an embodiment of the present application is shown, and the preparation process includes the following steps:

[0067] Step 001: preparing a transition layer 9 on the first transparent conductive layer 6;

[0068] Specifically, the transition layer 9 is printed or sprayed on the first transparent conductive layer 6 by screen printing or spraying, and the transition layer 9 is cured. The formed transition layer 9 is stacked with the first transparent conductive layer 6 and is located on the side of the first transparent conductive layer 6 away from the first doped amorphous silicon layer 4.

[0069] The shape and size of the transition layer 9 match the shape and size of the first gate metal layer 10. That is, when the transition layer is provided, the shape of the transition layer 9 is substantially the same as that of the first gate metal layer 10, such as being completely the same, or there is a slight difference in the width of the line type (such as an error caused during the preparation process).

[0070] The transition layer 9 can be made of different materials. For example, the transition layer 9 can be a metal substance or a non-metal substance, an organic substance or an inorganic substance, and can be conductive or insulating. As an optional solution, the transition layer 9 is preferably a conductive metal substance. For example, the transition layer is a layer structure made of an indium tin alloy or a bismuth-lead-tin alloy and a low-temperature resin.

[0071] When the transition layer 9 is made of non-conductive material, the doping amount of the material of the transition layer 9 and the first gate metal layer 10 is less than 20%. The above doping concentration refers to the concentration of the transition layer 9 and the first gate metal layer 10 when the portion connected to the first transparent conductive electrode 6 is doped. The specific doping concentration can be 19%, 18%, 17%, 12%, 8%, 5% and other different concentrations. When the above concentration is used, it is avoided that too much transition layer 9 affects the effect of the electrical connection between the first gate metal layer 10 and the first transparent conductive electrode 6.

[0072] However, it should be understood that no matter what material the transition layer 9 is made of, it must satisfy the following requirements: the melting point of the transition layer 9 is lower than the curing temperature of the gate metal layer to be printed later, so that the transition layer 9 can be melted when the gate metal layer is cured.

[0073] Step 002: preparing an anti-reflection layer 8, wherein the anti-reflection layer 8 partially covers the first transparent conductive layer 6 and partially covers the transition layer 9;

[0074] Specifically, the anti-reflection layer 8 is prepared by depositing the anti-reflection layer 8 on the first transparent conductive layer 6 and the transition layer 9 by using a PVD or CVD method.

[0075] The formed anti-reflection layer 8 covers the first transparent conductive layer 6 and the transition layer 9. Exemplarily, when the anti-reflection layer 8 is formed, the side of the anti-reflection layer 8 facing away from the first transparent conductive layer 6 is a plane. When the anti-reflection layer 8 is formed, the anti-reflection layer 8 partially covers the first transparent conductive layer 6 (the area not blocked by the transition layer 9) and partially covers the transition layer 9.

[0076] Since the transition layer 9 is stacked with the first transparent conductive layer 6, and the surface morphology of the transition layer 9 is different from that of the first transparent conductive layer 6, the thickness of the anti-reflection layer 8 covering the transition layer 9 is different from that of the anti-reflection layer 8 covering the first transparent conductive layer 6. As an example, the thickness of the anti-reflection layer 8 covering the transition layer 9 is less than the thickness of the anti-reflection layer 8 covering the first transparent conductive layer 6. For example, the thickness of the anti-reflection layer 8 covering the transition layer 9 is 1 to 20 nm less than the thickness of the anti-reflection layer 8 covering the first transparent conductive layer 6, such as 2 nm, 8 nm, and other different thicknesses. Of course, the thickness of the anti-reflection layer 8 covering the transition layer 9 may also be equal to or greater than the thickness of the anti-reflection layer 8 covering the first transparent conductive layer 6.

[0077] The anti-reflection layer 8 can be made of different materials, as long as it can reduce the reflection of sunlight. Exemplarily, the anti-reflection layer 8 is one of SiNx, SiOx, SiOxNy, AlOx, MgF2 and TiO2, or at least two laminated films; wherein x and y are natural numbers. For example, the anti-reflection layer 8 is an anti-reflection layer 8 made of any one of SiNx, SiOx, SiOxNy, AlOx, MgF2 and TiO2. Alternatively, the anti-reflection film is a film formed by stacking SiNx and SiOx, or a film layer formed by stacking SiOx and SiOxNy, or a film layer formed by stacking AlOx, MgF2 and TiO2. It should be understood that when multiple films are stacked, they can be combined arbitrarily according to needs, and are not limited to the several stacking methods exemplified above.

[0078] Step 003: forming a gate metal layer corresponding to the first transparent conductive layer 6 on the anti-reflection layer 8; wherein the melting temperature of the transition layer 9 is lower than the solidification temperature of the gate metal layer;

[0079] Specifically, in this step, the gate metal layer is referred to as Figure 1 The first gate metal layer 10 in the embodiment of the present invention is referred to as the gate metal layer, and in the following text, unless otherwise specified, the gate metal layer is referred to as the first gate metal layer. When preparing the gate metal layer, a slurry of the gate metal layer is printed on the anti-reflection layer 8 by a screen printing method, and the slurry of the gate metal layer is dried; wherein the drying temperature is lower than the melting temperature of the transition layer 9.

[0080] Step 004: solidify the gate metal layer, and destroy the anti-reflection layer 8 through the melted transition layer 9; the gate metal layer passes through the anti-reflection layer 8 and is conductively connected to the first transparent conductive layer 6.

[0081] Specifically, the curing temperature of the gate metal layer is 180-240°C, and the curing time is 5-30 minutes. It is reasonable, and the curing temperature of the gate metal layer is different temperatures such as 180°C, 200°C, 220°C, and 240°C. When the gate metal layer passes through the anti-reflection layer 8 and is conductively connected to the first transparent conductive layer 6, it can be specifically done in the following ways:

[0082] The anti-reflection layer 8 is destroyed by the melted transition layer 9 ; the gate metal layer passes through the anti-reflection layer 8 and is conductively connected to the first transparent conductive layer 6 through the transition layer 9 or directly.

[0083] Exemplarily, since the melting temperature of the transition layer 9 is lower than the solidification temperature of the gate metal layer, when the gate metal layer melts, the transition layer 9 is melted first. As can be seen from step 002, the transition layer 9 is below the anti-reflection layer 8. After the transition layer 9 melts, the height of the transition layer 9 decreases, forming a trapezoidal structure or other special-shaped structure that is larger than the gate metal layer. The anti-reflection layer 8 located above the transition layer 9 will collapse due to lack of support, thereby forming a channel or gap that can accommodate the metal of the gate metal layer to flow in. It should be understood that the channel or gap is an irregular channel shape formed by the collapse of the anti-reflection layer 8. The figure only illustrates the position of the channel and does not represent the actual shape of the channel.

[0084] The gate metal layer flows into the channel before solidification and is conductively connected to the first transparent conductive layer 6 directly or indirectly through the transition layer 9 as follows:

[0085] refer to Figure 3 , illustratively, in a layer structure where the transition layer 9 is made of a conductive material, the gate metal layer is conductively connected to the first transparent conductive layer 6 through the transition layer 9. That is, the gate metal layer is conductively connected to the transition layer 9, and the transition layer 9 is conductively connected to the first transparent conductive layer 6. Alternatively, it can be understood that the gate metal layer is melted with the transition layer 9 and conductively connected to the first transparent conductive layer 6.

[0086] refer to Figure 4 , illustratively, in a layer structure where the transition layer 9 is made of an insulating material, the gate metal layer is doped with the transition layer 9, and the doped gate metal layer is conductively connected to the first transparent conductive layer 6. illustratively, during the curing process of the gate metal layer, the material of the transition layer 9 is doped with the material of the gate metal layer to form a conductive mixture, and the doped gate metal layer is directly in contact with the first transparent conductive layer 6 and conductively connected.

[0087] It can be seen from the above description that by adding a transition layer 9 between the first transparent conductive layer 6 and the anti-reflection layer 8, and forming a gap in the anti-reflection layer 8 through the transition layer 9, the gate metal layer can be conductively connected to the first transparent conductive layer 6. Compared with the prior art, the preparation method disclosed in the present application only needs to prepare one transition layer 9, and there is no need to etch the anti-reflection layer 8 as in the prior art, thereby improving the preparation process of the solar cell and improving the effect of the prepared solar cell.

[0088] In the method for preparing the solar cell panel provided in the embodiment of the present application, in addition to the above steps, it can also include a method for preparing the first intrinsic amorphous silicon layer 2, the second intrinsic amorphous silicon layer 3, the first doped amorphous silicon layer 4, the second doped amorphous silicon layer 5, and the second transparent electrode layer.

[0089] refer to Figure 5 When preparing the above layer structure, the preparation method further comprises:

[0090] Step 01: forming a first intrinsic amorphous silicon layer 2 and a second intrinsic amorphous silicon layer 3 on two opposite surfaces of a silicon wafer 1;

[0091] Specifically, when forming the first intrinsic amorphous silicon layer 2 and the second intrinsic amorphous silicon layer 3 , the surface of the silicon wafer 1 may be etched to form a pyramid-structured velvet surface, so as to better form the first intrinsic amorphous silicon layer 2 and the second intrinsic amorphous silicon layer 3 on the silicon wafer 1 .

[0092] Step 02: forming a first doped amorphous silicon layer 4 on a side of the first intrinsic amorphous silicon layer 2 facing away from the silicon wafer 1; forming a second doped amorphous silicon layer 5 on a side of the second intrinsic amorphous silicon layer 3 facing away from the silicon wafer 1;

[0093] Step 03: forming a first transparent conductive layer 6 on a side of the first doped amorphous silicon layer 4 facing away from the silicon wafer 1;

[0094] Step 04: Form a second transparent conductive layer 7 on the side of the second doped amorphous silicon layer 5 facing away from the silicon wafer 1 .

[0095] After the above structure is prepared, a transition layer 9 , a gate metal layer, an anti-reflection layer 8 and other structures can be prepared on the first transparent conductive layer 6 .

[0096] To facilitate understanding of the above-mentioned preparation method provided in the embodiment of the present application, the preparation process of the solar cell panel provided in the embodiment of the present application is described in detail below.

[0097] 1) The silicon wafer 1 is textured and cleaned.

[0098] Specifically, a 3 μm mechanical damage layer of the N-type silicon wafer can be removed with a 50% KOH solution, and then the surface of the silicon wafer 1 is corroded with a 10% NaOH solution and a texturing additive to form a 2.5 μm pyramid structure texturing surface.

[0099] 2) growing a first intrinsic amorphous silicon layer 2 and a first doped amorphous silicon layer 4 on one side of the textured substrate using a plasma enhanced chemical vapor deposition (PECVD) device; then growing a second intrinsic amorphous silicon layer 3 and a second doped amorphous silicon layer 5 on the other side of the textured substrate;

[0100] Specifically, a PECVD method is used to deposit a first intrinsic amorphous silicon layer 2 with a thickness of 5 nm and an N-type doped amorphous silicon layer (first doped amorphous silicon layer 4 ) with a thickness of 15 nm on the front side of the silicon wafer 1 .

[0101] A 5 nm thick second intrinsic amorphous silicon layer 3 and a 20 nm thick P-type doped amorphous silicon layer (second doped amorphous silicon layer 5 ) are deposited on the back side of the silicon wafer 1 by using a PECVD method.

[0102] 3) depositing a first transparent conductive layer 6 on the N-type doped amorphous silicon layer and a second transparent conductive layer 7 on the P-type doped amorphous silicon layer by using a PVD deposition method selected from magnetron sputtering, reactive plasma deposition and electron beam evaporation;

[0103] Specifically, a 40 nm thick ITO film layer (first transparent conductive layer 6) is deposited on the N-type doped amorphous silicon layer, and a 70 nm thick ITO film layer (second transparent conductive layer 7) is deposited on the surface of the P-type doped amorphous silicon layer by magnetron sputtering.

[0104] 4) Print or spray the transition layer 9 on the first transparent conductive layer 6 by screen printing or spraying, and cure it.

[0105] Specifically, a gate-shaped transition layer 9 is printed on the ITO film layer by screen printing and then dried. The gate-shaped transition layer 9 is referred to as: the transition layer 9 is a gate-shaped pattern, which matches the shape and size of the first gate metal layer 10 pattern.

[0106] The melting point of the transition layer 9 is lower than the curing temperature of the gate metal layer printed later. The transition layer 9 can be a metal substance or a non-metal substance, an organic substance or an inorganic substance, and can be conductive or insulating, preferably a conductive metal substance. Exemplarily, the transition layer 9 is a conductive substance containing indium, with a melting point of about 160°C and a thickness of about 2um. The melting point is relatively low.

[0107] 5) Depositing an anti-reflection thin film layer on the first transparent conductive layer 6 and the transition layer 9 by PVD or CVD method; the anti-reflection film is one or more laminated films selected from SiNx, SiOx, SiOxNy, AlOx, MgF2 and TiO2.

[0108] Specifically, a 70 nm thick SiNx film (anti-reflection layer 8) is deposited on the ITO film layer (first transparent conductive layer 6) and the transition layer 9 using a PECVD method, and the deposition temperature is 25°C.

[0109] Exemplarily, the thickness of the anti-reflection layer 8 may be 1-200 nm, such as 1 nm, 5 nm, 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, etc. As an optional solution, the thickness of the anti-reflection layer 8 may be 30-100 nm, such as 30 nm, 40 nm, 60 nm, 70 nm, 80 nm, 100 nm, etc.

[0110] 6) Printing a back gate metal layer on the second transparent conductive layer 7 and drying it. The drying temperature can be higher or lower than the melting point of the transition layer 9 .

[0111] Specifically, a screen printing method is used to print a gate metal layer on the ITO film layer (second transparent conductive layer 7). Exemplarily, the gate metal layer has a width of about 45 um, and the paste is dried at 150° C. for 3 minutes.

[0112] 7) Printing a gate metal layer on the anti-reflection layer 8 and curing it. The curing temperature is higher than the melting point of the transition layer 9 .

[0113] Specifically, the front gate metal layer pattern matches the shape of the transition layer 9 pattern, and the size of the gate line pattern can be greater than, equal to, or less than the length and width of the gate line pattern of the transition layer 9. During the solidification process of the gate metal layer, the transition layer 9 melts and flows, so that the anti-reflection layer 8 above it is torn, so that the gate line electrode contacts the transparent conductive electrode.

[0114] In the specific preparation process, a gate metal layer is printed on the ITO film layer (first transparent conductive layer 6) by screen printing, and the gate metal layer matches the position of the transition layer 9. The gate metal layer has a width of about 40 um, and the slurry is dried at 150° C. for 3 minutes. Then, the slurry is cured at 210° C. for 10 minutes.

[0115] The transition layer 9 melts and flows during the solidification process of the gate metal layer, so that the reflective film layer 8 above it is torn, so that the first gate metal layer 10 is in contact with the ITO film layer 6 .

[0116] In the above technical solution, a transition layer 9 is added between the first transparent conductive layer 6 and the anti-reflection layer 8, and the transition layer 9 is melted when the gate metal layer is solidified to form a gap in the anti-reflection layer 8, so that the gate metal layer can be conductively connected to the first transparent conductive layer 6. Compared with the prior art, the preparation method disclosed in the present application only needs to prepare a layer of transition layer 9, and there is no need to etch the anti-reflection layer 8 as in the prior art, which improves the preparation process of the solar cell and improves the effect of the prepared solar cell. In addition, adding an anti-reflection film layer on the front of the heterojunction solar cell makes the heterojunction solar cell of this structure have the advantages of high opening voltage and short-circuit current, thereby improving the conversion efficiency of the solar cell.

[0117] Continue to refer Figure 1 , the embodiment of the present application also provides a solar cell, the main structure of which includes a plurality of stacked structures. Exemplarily, the solar cell may include a silicon wafer 1, a first intrinsic amorphous silicon layer 2 and a second intrinsic amorphous silicon layer 3 stacked with the silicon wafer 1; wherein the silicon wafer 1 is located between the first intrinsic amorphous silicon layer 2 and the second intrinsic amorphous silicon layer 3; and further includes: a first doped amorphous silicon layer 4 arranged on a side of the first intrinsic amorphous silicon layer 2 away from the silicon wafer 1; a first transparent conductive layer 6 arranged on a side of the first intrinsic amorphous silicon layer 2 away from the silicon wafer 1; a second doped amorphous silicon layer 5 arranged on a side of the second intrinsic amorphous silicon layer 3 away from the silicon wafer 1; and a second transparent conductive layer 7 arranged on a side of the second doped amorphous silicon layer 5 away from the silicon wafer 1. The details of the first doped amorphous silicon layer 4, the first intrinsic amorphous silicon layer 2, the silicon wafer 1, the second intrinsic amorphous silicon layer 3, and the second doped amorphous silicon layer 5 can be referred to the above description about Figure 1 The relevant description in will not be repeated here.

[0118] The solar cell provided in the embodiment of the present application also includes a transition layer 9 located on the first transparent conductive layer 6, and an anti-reflection layer 8 covering the first transparent conductive layer 6 and the transition layer 9; the gate metal layer passes through the anti-reflection layer 8 and is conductively connected to the first transparent conductive layer 6; the transition layer 9 is a layer structure made of a conductive material, and the gate metal layer is conductively connected to the first transparent conductive layer 6 through the transition layer 9; or, the transition layer 9 is a layer structure made of an insulating material, and the gate metal layer is doped with the transition layer 9 and is conductively connected to the first transparent conductive layer 6.

[0119] Exemplarily, the transition layer 9 is a layer structure made of indium-tin alloy or bismuth-lead-tin alloy and low-temperature resin.

[0120] When the transition layer 9 is provided, the shape and size of the transition layer 9 match the shape and size of the first gate metal layer 10. That is, when the transition layer is provided, the shape of the transition layer 9 is substantially the same as the shape of the first gate metal layer 10, such as being completely the same, or there is a slight difference in the width of the line type (such as an error caused during the preparation process).

[0121] In addition, when the transition layer 9 is made of insulating material, the volume ratio of the material of the transition layer 9 to the portion of the first gate metal layer 10 passing through the anti-reflection layer is 1:4. The above volume ratio refers to the volume ratio of the transition layer 9 to the portion of the first gate metal layer 10 used to connect with the first transparent conductive electrode 6. The specific volume ratio of the two can be: 1:6, 1:7, 1:8, 1:9, 1:10 and other different volume ratios. When the above concentration is used, it is avoided that too much transition layer 9 affects the effect of the electrical connection between the first gate metal layer 10 and the first transparent conductive electrode 6.

[0122] In the above technical solution, a transition layer 9 is added between the first transparent conductive layer 6 and the anti-reflection layer 8, and the transition layer 9 is melted when the gate metal layer is solidified to form a gap in the anti-reflection layer 8, so that the gate metal layer can be conductively connected to the first transparent conductive layer 6. Compared with the prior art, the preparation method disclosed in the present application only needs to prepare one transition layer 9, and there is no need to etch the anti-reflection layer 8 as in the prior art, thereby improving the preparation process of the solar cell and improving the effect of the prepared solar cell.

[0123] When the transition layer 9 is specifically provided, the melting temperature of the transition layer 9 is lower than the solidification temperature of the gate metal layer. For details, reference may be made to the relevant descriptions in step 001 and step 004.

[0124] When the anti-reflection layer 8 is provided, the thickness of the anti-reflection layer 8 located above the transition layer 9 is less than the thickness of the transition layer 9. Thus, the thickness of the anti-reflection layer 8 located above the transition layer 9 is relatively low, so that when the transition layer 9 melts, the anti-reflection layer 8 located above the transition layer 9 can collapse, forming a space for accommodating the flow of the gate metal layer.

[0125] In addition, the anti-reflection layer 8 is one or at least two laminated films of SiNx, SiOx, SiOxNy, AlOx, MgF2 and TiO2; wherein x and y are natural numbers. For details, please refer to the relevant description in step 002. When the anti-reflection layer 8 is specifically set, the thickness of the anti-reflection layer 8 is between 1-200nm. For example, different thicknesses such as 1nm, 50nm, 100nm, 150nm, and 200nm.

[0126] When the anti-reflection layer 8 is specifically prepared, the anti-reflection layer 8 covers the transition layer 9 by deposition. For details, please refer to the relevant description in step 002, which will not be repeated here.

[0127] In the description of the present application, it should be noted that the terms "upper", "lower", "inside", "outside", "front", "back", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships in the working state of the present application. They are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they should not be understood as limitations on the present application.

[0128] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "install", "connect" and "connect" should be understood in a broad sense. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0129] The present application has been described above in conjunction with preferred embodiments, but these embodiments are only exemplary and serve only as an illustration. On this basis, various replacements and improvements may be made to the present application, all of which fall within the scope of protection of the present application.

Claims

1. A method for preparing a solar cell, characterized in that: The following steps are involved: preparing a transition layer on the first transparent conductive layer; preparing an anti-reflection layer, wherein the anti-reflection layer partially covers the first transparent conductive layer and partially covers the transition layer; forming a gate metal layer corresponding to the first transparent conductive layer on the anti-reflection layer; wherein the melting temperature of the transition layer is lower than the solidification temperature of the gate metal layer, and the shape of the transition layer is substantially the same as that of the gate metal layer; The gate metal layer is solidified, and the anti-reflection layer is destroyed by a melted transition layer; the gate metal layer is conductively connected to the first transparent conductive layer through the anti-reflection layer, specifically: destroying the anti-reflection layer by a melted transition layer; The gate metal layer passes through the anti-reflection layer and is conductively connected to the first transparent conductive layer through the transition layer or directly; Wherein, the transition layer is a layer structure made of a conductive material, and the gate metal layer is conductively connected to the transition layer; or, The transition layer is a layer structure made of an insulating material, the gate metal layer is doped with the transition layer, and the doped gate metal layer is conductively connected to the first transparent conductive layer.

2. The preparation method according to claim 1, characterized in that: The step of preparing a transition layer on the first transparent conductive layer comprises: The transition layer is printed or sprayed on the first transparent conductive layer by screen printing or spraying, and the transition layer is cured.

3. The preparation method according to claim 1, characterized in that: The preparation of the anti-reflection layer specifically includes: depositing the anti-reflection layer on the first transparent conductive layer and the transition layer by using a PVD or CVD method.

4. The preparation method according to claim 3, characterized in that: The anti-reflection layer is one or a stacked film of at least two of SiNx, SiOx, SiOxNy, AlOx, MgF2 and TiO2; wherein x and y are natural numbers.

5. The preparation method according to claim 1, characterized in that: The gate metal layer corresponding to the first transparent conductive layer is formed on the anti-reflection layer; specifically: The gate metal layer slurry is printed on the anti-reflection layer by a screen printing method, and the gate metal layer slurry is dried; wherein the drying temperature is lower than the melting temperature of the transition layer.

6. The preparation method according to claim 1, characterized in that: The curing temperature is 180-240° C., and the curing time is 5-30 minutes.

7. The preparation method according to claim 1, characterized in that: The transition layer is a layer structure made of indium tin alloy or bismuth lead tin alloy and low-temperature resin.

8. The preparation method according to claim 1, characterized in that: The gate metal layer is doped with the transition layer, and the doped gate metal layer is conductively connected with the first transparent conductive layer, specifically: The material of the transition layer and the gate metal layer are doped with a doping amount less than 20%.

9. A solar cell, characterized in that: It includes a first transparent conductive layer, a transition layer located on the first transparent conductive layer, and an anti-reflection layer covering the first transparent conductive layer and the transition layer; It also includes a gate metal layer; the gate metal layer passes through the anti-reflection layer and is conductively connected to the first transparent conductive layer; the transition layer is a layer structure made of conductive material, and the gate metal layer is conductively connected to the first transparent conductive layer through the transition layer; or, The transition layer is a layer structure made of insulating material, and the gate metal layer is doped with the transition layer and is conductively connected to the first transparent conductive layer; The melting temperature of the transition layer is lower than the solidification temperature of the gate metal layer, and the shape of the transition layer is substantially the same as that of the gate metal layer.

10. The solar cell according to claim 9, characterized in that: The thickness of the anti-reflection layer located above the transition layer is smaller than the thickness of the transition layer.

11. The solar cell according to claim 9, characterized in that: The transition layer is a layer structure made of indium tin alloy or bismuth lead tin alloy and low-temperature resin.

12. The solar cell according to claim 9, characterized in that: When the transition layer is a layer structure made of insulating material, the volume ratio of the material of the transition layer to the portion of the gate metal layer passing through the anti-reflection layer is 1:

4.

13. The solar cell according to claim 9, characterized in that: The anti-reflection layer is one or a stacked film of at least two of SiNx, SiOx, SiOxNy, AlOx, MgF2 and TiO2; wherein x and y are natural numbers.

14. The solar cell according to claim 9, characterized in that The thickness of the anti-reflection layer is between 1 and 200 nm.

15. The solar cell according to any one of claims 9 to 14, characterized in that: The anti-reflection layer covers the transition layer and the first transparent conductive layer by deposition.

16. The solar cell according to claim 15, characterized in that: It also includes a silicon wafer that supports the first transparent conductive layer, and the surface of the silicon wafer has a pyramid-structured velvet surface.