A method for preparing high-strength and high-hardness stainless steel-based composite materials by selective laser melting

FeCoNiAlTi high-entropy alloy and 316L stainless steel powder are mixed through selective laser melting technology to prepare high-strength and high-hardness stainless steel-based composite materials, which solves the problem of easy failure of materials under high-strength working conditions in traditional methods and realizes the improvement of materials. The uniform composition and fine-grained structure significantly improve its mechanical properties.

CN116021035BActive Publication Date: 2024-10-15SHANGHAI UNIV OF ENG SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310140339.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-21
Publication Date
2024-10-15
Estimated Expiration
2043-02-21

AI Technical Summary

Technical Problem

316L stainless steel prepared by traditional methods is prone to failure under high-strength working conditions, with uneven composition and coarse grains, affecting its mechanical properties.

Method used

Selective laser melting technology is used to mix FeCoNiAlTi high-entropy alloy powder and 316L stainless steel powder in a specific ratio. After screening and baking powder processing, selective laser melting technology is used for laser printing to prepare a stainless steel-based composite with uniform composition and fine-grained structure. Material.

Benefits of technology

The tensile strength and hardness of stainless steel-based composite materials are significantly improved. The tensile strength can reach 1262MPa and the hardness can reach 5.4GPa, which solves the problem of easy failure of materials prepared by traditional methods under high-strength working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116021035B_ABST
    Figure CN116021035B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a high-strength and high-hardness stainless steel-based composite material by selective laser melting, which belongs to the field of alloy manufacturing technology and comprises the following steps: adding FeCoNiAlTi high entropy alloy powder to 316L stainless steel powder with a reinforcement ratio of xwt.% (x=2, 5, 10), mechanically mixing in a three-dimensional motion powder mixer to obtain composite material powder; then directly forming a stainless steel composite material component by selective laser melting printing; the stainless steel composite material prepared by the selective laser melting of the present invention has excellent mechanical properties and dimensional accuracy. After testing, it was found that its tensile strength at room temperature is up to 1262MPa, and its hardness can reach up to 5.4GPa. The present invention solves the problem that stainless steel is prone to failure under high-strength working conditions, and provides a new idea for the strengthening and processing of stainless steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy manufacturing, and in particular relates to a method for preparing a high-strength and high-hardness stainless steel-based composite material by selective laser melting. Background Art

[0002] 316L stainless steel is widely used in all aspects of daily life because of its good forming properties, corrosion resistance, welding properties and other advantages. At present, this material has become very mature after long-term research, and its performance has reached its limit. Therefore, in order to solve the problem that 316L stainless steel is prone to failure under high-strength conditions, a reinforcement phase is usually added to stainless steel to prepare stainless steel composite materials. High entropy alloys, also known as multi-principal alloys, have excellent properties such as high strength, good plasticity and corrosion resistance, and are an ideal reinforcement phase material. At present, the commonly used preparation methods for stainless steel composite materials are casting and powder metallurgy. However, composite materials prepared by traditional methods usually have uneven composition and coarse grains. The selective laser melting method is a process in which powder is melted by a high-energy laser and stacked layer by layer. This technology can obtain components with uniform composition and fine grain structure, and improve the mechanical properties of stainless steel. Summary of the invention

[0003] In order to solve the above technical problems, the present invention proposes a method for preparing high-strength and high-hardness stainless steel-based composite materials by selective laser melting, so as to solve the problem that 316L stainless steel prepared by the current traditional method is prone to failure under high-strength working conditions.

[0004] To achieve the above object, the present invention provides a method for preparing a high-strength and high-hardness stainless steel-based composite material by selective laser melting, comprising the following steps: mixing FeCoNiAlTi high-entropy alloy powder with stainless steel powder to obtain composite material powder, and performing laser printing by selective laser melting technology to obtain a stainless steel-based composite material;

[0005] The scanning speed of the laser printing is 650 mm / s to 1000 mm / s. Beyond this scanning range, there are many defects such as pores and cracks, and even the printing cannot be formed.

[0006] Furthermore, the FeCoNiAlTi high entropy alloy powder is mixed with the stainless steel powder according to a reinforcement ratio of xwt.%, wherein x=2-10, preferably x=2, 5, 10. When the reinforcement ratio exceeds 10wt.%, the molding may fail; when the reinforcement ratio is less than 2wt.%, the strengthening effect is not obvious.

[0007] Furthermore, the chemical compositions of the FeCoNiAlTi high entropy alloy powder are, by mass fraction, Fe 28.7%, Co 31.9%, Ni 29.6%, Al 4.2% and Ti 5.6%.

[0008] Furthermore, after obtaining the composite material powder, the process further includes screening the composite material powder to obtain a powder with a particle size of 15 to 53 μm, and then baking the powder in a drying oven at 80° C. for 2 hours.

[0009] Furthermore, the stainless steel is 316 stainless steel.

[0010] Furthermore, the method for preparing a high-strength and high-hardness stainless steel-based composite material by selective laser melting specifically comprises the following steps:

[0011] The FeCoNiAlTi high entropy alloy powder and the 316L stainless steel powder are mixed in proportion to obtain a composite material powder;

[0012] Using 316 stainless steel as the substrate, the substrate was cleaned and sandblasted;

[0013] Put the composite material powder into the powder cylinder, install the sandblasted substrate in the forming cylinder, adjust the scraper position, spread the powder according to the powder amount of 150μm / layer, until the composite material powder covers the substrate, and close the hatch;

[0014] Construct a three-dimensional model of the stainless steel-based composite material to be prepared, import it into the slicing software, set the number of prints and their placement, and set the layer thickness, laser power, scanning speed, scanning path and scanning angle before slicing, then import it into the equipment software, close the equipment molding chamber and introduce argon gas for deoxygenation, turn on the laser, and start printing after the laser is stable;

[0015] After printing, the laser and argon gas are turned off and the mixture is cooled to room temperature to obtain a stainless steel-based composite material.

[0016] Furthermore, the deoxidation is performed until the oxygen concentration in the molding chamber is lower than 100 ppm.

[0017] Furthermore, the layer thickness is 30 μm / layer, the laser power is 180 W, the scanning angle is 67°, and the scanning path is strip-shaped.

[0018] Compared with the prior art, the present invention has the following advantages and technical effects:

[0019] The material of the present invention has excellent mechanical properties, and its tensile strength can reach 1262MPa and hardness can reach 5.4GPa, thereby solving the problem that 316L stainless steel prepared by the current traditional method is prone to failure under high-strength working conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0021] Figure 1 This is a scanning electron microscope image of the high entropy alloy powder in Example 1.

[0022] Figure 2 Schematic diagram of the working principle of the selective laser melting forming equipment used in Example 1, wherein: 1-galvanometer scanning system; 2-forming chamber (argon environment); 3-forming sample; 4-stainless steel substrate; 5-forming cylinder; 6-powder cylinder; 7-scraper; 8-scraper; 9-robotic arm; 10-laser transmitter; 11-high-energy laser beam.

[0023] Figure 3 This is a dimension diagram of the tensile specimen of the stainless steel composite material sample of Example 1.

[0024] Figure 4 This is the XRD diagram of the stainless steel composite material component with a reinforcement ratio of 2 wt.% prepared in Examples 1 to 3.

[0025] Figure 5 Statistical diagrams of tensile strength and hardness of the stainless steel composite material components prepared in Examples 1 to 3 and pure 316L stainless steel components prepared under the same process parameters, (a) is a hardness comparison diagram, and (b) is a tensile strength comparison diagram.

[0026] Figure 6 EBSD image of pure 316L stainless steel in Example 1;

[0027] Figure 7 EBSD image of the composite material in Example 1 (x=2wt.%). DETAILED DESCRIPTION

[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0029] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0031] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0032] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0033] The room temperature in the present invention refers to 25±2°C.

[0034] The chemical compositions of the FeCoNiAlTi high entropy alloy powder in the embodiment of the present invention are, by mass fraction, respectively Fe28.7%, Co31.9%, Ni29.6%, Al4.2% and Ti5.6%, which are purchased from Ningbo Zhongyuan New Materials Co., Ltd.

[0035] Example 1

[0036] The preparation of the stainless steel composite material comprises the following steps:

[0037] (1) FeCoNiAlTi high entropy alloy powder was mixed with 316L stainless steel powder with a reinforcement ratio of x wt.% (x=2, 5, 10) to obtain a composite material powder.

[0038] The mixed composite material powder has good sphericity and the powder morphology is as follows Figure 1 As shown, some small particles of "satellite" particle powder are adhered to or surrounded by its surface.

[0039] (2) The composite material powder obtained in step (1) is sieved through 300 mesh and 1000 mesh sieves to ensure that the powder particle size used in the printing process is between 15 and 53 μm. After the sieving is completed, the sieved powder is placed in a glass container, which is placed in an oven and baked at 80° C. for 2 hours.

[0040] (3) The HBD-100 printer from Hanbang Laser Technology Co., Ltd. is used. Its working principle is as follows Figure 2 As shown. Set the powder layer thickness to 30μm / layer, the scanning speed to 650mm / s, the laser power to 180W, the scanning angle to 67°, and the scanning path to strip shape. Slice after the settings are completed.

[0041] (4) Figure 2 As shown, the stainless steel substrate 4 used for molding is cleaned with alcohol to remove surface impurities, and then sandblasted after being blown dry. It is then installed and fixed on the molding cylinder 5 and leveled to ensure that the substrate and the platform in the cavity are in the same plane. An appropriate amount of powder 7 dried in step (2) is added to the powder cylinder 6, the position of the scraper 8 is adjusted, and the powder spreading operation is performed multiple times according to the powder amount of 150μm / layer until the powder completely covers the entire substrate.

[0042] (5) Import the slicing software program into the corresponding software of the device, close the molding chamber 2 and introduce protective gas argon for deoxygenation treatment so that the oxygen concentration in the molding chamber is lower than 100 ppm, turn on the laser emitter 10, wait for the laser to stabilize, and then start printing.

[0043] During the printing process, the scraper evenly spreads the metal powder in the powder cylinder on the molding substrate, and the laser emitter emits a high-energy laser beam 11. The laser selectively melts the metal powder on the substrate through the galvanometer scanning system 1 according to the pre-set parameters. Every time the molding cylinder decreases a printing layer thickness, the powder cylinder rises a printing layer thickness, so that the mechanical arm 9 drives the scraper 8 to spread a printing layer thickness of metal powder on the molding platform. The above operations are repeated in this way, and finally the desired molding sample 3 can be prepared.

[0044] (6) After the printing is completed, turn off the laser and argon gas, and cool for more than 30 minutes to ensure that the powder in the molding cylinder is completely cooled to room temperature. Open the cabin door, raise the molding cylinder to the limit through the equipment control system, and sweep the excess powder into the recovery cabin in the equipment with a brush. Use a vacuum cleaner to suck away the excess powder in the equipment, remove the substrate, and separate the sample on the substrate from the matrix by wire cutting to obtain the stainless steel composite material.

[0045] Embodiment 2-3

[0046] The difference between Examples 2 to 3 and Example 1 is that the scanning speeds in step (3) are different. The scanning speeds of Examples 2 and 3 are 800 mm / s and 1000 mm / s, respectively.

[0047] Comparative Example 1

[0048] The same as Example 1, except that the scanning speed in step (3) is 200 mm / s. The scanning speed determines the length of time the high-energy laser beam acts on the powder. When the scanning speed is too low, the laser acts on the powder for too long and the laser energy density is too high, causing the molten pool to splash, affecting the sintering size, and increasing the deformation and spheroidization tendency of the formed part. Therefore, no subsequent performance test was performed.

[0049] Comparative Example 2

[0050] The same as Example 1, except that the scanning speed in step (3) is 1500 mm / s. When the scanning speed is too high, the powder sintering reaction is insufficient, resulting in poor bonding effect, and also aggravating the instability of the molten pool, resulting in an increase in defects. Therefore, no subsequent performance test was performed.

[0051] Comparative Example 3

[0052] Same as Example 1, except that the enhancement ratio of the FeCoNiAlTi high entropy alloy powder to the stainless steel powder is 20wt%.

[0053] Comparative Example 4

[0054] Same as Example 1, except that the enhancement ratio of the FeCoNiAlTi high entropy alloy powder to the stainless steel powder is 15wt%.

[0055] The melting point of FeCoNiAlTi high entropy alloy is much higher than that of 316L stainless steel, and it requires more energy to melt. The more reinforcing phase is added to the composite material, the more energy is required. Therefore, under the same forming parameters, the composite material with a high reinforcing phase content cannot receive enough energy, resulting in more defects (such as Comparative Examples 3 and 4), such as unmelted particles. On the contrary, if too few reinforcing particles are added, the closer its composition is to pure 316L stainless steel, and there will be no significant difference in the mechanical properties tested, such as Figure 5 It is shown that the tensile strength and hardness are inversely proportional to the number of defects in the sample, that is, the more defects there are, the worse the mechanical properties are. The mechanical properties of the composite material are about twice that of pure stainless steel.

[0056] Effect verification

[0057] The 5 mm thick stainless steel composite block samples obtained in Examples 1 to 3 and printed were coarsely ground with #400, #800, and #1500 sandpapers in turn. The phase composition was analyzed by X-ray diffraction analysis. The X-ray diffraction related parameters included: working voltage of 40KV, measurement range of 10° to 90°, and scanning speed of 2° / min. The test results are shown in Figure 2. Figure 4 shown.

[0058] The sample surface was then polished. The polished sample was ultrasonically cleaned with alcohol, and then the hardness of the sample was tested using a German Bruker Hysitron T1980 nanoindentation device. The maximum load of the nanoindentation was 5mN, the loading rate was 1mN / s, and the holding time was 2s. The test results showed that the hardness of the stainless steel composite materials prepared in Examples 1 to 3 was greater than 4GPa. Figure 5 As shown in (a).

[0059] The 1mm thick stainless steel composite tensile specimens printed in Examples 1 to 3 were polished with #400, #800, and #1500 sandpapers in turn. The tensile properties of the samples were then tested using a CMT-5205 microcomputer-controlled electronic testing machine. The experimental conditions were as follows: room temperature, preload 30kN, and tensile rate 1mm / min. The block specimen size of each example and comparative example was 15mm*10mm*5mm. The size of the stainless steel composite tensile specimen of Example 1 was as follows: Figure 3 The test results show that the tensile strength of the stainless steel composite materials prepared in Examples 1 to 3 is greater than 1000 MPa. Figure 5 As shown in (b).

[0060] The EBSD image of pure 316L stainless steel in Example 1 is shown in Figure 6 , the EBSD image of the composite material (x = 2wt.%) in Example 1 is shown in Figure 7 It can be seen that after compounding, the columnar crystals transform into cellular crystals, and the grain size is greatly reduced.

[0061] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing high-strength and high-hardness stainless steel-based composite materials by selective laser melting. It is characterized in that The method comprises the following steps: mixing FeCoNiAlTi high entropy alloy powder with stainless steel powder to obtain composite material powder, and performing laser printing by using a selective laser melting technology to obtain a stainless steel-based composite material; The scanning speed of the laser printing is 650 mm / s~1000 mm / s; The FeCoNiAlTi high entropy alloy powder is mixed with the stainless steel powder according to a reinforcement ratio of x wt.%, wherein x=2-10; The chemical compositions of the FeCoNiAlTi high entropy alloy powder are, by mass fraction, Fe28.7%, Co31.9%, Ni29.6%, Al4.2% and Ti5.6% respectively; The stainless steel is 316 stainless steel; During laser printing, the layer thickness is 30 μm / layer, the laser power is 180 W, the scanning angle is 67°, and the scanning path is strip-shaped; The hardness of the stainless steel-based composite material is greater than 4 GPa, and the tensile strength is greater than 1000 MPa.

2. A method for preparing a high-strength and high-hardness stainless steel-based composite material by selective laser melting according to claim 1, It is characterized in that After obtaining the composite material powder, the method further includes screening the composite material powder to obtain a powder with a particle size of 15 to 53 μm, and then baking the powder.

3. According to the method for preparing high-strength and high-hardness stainless steel-based composite materials by selective laser melting according to claim 1, It is characterized in that The specific steps include: The FeCoNiAlTi high entropy alloy powder and the 316L stainless steel powder are mixed in proportion to obtain a composite material powder; Using 316 stainless steel as the substrate, the substrate was cleaned and sandblasted; Put the composite material powder into the powder cylinder, install the sandblasted substrate in the forming cylinder, adjust the scraper position, spread the powder according to the powder amount of 150μm / layer, until the composite material powder covers the substrate, and close the hatch; Construct a three-dimensional model of the stainless steel-based composite material to be prepared, import it into the slicing software, set the number of prints and their placement, and set the layer thickness, laser power, scanning speed, scanning path and scanning angle before slicing, then import it into the equipment software, close the equipment molding chamber and introduce argon gas for deoxygenation, turn on the laser, and start printing after the laser is stable; After printing, the laser and argon gas are turned off and the mixture is cooled to room temperature to obtain a stainless steel-based composite material.

4. A method for preparing a high-strength and high-hardness stainless steel-based composite material by selective laser melting according to claim 3, It is characterized in that The deoxidation is performed until the oxygen concentration in the molding chamber is lower than 100 ppm.