A kind of high-purity ammonium metavanadate and preparation method thereof

By dissolving vanadium oxide in dilute acid and adding oxidant, the preparation process of high-purity ammonium metavanadate is simplified, solving the problems of complex process, long process and large amount of waste water, and achieving high purity, low impurities and high The effect of vanadium yield is suitable for industrial applications.

CN116040680BActive Publication Date: 2024-10-11DALIAN RONGKE ENERGY STORAGE GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211697180.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-10-11
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

The preparation process of traditional high-purity ammonium metavanadate is complicated, the process is long, the vanadium yield is low, the output is low, and the wastewater is large, making it difficult to meet the needs of industrialization.

Method used

Dissolve vanadium oxide in dilute sulfuric acid or dilute hydrochloric acid, adjust the pH value and add oxidant. High-purity ammonium metavanadate is generated through the oxidation process, simplifying the process and increasing vanadium yield and output.

Benefits of technology

It achieves rapid and effective preparation of high-purity ammonium metavanadate, reduces preparation costs and wastewater volume, is suitable for industrial promotion, and provides raw materials for high-purity vanadium and vanadium ion battery materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116040680B_ABST
    Figure CN116040680B_ABST
Patent Text Reader

Abstract

The present invention provides a high-purity ammonium metavanadate and a preparation method thereof, wherein the preparation method of the high-purity ammonium metavanadate comprises the following steps: step 1: adding vanadium oxide to dilute sulfuric acid and / or dilute hydrochloric acid, stirring and heating to 60-95°C; step 2: after the vanadium oxide is completely dissolved, cooling the solution to 20-50°C, adding ammonia water to the solution, and adjusting the solution pH to 7-9; step 3: adding an oxidant to the solution for oxidation, supplementing ammonia water during the oxidation process to keep the solution pH to 7-9, and stirring the solution to react for 1 hour until the solution turns light yellow or colorless, and filtering to obtain high-purity ammonium metavanadate. The method has the advantages of simple process, short flow, high vanadium yield and high output; the high-purity ammonium metavanadate prepared by the present invention has high purity, and each impurity element is less than 30ppm, and can be used for the production of high-purity vanadium, vanadium ion batteries, yttrium vanadate and other materials, providing a choice of raw materials for cutting-edge vanadium materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to ammonium metavanadate technology, in particular to high-purity ammonium metavanadate and a preparation method thereof. Background Art

[0002] Chinese patent CN103708553A discloses a method for improving the quality of industrial ammonium metavanadate, the main process includes: dissolving industrial ammonium metavanadate in 2-10wt% ammonia water at room temperature, adding ammonium sulfate while stirring, and passing the obtained feed solution through a strong alkaline anion exchange resin at a rate of 2-4 times column volume / hour, and the obtained feed solution is warmed to 40-60°C, adding ammonium chloride, stirring until the ammonium chloride is dissolved, cooling to 0-5°C, and the precipitated crystals are filtered, washed, and ventilated and dried under the conditions of 20-30°C to obtain ammonium metavanadate with improved quality. The above technical scheme has the following problems: 1. Ammonia water is used to dissolve ammonium metavanadate and the solution is a strong alkaline condition, ammonia in the solution will continue to volatilize, the operating environment is harsh, and the feed solution is warmed to 40-60°C, and ammonia water will also continue to decompose into ammonia; 2. The technical scheme adds ammonium sulfate and ammonium chloride respectively during the purification process, and a large amount of sulfate and chloride ions will remain in the wastewater, which is highly corrosive.

[0003] Chinese patent CN109437299A discloses a method for purifying industrial-grade ammonium metavanadate, the main process of which includes: heating industrial-grade ammonium metavanadate to dissolve in water, adding ammonium sulfide for sulfidation for a certain period of time, adjusting the pH value of the solution to 3.0-3.5, reacting for 20-50 minutes, filtering to obtain filtrate No. 1; heating filtrate No. 1, adding a certain amount of ferrous salt to reduce high-valent chromium, reacting for 20-120 minutes, adding phosphate, adjusting the pH value of the solution to 7.5-8.0, reacting for 20-40 minutes, filtering to obtain filtrate No. 2; heating filtrate No. 2, adding hydrogen peroxide, and removing the residual Fe 2+ , react for 20-40 minutes, then add a certain amount of aluminum salt, adjust the pH value of the solution to 7.5-8.0, react for 40-150 minutes, and filter to obtain filtrate No. 3; filtrate No. 3 is crystallized at medium temperature, washed, and dried to obtain a high-purity ammonium metavanadate product. The above technical scheme has the following problems: 1. The process is complicated and the process is long, which is not suitable for wide application. 2. The purification process introduces more auxiliary materials, such as ammonium sulfide, ferrous salts, phosphates, hydrogen peroxide and aluminum salts, and the auxiliary materials will have a certain amount of residue, affecting the purity of ammonium metavanadate. 3. The impurity removal process of ferrous salts, phosphates and aluminum salts will produce solid precipitates, which will carry a large amount of vanadium and affect the yield of vanadium.

[0004] The cooling crystallization method produces high-purity AMV. This method uses hot water to completely dissolve the AMV, and then adds ammonium salt to crystallize the AMV after cooling. This method has the disadvantages of low yield and large amount of wastewater.

[0005] The traditional production methods of high-purity AMV have problems to varying degrees, such as complex process, long process, low vanadium yield, low output and large amount of wastewater. There is an urgent need for a fast and efficient method for preparing high-purity ammonium metavanadate. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing high-purity ammonium metavanadate in view of the problems of complex preparation process, long process, low vanadium yield, low output and large amount of wastewater in traditional ammonium metavanadate preparation. The method has the advantages of simple process, short process, high vanadium yield and large output. The high-purity ammonium metavanadate prepared by the present invention has high purity, and each impurity element is less than 30ppm. The high-purity ammonium metavanadate can be used for the production of high-purity vanadium, vanadium ion batteries, yttrium vanadate and other materials, and provides a raw material selection for cutting-edge vanadium materials.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing high-purity ammonium metavanadate (AMV), comprising the following steps:

[0008] Step 1: Add vanadium oxide to dilute sulfuric acid and / or dilute hydrochloric acid, stir and heat to 60-95° C.;

[0009] Step 2: After the vanadium oxide is completely dissolved, the solution is cooled to 20-50° C., and ammonia water is added to the solution to adjust the solution pH to 7-9;

[0010] Step 3: Add an oxidant to the solution for oxidation. During the oxidation process, add ammonia water to keep the pH of the solution at 7-9. When the solution turns light yellow or colorless, stir the reaction for 1-2 hours, filter and wash to obtain high-purity ammonium metavanadate.

[0011] Furthermore, the total concentration of the dilute sulfuric acid and the dilute hydrochloric acid in step 1 is 1.6 to 2 mol / L, preferably 1.8 to 2 mol / L.

[0012] Furthermore, the vanadium oxide in step 1 is a mixture of one or more of vanadium pentoxide, vanadium tetroxide, vanadium trioxide and vanadium dioxide.

[0013] Furthermore, the amount of vanadium oxide added in step 1 satisfies the following condition: the sum of Cl ions and S ions: V=1-1.2 (molar ratio).

[0014] Furthermore, step 1 is stirred and heated to 80°C to 95°C.

[0015] Furthermore, in step 2, the solution is cooled to 30-40°C.

[0016] Furthermore, the concentration of aqueous ammonia in step 2 is 13-20%wt.

[0017] Furthermore, in step 2, the solution pH is adjusted to 8-9.

[0018] Furthermore, the oxidant in step 3 is a mixture of one or more of hydrogen peroxide, peracetic acid, sodium dichromate, potassium permanganate, sodium persulfate, ammonium persulfate, sodium hypochlorite, sodium perborate, potassium perborate, oxygen and chlorine.

[0019] Furthermore, the amount of the oxidant added in step 3 is 80 to 120 g / L, preferably 100 to 120 g / L.

[0020] Furthermore, the stirring reaction time in step 3 is 1 to 1.5 hours.

[0021] Furthermore, in step 3, ammonia water is added during the oxidation process to maintain the solution pH at 8-9.

[0022] The reaction principle of the present invention is as follows: vanadium oxide is dissolved with sulfuric acid and / or hydrochloric acid to become low-valent vanadium ions; ammonia water is added to react with the low-valent vanadium ions to form vanadium hydroxide precipitate; under alkaline conditions and under the oxidizing action of an oxidant, the vanadium hydroxide precipitate gradually dissolves and becomes soluble metavanadate ions VO3 - , VO3 - With NH4 in solution + Combined to generate high-purity NH4VO3 ammonium metavanadate solid.

[0023] Another object of the present invention is to disclose high-purity ammonium metavanadate, which is prepared by the above method.

[0024] Furthermore, the content of each impurity element in the high-purity ammonium metavanadate is less than 30 ppm, and the total impurity content is less than 200 ppm.

[0025] The invention discloses a method for preparing high-purity ammonium metavanadate AMV, which has the following advantages compared with the prior art: the ammonium metavanadate prepared by the method has extremely high purity, and compared with the conventional cooling crystallization method, the method has large output, small amount of waste water, high purity of AMV, and low impurity content. Compared with the traditional alkali dissolution method, no sodium salt-containing waste water is generated, the influence of sodium salt can be eliminated, the amount of washing water is small, the purity of AMV is high, and the impurity content is low.

[0026] 1) The present invention uses acid-soluble vanadium oxide, which is different from the conventional preparation method of high-purity vanadium. The method of alkali dissolution and adding ammonium salt is not used, so the preparation cost of high-purity ammonium metavanadate is greatly reduced, and no alkali metal ion wastewater is generated, and the amount of washing water is greatly reduced.

[0027] 2) The preparation process of the high-purity ammonium metavanadate of the present invention is simple, the process is short, and it is suitable for industrial promotion;

[0028] 3) The impurity elements in the high-purity metavanadic acid prepared by the present invention are all lower than 30 ppm, and can be used for the production of high-purity vanadium, vanadium ion batteries, yttrium vanadate and other materials, providing a raw material option for cutting-edge vanadium materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Picture 1 The present invention is a flow chart of the preparation method of high-purity ammonium metavanadate. DETAILED DESCRIPTION

[0030] The present invention is further described below in conjunction with embodiments:

[0031] Example 1

[0032] This embodiment discloses a high-purity ammonium metavanadate and a preparation method thereof, comprising the following steps:

[0033] Step 1: Dilute sulfuric acid to 2 mol / L with water, add 60 g vanadium tetroxide and 12 g vanadium trioxide to 500 mL of dilute sulfuric acid, stir and heat to 85 °C;

[0034] Step 2: After the vanadium oxide is completely dissolved, the solution is cooled to 30°C, 350 ml of 16% ammonia water is added to the solution, and the pH value of the solution is adjusted to 8.0;

[0035] Step 3: Add 50 g of 25% hydrogen peroxide to the solution for oxidation. During the oxidation process, add ammonia water to keep the solution pH = 8.0. When the solution turns light yellow, stir and react for 1 hour, filter and wash to obtain high-purity AMV.

[0036] Table 1. Summary of impurity element detection data of high-purity AMV

[0037] name <![CDATA[V2O5(%)]]> K(%) Na(%) Fe(%) Al(%) Mo(%) Cr(%) Ca(%) Mg(%) Si(%) Ni(%) AMV 77.75 0.0002 0.0002 0.0021 0.0021 0.0003 0.0003 0.0019 0.0003 0.0017 0

[0038] As shown in Table 1, the impurities of the high-purity AMV prepared in this embodiment are all less than 25ppm, and the purity is extremely high. The concentration of V2O5 in the mother liquor is 0.8g / L, the vanadium yield is 99.50%, and the single vanadium precipitation AMV output is 102.45g (dry basis). The V2O5 (%) in the table of the present invention are all converted contents.

[0039] Example 2

[0040] This embodiment discloses a high-purity ammonium metavanadate and a preparation method thereof, comprising the following steps:

[0041] Step 1: Dilute hydrochloric acid to 2 mol / L with water, add 60 g vanadium trioxide and 10 g vanadium pentoxide to a volume of 500 mL, stir and heat to 95°C;

[0042] Step 2: After the vanadium oxide is completely dissolved, the solution is cooled to 40°C, 400 ml of 16% ammonia water is added to the solution, and the pH value of the solution is adjusted to 8.2;

[0043] Step 3: Add 60 g of sodium persulfate to the solution for oxidation. During the oxidation process, add ammonia water to keep the solution pH = 8.2. When the solution turns light yellow, stir the reaction for 1 hour, filter and wash to obtain high-purity AMV.

[0044] Table 2. Summary of impurity element detection data of high-purity AMV

[0045] name <![CDATA[V2O5(%)]]> K(%) Na(%) Fe(%) Al(%) Mo(%) Cr(%) Ca(%) Mg(%) Si(%) Ni(%) AMV 77.76 0.0010 0.0011 0.0009 0.0020 0.0006 0.0003 0.0028 0.0005 0.0018 0

[0046] As shown in Table 2, the impurities of the high-purity AMV prepared in this embodiment are all less than 28 ppm, and the purity is extremely high. The concentration of V2O5 in the mother liquor is 0.92 g / L, the vanadium yield is 99.44%, and the single vanadium precipitation AMV yield is 105.21 g (dry basis).

[0047] Example 3

[0048] This embodiment discloses a high-purity ammonium metavanadate and a preparation method thereof, comprising the following steps:

[0049] Step 1: Dilute sulfuric acid to 1.9 mol / L with water, add 75 g of vanadium dioxide to 500 mL of dilute sulfuric acid, and stir to raise the temperature to 80 °C;

[0050] Step 2: After the vanadium dioxide is completely dissolved, the solution is cooled to 30°C, 390 ml of 15% ammonia water is added to the solution, and the pH value of the solution is adjusted to 7.8;

[0051] Step 3: Add 60 g of ammonium persulfate to the solution for oxidation. During the oxidation process, add ammonia water to keep the solution pH = 8.2. When the solution becomes colorless, stir the reaction for 1 hour, filter and wash to obtain high-purity AMV.

[0052] Table 3. Summary of impurity element detection data of high-purity AMV

[0053] name <![CDATA[V2O5(%)]]> K(%) Na(%) Fe(%) Al(%) Mo(%) Cr(%) Ca(%) Mg(%) Si(%) Ni(%) AMV 77.76 0.0006 0.0002 0.0023 0.0015 0.0006 0.0002 0.0020 0.0004 0.0014 0

[0054] As shown in Table 3, the impurities of the high-purity AMV prepared in this embodiment do not exceed 23 ppm, and the purity is extremely high. The concentration of V2O5 in the mother liquor is 0.63 g / L, the vanadium yield is 99.61%, and the single vanadium precipitation AMV yield is 105.08 g (dry basis).

[0055] Comparative Example 1

[0056] This comparative example discloses a method for preparing AMV, comprising the following steps:

[0057] Step 1: Add 26 g AMV to 500 mL tap water, stir and heat to 98°C until AMV is completely dissolved;

[0058] Step 2: Cool the solution to 50°C and add 20 g of ammonium sulfate solid to the solution;

[0059] Step 3: Add ammonia water to keep the solution pH = 8.0, stir the reaction for 1 hour, filter and wash to obtain high-purity AMV, the mother liquor V2O5 concentration is 2.5 g / L, the vanadium yield is 93.80%, and the single vanadium precipitation AMV yield is 24.40 g (dry basis).

[0060] Note: The solubility of AMV in water increases with increasing temperature. The maximum solubility of AMV in 98°C hot water is 52g / L. If too much AMV is added, the solution will be oversaturated and AMV cannot be completely dissolved, which will eventually affect the impurity content of AMV.

[0061] Table 4. Summary of AMV impurity element detection data

[0062] name <![CDATA[V2O5(%)]]> K(%) Na(%) Fe(%) Al(%) Mo(%) Cr(%) Ca(%) Mg(%) Si(%) Ni(%) AMV 77.52 0.0015 0.0012 0.0006 0.0030 0.0032 0.0012 0.0050 0.0009 0.0114 0.0005

[0063] As shown in Table 4, the single impurity content in the AMV prepared in this comparative example is as high as 114 ppm, and the purity is relatively low. The vanadium yield is only 93.80%, and the single vanadium precipitation AMV output is 24.40 g (dry basis). Compared with Examples 1-3, the single production capacity of the cooling crystallization process in this comparative example is only 1 / 4 of that of Examples 1-3, and the purity is not as good as that of Examples 1-3.

[0064] Comparative Example 2

[0065] This comparative example discloses a method for preparing AMV, comprising the following steps:

[0066] Step 1: Add 103 g AMV to 2000 mL tap water, stir and heat to 98°C until AMV is completely dissolved;

[0067] Step 2: Cool the solution to 50°C and add 79 g of ammonium sulfate solid to the solution;

[0068] Step 3: Add ammonia water to keep the solution pH = 8.0, stir the reaction for 1 hour, filter and wash to obtain high-purity AMV, the mother liquor V2O5 concentration is 2.3 g / L, the vanadium yield is 94.24%, and the single vanadium precipitation AMV output is 97.06 g (dry basis).

[0069] Note: The solubility of AMV in water increases with increasing temperature. The maximum solubility of AMV in 98°C hot water is 52 g / L. To increase the amount of AMV added to the same mass as V2O5 in Example 1-3, the volume of tap water needs to be increased from 500 mL to 2000 mL. It can be seen that to produce the same mass of AMV, this solution requires more energy consumption and generates more wastewater.

[0070] Table 5. Summary of AMV impurity element detection data

[0071] name <![CDATA[V2O5(%)]]> K(%) Na(%) Fe(%) Al(%) Mo(%) Cr(%) Ca(%) Mg(%) Si(%) Ni(%) AMV 77.53 0.0014 0.0010 0.0005 0.0035 0.0025 0.0015 0.0046 0.0012 0.0120 0.0005

[0072] As shown in Table 5, the single impurity content in the AMV prepared in this comparative example is as high as 120ppm, and the purity is relatively low. The vanadium yield is only 94.24%. Although the single vanadium precipitation AMV yield is 97.06g (dry basis), which is close to Example 1-3, the water volume of this group is 4 times that of Example 1-3, and the corresponding wastewater output is also relatively large. And the purity is not as good as Example 1-3.

[0073] Comparative Example 3

[0074] This comparative example discloses a method for preparing AMV, comprising the following steps:

[0075] Step 1: Add 52 g AMV to 500 mL tap water, add 20 g sodium hydroxide, stir and heat to 60°C until AMV is completely dissolved and the solution pH = 9.3;

[0076] Step 2: Cool the solution to 40°C and add 60 g of ammonium sulfate solid to the solution;

[0077] Step 3: Add ammonia water to keep the solution pH = 8.0, stir the reaction for 1 hour, filter and wash multiple times to obtain high-purity AMV, the mother liquor V2O5 concentration is 2.8 g / L, the vanadium yield is 96.53%, and the single vanadium precipitation AMV yield is 50.19 g (dry basis).

[0078] Note: Compared with hot water soluble AMV, although adding sodium hydroxide can increase the solubility of AMV, it will introduce sodium ions, which will not only affect the particle size and purity of AMV, but also increase the number of washing times and the amount of wastewater.

[0079] Table 6. Summary of AMV impurity element detection data

[0080] name <![CDATA[V2O5(%)]]> K(%) Na(%) Fe(%) Al(%) Mo(%) Cr(%) Ca(%) Mg(%) Si(%) Ni(%) AMV 77.52 0.0025 0.0050 0.0012 0.0063 0.0032 0.0015 0.0050 0.0009 0.0142 0.0006

[0081] As shown in Table 6, the single impurity content in the AMV prepared in this comparative example is as high as 142ppm, and the purity is relatively low. The vanadium yield is only 96.53%, and the single vanadium precipitation AMV output is 50.19g (dry basis). Compared with Example 1-3, the single production capacity of the alkaline dissolution vanadium precipitation process is only 1 / 2 of that of Example 1-3, and the purity is not as good as that of Example 1-3.

[0082] Comparative Example 4

[0083] This comparative example discloses a method for preparing AMV, comprising the following steps:

[0084] Step 1: Add 104 g AMV to 500 mL tap water, add 40 g sodium hydroxide, stir and heat to 60°C until AMV is completely dissolved and the solution pH = 9.3;

[0085] Step 2: Cool the solution to 40°C and add 120 g of ammonium sulfate solid to the solution;

[0086] Step 3: Add ammonia water to keep the solution pH = 8.0, stir the reaction for 1 hour, filter, and wash with a large amount of water for multiple times to obtain high-purity AMV. The mother liquor V2O5 concentration is 3.2 g / L, the vanadium yield is 98.01%, and the single vanadium precipitation AMV output is 101.94 g (dry basis).

[0087] Note: Although increasing the amount of sodium hydroxide can increase the solubility of AMV and double the vanadium concentration of the solution, the sodium ion concentration of the solution will also double, and the amount of ammonium sulfate used for vanadium precipitation will also double, which will not only affect the particle size and purity of AMV, but also increase the amount of wash water, the amount of wastewater, and the concentration of sodium sulfate in the wastewater.

[0088] Table 7. Summary of AMV impurity element detection data

[0089] name <![CDATA[V2O5(%)]]> K(%) Na(%) Fe(%) Al(%) Mo(%) Cr(%) Ca(%) Mg(%) Si(%) Ni(%) AMV 77.42 0.0062 0.0153 0.0030 0.0120 0.0063 0.0035 0.0068 0.0021 0.0325 0.0015

[0090] As shown in Table 7, the single impurity content in the AMV prepared in this control example is as high as 325ppm, and the purity is relatively low. The vanadium yield is only 98.01%, and the single vanadium precipitation AMV output is 101.94g (dry basis), which is close to Example 1-3. Due to the high vanadium concentration and sodium concentration of the solution, the prepared AMV has a small particle size, and the impurity ions entrained in the AMV are extremely difficult to wash. After multiple washings, the impurity content in the AMV is still relatively high, and the amount of wastewater from washing the AMV in this group is large, and the wastewater contains a large amount of sodium ions. Although the single production capacity of this group of alkaline vanadium precipitation processes reaches Example 1-3, the purity is far less than that of Example 1-3, and the amount of wastewater is large, and the sodium ion concentration in the wastewater is high.

[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing high-purity ammonium metavanadate, It is characterized in that The following steps are involved: Step 1: Add vanadium oxide to dilute sulfuric acid and / or dilute hydrochloric acid, stir and heat to 60-95°C; Step 2: After the vanadium oxide is completely dissolved, the solution is cooled to 20-50°C, and ammonia water is added to the solution. The concentration of ammonia water is 13-20 wt %, and the pH value of the solution is adjusted to 7-9; Step 3: Add an oxidant to the solution for oxidation. During the oxidation process, add ammonia water to keep the pH of the solution at 7-9. When the solution turns light yellow or colorless, stir the reaction for 1-2 hours, filter and wash to obtain high-purity ammonium metavanadate. The oxidant is a mixture of one or more of hydrogen peroxide, peracetic acid, sodium dichromate, potassium permanganate, sodium persulfate, sodium hypochlorite, sodium perborate, potassium perborate, oxygen and chlorine; The amount of the oxidant added is 80-120 g / L; The content of each impurity element in the high-purity ammonium metavanadate is lower than 30 ppm, and the total impurity content is lower than 200 ppm.

2. The method for preparing high-purity ammonium metavanadate according to claim 1, It is characterized in that The total concentration of the dilute sulfuric acid and dilute hydrochloric acid in step 1 is 1.6-2 mol / L.

3. The method for preparing high-purity ammonium metavanadate according to claim 1, It is characterized in that The vanadium oxide in step 1 is a mixture of one or more of vanadium pentoxide, vanadium tetroxide, vanadium trioxide and vanadium dioxide.