A method for increasing the heat of slag and iron in the initial stage of long-term wind-restoration in a copper-cooled stave blast furnace

By adjusting the rest air mass coke ratio, adding air coke and adjusting the cooling water volume and adding air rhythm, the problem of low slag iron heat in the early stage of resuscitation of copper cooling wall blast furnace is solved, efficient furnace condition recovery is achieved, and fuel consumption and carbon are reduced emission.

CN116103455BActive Publication Date: 2024-11-01SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310024595.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-09
Publication Date
2024-11-01
Estimated Expiration
2043-01-09

AI Technical Summary

Technical Problem

The copper-cooled wall blast furnace has low heat in the early stage of resuscitation after long-term restoration, which leads to difficulty in recovering the furnace condition and increases fuel consumption and carbon emissions.

Method used

By adjusting the rest air mass coke ratio, adding air coke, adjusting the cooling water volume and air-adding rhythm, the heat of slag iron in the early stage of resumption of air is increased and the furnace recovery time is shortened.

Benefits of technology

The slag iron temperature in the early stage of re-refrigeration of copper-cooled wall blast furnace was successfully increased, which shortened the air supply recovery time, reduced coke consumption and output losses, and improved the furnace condition recovery efficiency and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116103455B_ABST
    Figure CN116103455B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of blast furnace ironmaking, and is a method for increasing the heat of slag iron in the initial stage of long-term wind stop and wind rewinding of a copper cooling stave blast furnace, comprising the following steps: 1) increasing the coke ratio by 10-15 kg / t in two smelting cycles before the blast furnace is stopped; 2) determining the basic coke ratio of the wind stop material according to the length of the wind stop time; 3) adding empty coke according to the length of the wind stop time; 4) adjusting the cooling stave cooling water flow rate to 1.0 m / s and the furnace bottom water cooling pipe water flow rate to 0.6-0.7 m / s 6-8 hours after the wind stop; 5) rapidly adding air after wind rewinding, so that the air supply ratio reaches 0.5, that is, the air volume / furnace capacity reaches 0.5; 6) after taking steps 1) to 5), the slag iron temperature in the furnace cylinder is increased from 1300-1350° C. to 1400-1450° C., reaching a temperature above which the slag iron can flow freely, so that the heat of the slag iron in the copper cooling stave blast furnace is rapidly increased after long-term wind stop and wind rewinding, and the furnace condition is restored. The present invention significantly reduces the coke consumption and basically solves the problem of difficulty in air supply recovery that has long plagued copper cooling stave blast furnaces.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of blast furnace ironmaking, and in particular to a method for increasing the heat of slag and iron in the initial stage of long-term wind-stopping and wind-reopening of a copper-cooling stave blast furnace. Background Art

[0002] At present, copper cooling staves are usually used in the design and construction of medium and large blast furnaces from the furnace belly to the lower part of the furnace body. Copper cooling staves have the advantages of high thermal conductivity, good thermal shock resistance and heat flow shock resistance, which makes it easy to form protective slag skin on the hot surface of copper cooling staves during blast furnace production. However, once the slag skin falls off in a large area, it will also lead to low furnace temperature and even furnace cooling accidents.

[0003] Blast furnaces usually need to be overhauled after 3 to 4 months of operation, with a 16 to 48-hour shutdown. During the shutdown period, there is no coke burning in the furnace and no heat brought in by hot air, so the temperature in the furnace gradually decreases, especially for blast furnaces equipped with copper cooling staves. The high thermal conductivity of copper causes the heat in the furnace to dissipate quickly, and the furnace temperature further decreases. When the furnace is shut down for a long time, the low temperature of the furnace, the poor heat and fluidity of the slag iron, can easily cause abnormal airflow distribution during the recovery process, leading to material collapse, hanging material, pipeline formation and other malignant furnace conditions, affecting the recovery process and increasing fuel consumption.

[0004] Therefore, in order to achieve the goal of green and low-carbon metallurgy, the heat of slag and iron in the initial stage of resumption of the copper-cooled stave blast furnace after a long period of shutdown must be increased as much as possible to shorten the process of furnace recovery, thereby reducing fuel consumption and carbon emissions.

[0005] The method aims to provide a method for increasing the heat of slag and iron in the initial stage of rewinding of a copper-cooled stave blast furnace after a long-term shutdown. The method proposes adjusting the shutdown material-coke ratio, the empty coke position, the cooling water volume during the shutdown period, and the air-adding rhythm in the initial stage of rewinding according to different shutdown durations when the copper-cooled stave blast furnace is shut down for a long time, thereby significantly increasing the heat of slag and iron in the initial stage of rewinding, shortening the furnace condition recovery time, and reducing fuel consumption. Summary of the invention

[0006] The purpose of the present invention is to solve the above problems and provide a method for increasing the heat of slag and iron in the initial stage of long-term wind-down and wind-reopening of a copper-cooled stave blast furnace.

[0007] When the copper cooling stave blast furnace is shut down for a long time, the shut-down material-coke ratio, the empty coke position, the cooling water volume during the shut-down period, and the air-adding rhythm at the initial stage of re-blowing are adjusted according to different shut-down durations, thereby significantly increasing the heat of slag and iron at the initial stage of re-blowing, shortening the furnace condition recovery time, and reducing fuel consumption. The purpose of the present invention is achieved by:

[0008] A method for increasing the heat of slag and iron in the initial stage of long-term wind-down and rewinding of a copper cooling stave blast furnace, comprising the following steps: 1) increasing the coke ratio by 10-15 kg / t in the first two smelting cycles of the blast furnace wind-down; 2) determining the basic coke ratio of the wind-down material according to the wind-down time, and applying formula (1)

[0009] K 休风料 =K 正常料 +h 休风时长 ×1.5(1)

[0010] in:

[0011] K 休风料 ——Coke ratio of rest air material, kg / t;

[0012] K 正常料 ——Normal coke ratio, kg / t;

[0013] h 休风时长 ——Blow-off duration, h; by statistically analyzing the heat loss during the blow-off period and the heat deficit caused by the failure to inject coal after the blow-off, the basic coke ratio of the blow-off material in the whole furnace should be increased by 1.5 kg / t for every blow-off hour; the coke ratio charged in the smelting cycle before the blow-off is K 休风料 3) Add empty coke according to the length of the wind-break time, and add the amount of empty coke n 空焦 Calculated by formula (2);

[0014] n 空焦 =h 休风时间 / 16+0.5(2)

[0015] in:

[0016] n 空焦 ——Number of hollow coke in the resting material, rounded to the nearest integer, pieces;

[0017] h 休风时间 - the number of hours from the start of the planned wind break to the resumption of wind;

[0018] For long-term wind stop within 60 hours, hollow coke is added to the wind stop material;

[0019] After the last batch of normal materials are loaded and the furnace is shut down, the first group of empty coke is located at the upper part of the furnace belly; 4) After the shutdown, there is still direct reduction reaction of the charge in the blast furnace, and the molten slag will continue to drip into the furnace, so 6 to 8 hours after the shutdown, the cooling water flow rate of the cooling wall is adjusted to 1.0 m / s, and the water flow rate of the furnace bottom water cooling pipe is adjusted to 0.6 to 0.7 m / s; 5) After the wind is resumed, the air is added quickly to make the air supply ratio reach 0.5, that is, the air volume / furnace capacity reaches 0.5; 6) After taking steps 1) to 5), the slag temperature in the furnace hearth increases from 1300 to 1350°C to 1400 to 1450°C, reaching a temperature above which the slag can flow freely, so that the heat of the slag in the copper-cooled wall blast furnace is quickly increased after a long period of shutdown and resumption of wind, and the furnace condition is restored.

[0020] Step 3) The method of adding empty cokes in the medium- and long-term wind break is as follows: the wind break time is 8 hours, the number of empty cokes is 1, and the arrangement is (1C+x△)+y△; the wind break time is 12 hours, the number of empty cokes is 1, and the arrangement is (1C+x△)+(1C+x△)+y△; the wind break time is 24 hours, the number of empty cokes is 2, and the arrangement is (1C+x△)+(1C+x△)+y△; the wind break time is 36 hours, the number of empty cokes is 3, and the arrangement is (2C+x△)+(1C+x△)+y△; the wind break time is 48 hours, the number of empty cokes is 4, and the arrangement is (2C+x△)+(1C+x△)+(1C+x△)+y△; the wind break time is 60 hours, the number of empty cokes is 4, and the arrangement is (2C+x△)+(1C+x△)+(1C+x△)+y△;

[0021] x is the number of batches of normal material loaded after empty coke, calculated by formula (3);

[0022] x=(V 工作容积 ×0.85 / (1-η 压缩 )-V 空焦 ×n 空焦 ) / V 料批体积 / 8 (3)

[0023] in:

[0024] x——the number of batches of normal material loaded after empty coke, pieces;

[0025] V 工作容积 ——Blast furnace working volume, m 3 ;

[0026] η 压缩 ——Average compression rate of charge, 10% to 12%, 1000m 3 Blast furnace takes the lower limit, 4000m 3 The upper limit of the level blast furnace is taken;

[0027] V 空焦 ——The volume of a single empty focus, m 3 ;

[0028] n 空焦 ——Number of empty focal points, pieces;

[0029] V 料批体积 ——Volume of each batch of material, m 3 ;

[0030] y is the number of batches of material that need to be loaded after loading the last empty coke and x normal materials until the wind stops, calculated by formula (4);

[0031]

[0032] in:

[0033] Σx——the sum of the normal materials x loaded after each group of empty coke, pieces;

[0034] V 工作容积 ——Effective volume of blast furnace, m 3 ;

[0035] η 压缩 ——Average compression rate of charge, 10% to 12%, 1000m 3 Blast furnace takes the lower limit, 4000m 3 The upper limit of the level blast furnace is taken;

[0036] V 空焦 ——The volume of a single empty focus, m 3 ;

[0037] n 空焦 ——Number of empty focal points, pieces;

[0038] V 料批体积 ——Volume of each batch of material, m 3 .

[0039] Step 4) The specific adjustment rhythm is as follows: During normal production, the water flow rate of the furnace cylinder cooling wall is 2.7m / s, and the water flow rate of the furnace bottom water cooling pipe is 2.0m / s; 1 hour after the wind is stopped, the water flow rate of the furnace cylinder cooling wall is 2.10m / s, and the water flow rate of the furnace bottom water cooling pipe is 2.0m / s; 2 hours after the wind is stopped, the water flow rate of the furnace cylinder cooling wall is 1.80m / s, and the water flow rate of the furnace bottom water cooling pipe is 1.60m / s; 4 hours after the wind is stopped, the water flow rate of the furnace cylinder cooling wall is 1.40m / s, and the water flow rate of the furnace bottom water cooling pipe is 1.20m / s; 6 hours after the wind is stopped, the water flow rate of the furnace cylinder cooling wall is 1.00m / s, and the water flow rate of the furnace bottom water cooling pipe is 0.60m / s. The beneficial effects of the present invention are: 1. Taiyuan Iron and Steel Plant 1800m 3The blast furnace uses this method to increase the slag and iron temperature from 1300℃ to 1400℃ at the initial stage of re-airing during the long-term wind-down period of regular inspection, shorten the air supply recovery time from more than 24h to 10h, greatly reduce coke consumption, and basically solve the problem of difficulty in air supply recovery in copper cooling wall blast furnaces that has long plagued them. April 13, 2022 TISCO Ironmaking Plant 1800m 3 The blast furnace was shut down for 47 hours during scheduled inspection and resumed on April 15, with full wind restored after 10 hours. Compared with the previous shutdown of more than 40 hours, this reduced production losses by 1,000 tons, reduced coke consumption by 120 tons, and brought economic benefits of 1 million yuan.

[0040] 2. Copper cooling wall technology is widely used at home and abroad. The application of this patent can greatly shorten the recovery of blast furnaces and reduce the workload of employees. It has significant benefits in environmental protection, safety, greenness, low carbon, and high efficiency, and has strong promotion value. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The present invention will be further described below in conjunction with the accompanying drawings.

[0042] Figure 1 It is a position diagram of empty coke in a blast furnace according to the present invention.

[0043] Among them: 1. The third group is empty focus, 2. The second group is empty focus, 3. The first group is empty focus. DETAILED DESCRIPTION

[0044] The present invention adopts a basic technical concept: the copper-cooled stave blast furnace utilizes the high thermal conductivity of copper to quickly generate a slag skin with low thermal conductivity, which plays a role in protecting the cooling stave and regulating the airflow. In the past, when the wind was shut down for a long time, the furnace was often cleaned in advance, causing the slag skin attached to the copper cooling stave to fall off on a large scale, and then the furnace temperature was increased by a high fuel ratio to maintain the heat of the slag. The present invention adjusts the adhesion of the slag skin before the wind is shut down to avoid the slag skin from falling off, reduces heat loss during the wind shut-down, reduces the disturbance of the coal gas flow to the slag skin at the initial stage of the wind resumption, and at the same time replenishes heat as soon as possible to rapidly increase the heat of the slag iron at the initial stage of the wind resumption, thereby shortening the furnace condition recovery time.

[0045] The present invention proposes a method for increasing the heat of slag and iron in the initial stage of long-term wind-down and wind-reopening of a copper-cooled stave blast furnace, as follows: 1. According to the length of wind-down time of the blast furnace, the coke ratio is increased by 1.5×the number of wind-down hours kg / t in a smelting cycle before the wind-down. 2. According to the length of wind-down time, empty coke is added, and the number is (number of wind-down hours / 16+0.5), and the first empty coke is located in the middle and upper part of the furnace belly. 3. Within 6 to 8 hours after the wind-down, the cooling water volume is reduced, and the flow rate is controlled according to the cooling stave water flow rate of 1.0 m / s and the furnace bottom water cooling pipe water flow rate of 0.6 m / s to strengthen the adhesion of the slag skin. 4. After the wind-down, the air volume entering the furnace is increased by adding air in small amounts and multiple times to maintain the normal descent of the charge and eliminate the large-scale shedding of the slag skin.

[0046] The specific technical solutions of the present invention are as follows.

[0047] 1. Increase the coke rate by 10-15kg / t in the first two smelting cycles before the blast furnace is shut down.

[0048] 2. The basic coke ratio of the wind-off material is determined according to the wind-off time. The present invention uses formula (1):

[0049] K 休风料 =K 正产料 +h 休风时长 ×1.5(1)

[0050] in:

[0051] K 休风料 ——Coke ratio of rest air material, kg / t;

[0052] K 正常料 ——Normal coke ratio, kg / t;

[0053] h 休风时长 —— duration of wind break, h;

[0054] By statistically analyzing the heat loss during the wind stop period and the heat deficit caused by the failure to inject coal after the wind is supplied, the basic coke ratio of the wind stop material in the whole furnace should be increased by 1.5kg / t for every wind stop hour. 休风料 The wind-break material will be kept until the wind breaks.

[0055] 3. Add empty coke according to the length of the wind break time, and add the number of empty coke n 空焦 Calculated by formula (2).

[0056] n 空焦 =h 休风时间 / 16+0.5 (2)

[0057] in:

[0058] n 空焦 ——Number of hollow coke in the resting material, rounded to the nearest integer, pieces;

[0059] h 休风时间 ——The number of hours from the start of the planned wind break to the resumption of wind.

[0060] For long-term wind stoppage of less than 60 hours, the method of adding hollow coke into the wind stoppage material is shown in Table 1.

[0061] Table 1 Methods of adding long-term wind-free empty coke

[0062]

[0063] In the table, x is the number of batches of normal material loaded after empty coke, calculated by formula (3).

[0064] x=(V 工作容积×0.85 / (1-η 压缩 )-V 空焦 ×n 空焦 ) / V 料批体积 / 8 (3)

[0065] in:

[0066] x——the number of batches of normal material loaded after empty coke, pieces;

[0067] V 工作容积 ——Blast furnace working volume, m 3 ;

[0068] η 压缩 ——Average compression rate of charge, 10% to 12%, 1000m 3 Blast furnace takes the lower limit, 4000m 3 The upper limit of the level blast furnace is taken;

[0069] V 空焦 ——The volume of a single empty focus, m 3 ;

[0070] n 空焦 ——Number of empty focal points, pieces;

[0071] V 料批体积 ——Volume of each batch of material, m 3 .

[0072] In Table 1, y is the number of batches of material that need to be loaded after the last empty coke and x normal materials are loaded until the wind stops, calculated using formula (4).

[0073]

[0074] in:

[0075] Σx——the sum of the normal materials x loaded after each group of empty coke, pieces;

[0076] V 工作容积 ——Effective volume of blast furnace, m 3 ;

[0077] η 压缩 ——Average compression rate of charge, 10% to 12%, 1000m 3 Blast furnace takes the lower limit, 4000m 3 The upper limit of the level blast furnace is taken;

[0078] V 空焦 ——The volume of a single empty focus, m 3 ;

[0079] n 空焦 ——Number of empty focal points, pieces;

[0080] V料批体积 ——Volume of each batch of material, m 3 .

[0081] According to formula (2), formula (3) and formula (4), the quantity of empty coke and the quantity of normal coke are calculated. When the last batch of normal coke is charged and the wind is stopped, the first group of empty coke is located at the upper part of the blast furnace bosh, that is, Figure 1 Position shown.

[0082] 4. After the blast furnace is shut down, there is still a direct reduction reaction of the charge in the blast furnace, and the molten slag will continue to drip into the furnace. At this time, if the cooling intensity is still maintained at a high level, on the one hand, more slag will condense on the copper cooling wall, causing the slag skin to thicken and increase the risk of falling off. On the other hand, the cooling water will bring more heat from the furnace, further reducing the temperature of the slag. Therefore, the cooling water volume of the furnace body is adjusted after the blast furnace is shut down, and the cooling intensity is appropriately reduced, which is conducive to the stability of the slag skin and the maintenance of the heat of the slag in the furnace. Since the amount of cooling water in different blast furnaces is different, it should be controlled according to the actual flow rate of the cooling water in the cooling equipment. 6 to 8 hours after the blast furnace is shut down, the cooling water flow rate of the cooling wall is adjusted to 1.0m / s, and the water flow rate of the water cooling pipe at the bottom of the furnace is adjusted to 0.6~0.7m / s. See Table 2 for the specific adjustment rhythm.

[0083] Table 2 Adjustment method of cooling water for long-term shutdown of copper cooling stave blast furnace

[0084]

[0085] 5. After the air is restored, add air quickly to make the air supply ratio reach 0.5, that is, the air volume / furnace capacity reaches 0.5, with a speed of 2000m 3 Taking blast furnace as an example, the initial air volume should reach 1000m 3 / min. Then, the air is added in small increments and at a rate of 100 to 300 m / s every 7 to 10 minutes. 3 / min to increase the air volume entering the furnace, 1000m 3 Blast furnace takes the lower limit, 4000m 3 The upper limit of the first-level blast furnace is taken to maintain the normal descent of the charge, while keeping the slag skin attached to the copper cooling wall stable to avoid falling off.

[0086] 6. After taking steps 1 to 5, the blast furnace slag skin can be stably attached and not fall off, the heat consumption of the copper cooling wall is greatly reduced, the heat load of the blast furnace is stable, and the heat loss is reduced. At the same time, with the increase of the air volume entering the furnace, the additional empty coke in the wind-out material quickly reaches the tuyere area to burn and generate heat, further increasing the heat of the slag and iron in the furnace, so that the heat of the slag and iron in the copper cooling wall blast furnace can be quickly increased after a long-term wind-out and wind-reopening, which is beneficial to the recovery of the furnace condition.

[0087] This method was used in 1800m 3The blast furnace has been well utilized. Taking the wind stop on April 13, 2022 as an example, the specific implementation plan is as follows: 1. The planned inspection is 40 hours, and the planned wind stop time is from 4:30 on April 13 to 20:30 on April 14. 2. Raw material structure: 72% sintered ore + 28% Yuan ball + silica, 80% metallurgical coke + 20% medium block coke. 3. The order of loading wind stop materials: 12△ + (2C + 6△) + (1C + 6△) + (6tC + 6△) + 10△, a total of 40 batches, 49t of ore batches, 13.9t of coke batches (empty coke) (17.6 / 10.2), 0.5t of coke diced, 3 empty cokes, and the coke ratio of normal materials is 450kg / t. The coke ratio of the whole furnace is 487kg / t, the coke ratio above the tuyere is 494kg / t, and the coke ratio above the empty coke is 503kg / t. 4. Empty coke loading position: the first one is in the middle and upper part of the furnace belly, the second one is in the lower part of the 8th cooling wall of the furnace body, and there are 22 batches of normal materials above the empty coke. 5. The actual wind supply suspension time is from 4:30 on April 13 to 3:26 on April 15, and the actual wind suspension time is 46 hours and 56 minutes. 6. Water adjustment plan during the wind suspension period

[0088] Table 3 Adjustment method of cooling water for long-term shutdown of copper cooling stave blast furnace

[0089]

[0090] Air supply started at 3:26 on April 15, and then the air was gradually increased while maintaining normal pressure. At 4:30, the air was increased to 1700m 3 / min. The cumulative air volume reached 100,000, and coal injection began. 5:40 The air volume was increased to 2000m 3 / min. 6:36 The cumulative air volume was 280,000, and the iron mouth of the south field was opened. The first furnace had a shorter iron-out time of 30 minutes. 7:30 The ore batch was expanded to 39t, and the coke ratio was increased from 450 to 408. After the first furnace was closed, the big trench was cleaned. At 7:57, the south field of the second furnace was opened, and the temperature was measured at 1407℃, and later at 1445℃. 10:34 The door was closed, and the iron was tapped for 2h37min, 120t of iron was tapped, 30t of slag was tapped, the Si of molten iron was 1.41, and the slag basicity R2 was 1.06. 11:09 The third furnace in the south field was opened, and slag came in for 30 minutes, and the water slag was discharged. The temperature was measured at 1443℃, the Si of molten iron was 1.53, and the slag basicity R2 was 1.16. 12:56 The door was blocked and closed. Subsequently, according to the airflow in the furnace and the heat and emission of slag and iron in front of the furnace, the air was gradually added to expand the ore batch and increase the load. At 13:30, the air was added to 3050m 3 / min (90% of normal air volume), oxygen 11000m 3 / h, air supply recovery is completed.

[0091] The scheduled wind down period from April 13 to April 15 was restored compared to the previous wind down period of more than 40 hours, which reduced production losses by 1,000t, reduced coke consumption by 120t, and achieved economic benefits of 1 million yuan.

[0092] Taking the wind stop on September 14, 2021 as an example, the specific implementation plan is as follows: 1. Planned inspection for 24 hours, planned wind stop time: September 14 3:00 ~ 15 3:00. 2. Raw fuel structure: 72% sintered ore + 15% Yuan ball + 13% E ball + silica, 100% purchased coke. 3. The order of loading wind stop materials: 12△ + (2C + 6△) + (1C + 6△) + 16△, a total of 40 batches, 49t of ore batches, 13.0t of coke batches (empty coke), 0.5t of coke diced, 3 empty cokes, and a normal material coke ratio of 440kg / t. The coke ratio of the whole furnace is 472kg / t, the coke ratio above the tuyere is 475kg / t, and the coke ratio above the empty coke is 489kg / t. 4. Empty coke loading position: the first one is in the middle and upper part of the furnace belly, the second empty coke is in the lower part of the 8-section cooling wall of the furnace body, and there are 22 batches of normal materials above the empty coke. 5. The actual wind suspension time is from 3:00 on September 14 to 4:56 on September 15, with an actual wind suspension time of 25 hours and 56 minutes. 6. Water transfer plan during the wind suspension period.

[0093] Table 4 Adjustment method of cooling water for long-term shutdown of copper cooling stave blast furnace

[0094]

[0095] Air supply started at 4:56 on September 15, and then the air was gradually increased while maintaining normal pressure. At 5:30, the air was increased to 1500m 3 / min. The cumulative air volume reached 100,000, and coal injection began. 5:40 The air volume was increased to 2000m 3 / min. 5:09 The probe was placed to probe the material surface, the north foot was 3.37m, the south foot was 3.43m. 5:18 The material began to move obviously, and at 5:57 the material line was 3.85m north and 3.96m south. The first tank of material was placed (air volume 1640m 3 / min).

[0096] 6:10 Air volume increased to 1700m 3 / min, the cumulative air volume reaches 100,000, and coal injection begins.

[0097] 6:45 (air supply 1h49min) add air to 2000m 3 / min. Maintain air volume 2000m 3 / min no movement.

[0098] 7:40 The accumulated air volume reached 280,000, and the South Iron Gate was opened. After opening, the heat of slag iron was acceptable, so the slag skimmer was used instead. The temperature of the initial iron tapping was 1352℃, and the temperature of the later stage was 1407℃. The gate was closed at 10:07, and the iron tapping lasted 2h27min, with a total of 220t of iron tapping.

[0099] After the discharge of the South Field went smoothly, the furnace was filled with air, and at 9:46 the air was added to 2500m 3 min, expanded the ore batch to 36t, and increased the coke ratio from 440 to 420.

[0100] 10:45 The second furnace in the south field was opened, and the slag was flushed with water slag for 15 minutes, and the temperature was measured at 1415℃. 13:16 The opening was blocked and closed.

[0101] 11:28 Open the 18# air outlet and gradually increase the air volume. 12:09 The air volume reaches 2800m 3 / min, expand the ore batch to 40t, and the coke ratio to 406.

[0102] 13:29 The first opening of the north field, slag came in 13 minutes, and the temperature was measured at 1370℃. 13:58 The 8# and 22# tuyere were opened, and the tuyere was fully opened.

[0103] 14:17 Increase wind speed to 3000m 3 / min, expanded ore batch to 44t, coke ratio 395.

[0104] Then, according to the airflow in the furnace and the heat and discharge of slag iron in front of the furnace, the air was gradually added to expand the ore batch and increase the load. At 16:40, the air was added to 3500m 3 / min (90% of normal air volume), oxygen 14000m 3 / h, ore batch 47t, coke ratio 387. Air supply recovery completed.

[0105] The recovery time from the scheduled inspection and shutdown from September 14 to September 15, 2021 was shortened from 24 hours to 12 hours compared with the previous shutdown of more than 24 hours, reducing production losses by 750t, reducing coke consumption by 80t, and achieving economic benefits of 820,000 yuan.

[0106] The method provides a method for eliminating the risk of a large-scale shedding of slag skin on the copper cooling stave blast furnace during a long-term shutdown and rewinding process, such as the coke ratio of the shutdown material, the amount and position of the empty coke added to the shutdown material, the adjustment of the cooling system during the shutdown period, and the control of the air-adding rhythm at the initial stage of rewinding, thereby greatly improving the heat of the slag in the initial stage of rewinding by combining the heating effect of the empty coke in the shutdown material. This method greatly shortens the time for the copper cooling stave blast furnace to resume air flow after a long-term shutdown, reduces fuel consumption, and reduces production losses, laying a foundation for green and low-carbon ironmaking.

[0107] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.

Claims

1. A method for increasing the heat of slag and iron in the initial stage of long-term wind-restoration in a copper-cooled stave blast furnace, characterized in that: The following steps are involved: 1) Increase the coke rate by 10-15kg / t in the first two smelting cycles before the blast furnace is shut down; 2) Determine the basic coke ratio of the wind-off material according to the wind-off time, using formula (1) K 休风料 =K 正常料 +h 休风时长 ×1.5(1) in: K 休风料 ——Coke ratio of rest air material, kg / t; K 正常料 ——Normal coke ratio, kg / t; h 休风时长 ——Blow-off duration, h; by statistically analyzing the heat loss during the blow-off period and the heat deficit caused by the failure to inject coal after the blow-off, the basic coke ratio of the blow-off material in the whole furnace should be increased by 1.5 kg / t for every blow-off hour; the coke ratio charged in the smelting cycle before the blow-off is K 休风料 The wind-break material until the wind breaks; 3) Add empty coke according to the length of the wind-off time, and add the number of empty coke n 空焦 Calculated by formula (2); n 空焦 =h 休风时间 / 16+0.5(2) in: n 空焦 ——Number of hollow coke in the resting material, rounded to the nearest integer, pieces; h 休风时间 - the number of hours from the start of the planned wind break to the resumption of wind; For long-term wind stop within 60 hours, hollow coke is added to the wind stop material; After the last batch of normal materials are loaded, the first group of empty coke is located at the upper part of the blast furnace bosh; 4) After the blast furnace is shut down, there is still direct reduction reaction of the charge in the blast furnace, and the molten slag will continue to drip into the furnace, so the cooling water flow rate of the cooling wall is adjusted to 1.0m / s 6 to 8 hours after the blast furnace is shut down, and the water flow rate of the furnace bottom water cooling pipe is adjusted to 0.6 to 0.7m / s; 5) After the air is restored, add air quickly to make the air supply ratio reach 0.5, that is, the air volume / furnace capacity reaches 0.5; 6) After taking steps 1) to 5), the slag temperature in the furnace increases from 1300-1350°C to 1400-1450°C, reaching a temperature above which the slag can flow freely, so that the heat of the slag in the copper-cooled stave blast furnace can be quickly increased after a long period of rest and resumption of air flow, thereby restoring the furnace condition.

2. The method for increasing the heat of slag and iron in the initial stage of long-term wind-restoration of a copper-cooled stave blast furnace according to claim 1, characterized in that: Step 3) The method of adding empty cokes in the medium- and long-term wind break is as follows: the wind break time is 8 hours, the number of empty cokes is 1, and the arrangement is (1C+x△)+y△; the wind break time is 12 hours, the number of empty cokes is 1, and the arrangement is (1C+x△)+(1C+x△)+y△; the wind break time is 24 hours, the number of empty cokes is 2, and the arrangement is (1C+x△)+(1C+x△)+y△; the wind break time is 36 hours, the number of empty cokes is 3, and the arrangement is (2C+x△)+(1C+x△)+y△; the wind break time is 48 hours, the number of empty cokes is 4, and the arrangement is (2C+x△)+(1C+x△)+(1C+x△)+y△; the wind break time is 60 hours, the number of empty cokes is 4, and the arrangement is (2C+x△)+(1C+x△)+(1C+x△)+y△; x is the number of batches of normal material loaded after empty coke, calculated by formula (3); x=(V 工作容积 ×0.85 / (1-η 压缩 )-V 空焦 ×n 空焦 ) / V 料批体积 / 8 (3) in: x——the number of batches of normal material loaded after empty coke, pieces; V 工作容积 ——Blast furnace working volume, m 3 ; η 压缩 ——Average compression rate of charge, 10% to 12%, 1000m 3 Blast furnace takes the lower limit, 4000m 3 The upper limit of the level blast furnace is taken; V 空焦 ——The volume of a single empty focus, m 3 ; n 空焦 ——Number of empty focal points, pieces; V 料批体积 ——Volume of each batch of material, m 3 ; y is the number of batches of material that need to be loaded after loading the last empty coke and x normal materials until the wind stops, calculated by formula (4); in: Σx——the sum of the normal materials x loaded after each group of empty coke, pieces; V 工作容积 ——Effective volume of blast furnace, m 3 ; η 压缩 ——Average compression rate of charge, 10% to 12%, 1000m 3 Blast furnace takes the lower limit, 4000m 3 The upper limit of the level blast furnace is taken; V 空焦 ——The volume of a single empty focus, m 3 ; n 空焦 ——Number of empty focal points, pieces; V 料批体积 ——Volume of each batch of material, m 3 .

3. The method for increasing the heat of slag and iron in the initial stage of long-term wind-restoration of a copper-cooled stave blast furnace according to claim 1, characterized in that: Step 4) The specific adjustment rhythm is as follows: during normal production, the water flow rate of the furnace cylinder cooling wall is 2.7m / s, and the water flow rate of the furnace bottom water cooling pipe is 2.0m / s; 1 hour after the wind is stopped, the water flow rate of the furnace cylinder cooling wall is 2.10m / s, and the water flow rate of the furnace bottom water cooling pipe is 2.0m / s; 2 hours after the wind is stopped, the water flow rate of the furnace cylinder cooling wall is 1.80m / s, and the water flow rate of the furnace bottom water cooling pipe is 1.60m / s; 4 hours after the wind is stopped, the water flow rate of the furnace cylinder cooling wall is 1.40m / s, and the water flow rate of the furnace bottom water cooling pipe is 1.20m / s; 6 hours after the wind is stopped, the water flow rate of the furnace cylinder cooling wall is 1.00m / s, and the water flow rate of the furnace bottom water cooling pipe is 0.60m / s.

Citation Information

Patent Citations

  • Method for adjusting structure of furnace burden before blowing-down of iron smelting blast furnace

    CN105950808A

  • Rapid yield reaching method after damping down of medium titanium slag smelting blast furnace

    CN113174452A

  • Method for charging raw material at cooling time in blast furnace

    JP2000109909A