Copolymers, their preparation and use
By adjusting the molar ratio and structure of the repeating unit and the terminal unit of the copolymer, the problem of high melting temperature of the existing thermoplastic polymer materials is solved, and high performance polymers processed at low temperatures are achieved, and high glass transition temperatures are maintained. and mechanical properties reduce energy consumption and improve material recyclability.
Patent Information
- Application Number
- CN202180060592.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-01-08
- Filing Date
- 2021-06-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-06-22
AI Technical Summary
The existing thermoplastic polymer materials have high melting temperatures in processing and application, which leads to high energy consumption and difficult processing, while it is difficult to reduce the melting temperature and maintain high glass transition temperature and mechanical properties.
Copolymerization consisting essentially of [-ether-phenyl-ether-phenyl-carbonyl-phenyl-] and [ether-phenyl-ether-phenyl-ether-phenyl-carbonyl-phenyl-] repeating units and terminal units is adopted The molar ratio and structure of the copolymer are adjusted by specific nucleophilic polycondensation methods and reaction conditions to reduce the melting temperature while maintaining high glass transition temperature and crystallinity.
A copolymer that maintains high mechanical properties and chemical resistance at lower processing temperatures is achieved, reducing energy consumption and improving material recovery and reprocessing properties, while improving the thermal stability and crystallization rate of the material.
Smart Images

Figure CN116157471B_ABST
Abstract
Description
[0001] The present invention relates to copolymers consisting essentially of [-ether-phenyl-ether-phenyl-carbonyl-phenyl-] and [ether-phenyl-phenyl-ether-phenyl-carbonyl-phenyl-] repeating units and terminal units, which have a reduced melting temperature (Tm) compared to prior art copolymers comprising such repeating units. The copolymers of the present invention have crystallinity and have a glass transition temperature similar to that of prior art polymers.
[0002] There are many thermoplastic polymer materials available for use in industry, either as the sole material for making a component, or as part of a composite material, such as a polymer / fiber composite material, for making a component. However, there remains a need for thermoplastic polymer materials having improved properties in at least some respects over existing thermoplastic polymer materials.
[0003] Polyaryletherketone (PAEK), such as polyetheretherketone (PEEK), is a homopolymer with [-ether-phenyl-ether-phenyl-carbonyl-phenyl-] repeating units, commonly used as a high-performance thermoplastic polymer. PEEK is the material of choice for many commercial applications because it forms a highly crystalline solid when solidified from the melt, with excellent mechanical properties and chemical resistance. PEEK melts at about 343°C and has a Tg of about 143°C.
[0004] Unlike many conventional polymers, PAEK polymers or copolymers can be obtained in either amorphous or crystalline form as a direct result of the way the polymer is processed. The glassy or amorphous state is achieved by rapidly quenching the polymer from the melt to below Tg, while slowly cooling the polymer from the melt will allow crystallinity to develop in the sample (melt crystallization). The crystalline form of a polymer can also be obtained from the polymer in its amorphous form, for example at room temperature by heating the polymer to a temperature above Tg but below Tm (cold crystallization) and then cooling back to room temperature, or by holding the polymer at a constant temperature between Tg and Tm for a period of time (isothermal crystallization) and then cooling back to room temperature.
[0005] PAEK, including PEEK in particular, can be produced by nucleophilic polycondensation of bisphenols with organic dihalide compounds in the presence of alkali metal carbonates and / or alkali metal bicarbonates, or alkaline earth metal carbonates and / or alkaline earth metal bicarbonates in a suitable solvent. Such methods are given, for example, in EP0001879A, EP0182648A, EP0244167A and EP3049457A.
[0006] Copolymers of PEEK and PEDEK are disclosed in EP0184452A, which describes copolymers containing [-ether-phenyl-ether-phenyl-carbonyl-phenyl-] (i.e. R PEEK ) repeating units and [-ether-phenyl-phenyl-ether-phenyl-carbonyl-phenyl-] (ie, RPEDEK ) repeating units. The PEEK-PEDEK copolymer is disclosed to have chemical resistance and mechanical properties similar to those of PEEK, and at the same time has a Tm lower than that of PEEK, but has a Tg value similar to or higher than that of PEEK.
[0007] WO2014 / 207458A1 discloses a PEEK-PEDEK copolymer, which is prepared by a method comprising polycondensing a mixture of at least one dihydroxybenzene compound and at least one dihydroxybiphenyl compound in a molar ratio of 65:35 to 95:5 with at least one dihalobenzophenone in the presence of sodium carbonate and potassium carbonate, wherein the mole % of potassium carbonate used in the synthesis of the PEEK-PEDEK copolymer by nucleophilic polycondensation is at least 2.5, wherein the mole % of potassium carbonate is expressed as a percentage of the total moles of hydroxyl monomers used in the synthesis. The PEEK-PEDEK copolymer of WO2014 / 207458A1 has a higher crystallinity than the copolymer disclosed in EP0184452A.
[0008] WO2019 / 186085A1 discloses PEEK-PEDEK copolymers made by a specific nucleophilic condensation process, which includes stopping the polymerization (e.g., using a lithium salt) and end-capping the copolymer (to provide specific terminal units to the copolymer) in the presence of a reduced amount of an aromatic sulfone solvent to provide a PEEK-PEDEK copolymer having reduced chain branching and reduced melt viscosity at low shear rates compared to copolymers of similar molecular mass in the prior art.
[0009] Polyphenylene sulfide (PPS) is another known thermoplastic polymer material that has a lower melting temperature (Tm) than PEEK, specifically about 290°C. However, the glass transition temperature (Tg) of PPS is 85°C to 100°C, which is too low for many applications. Polyetheretherketone (PEEK) has a reasonably high Tg of 143°C, enabling it to be used in high temperature applications without loss of crystallinity, but its Tm of 343°C is much higher than desired because high temperatures are required to process PEEK in its molten state, typically requiring a temperature range of 370°C to 420°C. Nonetheless, PEEK is the material of choice for many commercial applications because it tends to form a highly crystalline structure with excellent chemical resistance and mechanical properties.
[0010] WO2019 / 122226A1 discloses a method of preparing a polyol having an R ratio of 95 / 5 to 45 / 55. PEEK / R PEmEK Molar ratio R PEEK Repeating unit and R PEmEK Repeating unit of PEEK-PEmEK copolymer,
[0011] R PEEK Repeating Unit
[0012] R PEmEK Repeating unit.
[0013] These are believed to provide a relationship between the melting temperature, Tm, and the heat of fusion ((ΔH)) satisfying the following equation:
[0014] ΔH≥-.00005(Tm) 2 +1.008(Tm)-226.33
[0015] In the example of WO2019 / 122226A1, due to R PEEK / R PEmEK The ratios of 95 / 5 to 50 / 50 vary, with Tm decreasing from 333°C to 253°C, Tg decreasing from 154°C to 129°C, and ΔH decreasing from 60 J / g to 3 J / g. This can be compared to PEEK's Tm of 339°C, Tg of 149°C, and ΔH of 49 J / g according to WO2019 / 122226A1.
[0016] Terminology PEmEK It means that two ether bonds are connected to the same phenyl group in the "meta" configuration (1,3) in the repeating unit, and for R PEEK , two ether bonds are connected to the same phenyl group in a "para" configuration (1,4) in the repeating unit.
[0017] WO2019 / 122226A1 also discloses that the PEEK-PEmEK copolymer may include repeating units R different from PEEK and R PEmEK The repeating unit R PAEK , relative to the total molar number of repeating units of the PEEK-PEmEK copolymer, specifically comprising 0.1 to 5 mol% of the repeating unit R PAEK . R PAEK The units are listed as KA to KM, but none of the additional repeating units disclosed corresponds to R PEDEK Repeating unit.
[0018] There is a need for other high performance PAEK polymers that have a reduced melting temperature (Tm) compared to PEEK, but have a high Tg and exhibit crystallinity, and have mechanical strength and chemical resistance comparable to PEEK. There is also a need for other high performance PAEK polymers that have thermal decomposition temperatures similar to PEEK polymers to allow recycling and reprocessing. There is also a need for methods of synthesizing such polymers.
[0019] Such polymers with a lower melting point Tm result in easier melt processing, for example because lower processing temperatures can be used, requiring less energy consumption and reducing the risk of thermal degradation of the copolymer as long as the polymer degradation temperature is not also reduced, thus making the copolymer also easier to recycle multiple times. In order to ensure that the polymer is at least as recyclable and reprocessable as prior art polymers such as PEEK, the polymer should have a thermal decomposition temperature Td5 similar to that of PEEK.
[0020] However, maintaining a high Tg for a polymer means that the polymer can still be used in high temperature applications. It is desirable to keep the polymer Tg as high as possible because Tg represents the temperature above which parts made from the polymer may lose strength and show reduced chemical resistance, fatigue resistance, and wear resistance. Crystallinity is also important to maintain performance at high temperatures, so a high Tg combined with a reasonable level of crystallinity can produce the desired material properties.
[0021] Additionally, due to the lowered Tm, the reduced processing temperature may allow for the inclusion of additives in the copolymer prior to melt processing, which additives would degrade when blended with polymers or copolymers having higher Tms.
[0022] In the present specification, the term "includes" or "comprising" means including specified components but not excluding the existence of other components.
[0023] The term "consisting essentially of" or "consisting essentially of" means including the specified ingredients but excluding other ingredients, except for materials present as impurities, unavoidable materials present as a result of the process used to provide the ingredients, and ingredients added for purposes other than achieving the technical effects of the invention. Typically, when referring to a composition, a composition consisting essentially of a set of ingredients will contain less than 5% by weight, typically less than 3% by weight, and more typically less than 1% by weight of non-specified ingredients. When referring to the copolymers of the present invention, the term "consisting essentially of" means that the copolymer chain has at least 95% by weight of only the specified repeating units and terminal units, and any other repeating units or terminal units present in the polymer chain are generally due to the presence of impurities in the monomers or organic dihalides further used to make the copolymer. The deliberate inclusion of other monomers and / or terminal units up to 5% by weight may be allowed.
[0024] The final product manufactured from the copolymer of the present invention includes, in addition to the copolymer itself consisting essentially of the specified repeating units and terminal units, certain reaction by-products from the manufacture, such as residual solvents, residual salts, and residual monomers, in addition to the polymer chains, as described in more detail below. Therefore, the term "copolymer consisting essentially of the repeating units and terminal units" refers to the polymer itself, but it must be understood that the term includes the presence of residual by-products resulting from the manufacture of the copolymer, which are present at up to 5% by weight of the final manufactured product, as well as polymer chains, the remaining 95% being copolymer chains.
[0025] The term "consisting of" or "composed of" means including the specified components but excluding other components.
[0026] Where appropriate, depending on the context, the use of the terms "comprising" or "including" may also be considered to include the meaning of "consisting essentially of" or "consisting essentially of", and may also be considered to include the meaning of "consisting of" or "consisting of."
[0027] As used herein, the term "nucleophilic polycondensation" is used to briefly refer to a method for preparing PAEK, especially PEEK-PEDEK copolymers, by nucleophilic polycondensation of bisphenols with organic dihalide compounds in the presence of alkali metal carbonates and / or alkali metal bicarbonates, and / or alkaline earth metal carbonates and / or alkaline earth metal bicarbonates, and in the presence of aromatic sulfone polymerization solvents such as diphenyl sulfone (DPS).
[0028] Reference to monomers, solvents and other additives for the nucleophilic condensation reaction is intended to mean that these compounds are used in their commercially available purity without further specialized purification.
[0029] A first aspect of the present invention provides a copolymer consisting essentially of a repeating unit of formula I, a repeating unit of formula II and a terminal unit,
[0030] -O-Ph-O-Ph-CO-Ph-I;
[0031]
[0032] wherein the molar ratio of the repeating unit of formula I to the repeating unit of formula II is 55:45 to 95:5; and
[0033] wherein the repeating units of formula I consist essentially of 50 to 90 mol % of repeating units of formula III and 10 to 50 mol % of repeating units of formula IV, repeating units of formula V or a mixture thereof,
[0034]
[0035] The repeating unit of formula IV is:
[0036] IV; and
[0037] The repeating unit of formula V is:
[0038]
[0039] Preferably, the molar ratio of the repeating unit of formula I to the repeating unit of formula II is 60:40 to 90:10, preferably 70:30 to 90:10, more preferably 80:20 to 90:10.
[0040] The repeating units of formula I consist essentially of or preferably consist of 50 to 90 mol % of repeating units of formula III in combination with 10 to 50 mol % of repeating units of formula IV and / or formula V. Preferably, the repeating units of formula I consist essentially of or preferably consist of 65 to 90 mol % of repeating units of formula III in combination with 10 to 35 mol % of repeating units of formula IV, repeating units of formula V, or mixtures thereof. More preferably, the repeating units of formula I consist essentially of or preferably consist of 80 to 90 mol % of repeating units of formula III in combination with 10 to 20 mol % of repeating units of formula IV, repeating units of formula V, or mixtures thereof.
[0041] In this specification, repeating unit III is referred to as R PEEK , repeating unit IV is called R mPEEK , and the repeating unit V is called R oPEEK .
[0042] Therefore, in other words, the repeating units of formula I are represented by a molar ratio of R PEEK :(R mPEEK +R oPEEK ).
[0043] In a particularly preferred embodiment, the copolymer is a copolymer as described above, wherein the molar ratio of repeating units of formula I to repeating units of formula II is 90:10 to 80:20, and wherein the repeating units of formula I consist essentially of or preferably consist of 80 to 90 mol % of repeating units of formula III in combination with 10 to 20 mol % of repeating units of formula IV, repeating units of formula V, or a mixture thereof.
[0044] It will be appreciated that Formula I: -O-Ph-O-Ph-CO-Ph- provides no information as to whether the ether bond of the -O-Ph-O- moiety is arranged in a para, meta or ortho configuration, whereas Formulas III, IV and V specify this, as do all other configurations within the repeat unit.
[0045] In one embodiment, the copolymer according to the first aspect of the present invention may be a copolymer that does not include a repeating unit of formula IV.
[0046] In another embodiment, the copolymer according to the first aspect of the present invention may be a copolymer that does not include the repeating unit of formula V.
[0047] It will be appreciated that the use of only one repeating unit IV or V results in a simplification of the manufacturing process.
[0048] The copolymer of the first aspect of the present invention includes terminal units in addition to the repeating units. The terminal units may be identical to the repeating units of the copolymer but terminated with a terminal -OH or halogen moiety (usually a -F moiety). This may occur when the polymer is polycondensed without the intentional addition of an end-capping agent to the reaction mixture.
[0049] The copolymer of the first aspect of the invention may also be end-capped so that in addition to the terminal units identical to the repeating units of the copolymer but terminated with a terminal -OH or halogen (such as -F) moiety, the repeating units also include As described below, the end-capping process does not necessarily result in all end units being terminal unit, but such end-capping will improve the thermal stability of the copolymer.
[0050] The second aspect of the present invention provides a method for producing the copolymer of the first aspect of the present invention, the method comprising polycondensing 4,4'-difluorobenzophenone with a mixture of dihydroxy compounds consisting of 1,4-dihydroxybenzene, 4,4'-dihydroxybiphenyl and at least one of 1,3-dihydroxybenzene and 1,2-dihydroxybenzene; wherein the dihydroxy compounds are in a molar proportion required to provide the copolymer of the first aspect of the present invention;
[0051] wherein the molar ratio of (4,4'-difluorobenzophenone) / (dihydroxy compound) is from 1.005 to 1.05; and
[0052] The polycondensation is carried out in the presence of particulate sodium carbonate and potassium carbonate in an aromatic sulfone solvent.
[0053] The reaction conditions required for the nucleophilic polycondensation of PEEK-PEDEK copolymers, as well as the subsequent purification and solvent removal, are well known to the skilled person and reference is made to EP0184452A, WO 2014 / 207458 and WO 2019 / 186085 A1.
[0054] In this method, sodium bicarbonate or a mixture of sodium bicarbonate and sodium carbonate can be considered equivalent to sodium carbonate based on providing the same molar equivalent of sodium ions to the reaction mixture. Similarly, potassium bicarbonate or a mixture of potassium bicarbonate and potassium carbonate can be considered equivalent to potassium carbonate based on providing the same molar equivalent of potassium ions to the reaction mixture.
[0055] The aromatic sulfone solvent used in this process may suitably be a solvent of the formula
[0056]
[0057] Wherein W is a directly connected oxygen atom or two hydrogen atoms (one on each benzene ring), and Z and Z' may be the same or different, being a hydrogen atom or a phenyl group. A mixture of such solvents may be used. Examples of such aromatic sulfones include diphenyl sulfone, dibenzothiophene sulfone dioxide, phenoxthiophene dioxide and 4-phenylsulfonyl biphenyl. Diphenyl sulfone is a preferred solvent. Step a of the method is preferably carried out in the presence of diphenyl sulfone as a solvent. Preferably, the aromatic sulfone solvent comprises 95% by weight or more of diphenyl sulfone. More preferably, the aromatic sulfone solvent is substantially composed of diphenyl sulfone, which means that the solvent comprises at least 95% by weight of diphenyl sulfone, preferably 98% by weight, more preferably 99% by weight.
[0058] The progress of polycondensation can be monitored by measuring the torque applied to the reaction agitator. As the molecular weight of the copolymer (degree of polymerization) increases, the torque increases. When the target torque is reached, the reaction will terminate. A standard curve of agitator torque as a function of degree of polymerization (such as measured by polymer MV) can be drawn and used for subsequent reaction control.
[0059] Once the desired degree of polycondensation has been achieved, the reaction can be terminated by adding a stopping agent to the reaction mixture. Typically, a salt such as lithium sulfate can be used as a stopping agent.
[0060] Once the polycondensation reaction is considered to be complete, or after the polycondensation is stopped using a stopping agent, additional organic dihalides can also be used to provide end-capping (i.e., providing terminal units) of the copolymer. Additional organic dihalides can be selected from one or more of 4,4'-difluorobenzophenone or 4,4'-dichlorodiphenyl sulfone, 1,3-bis(4-fluorobenzoyl)benzene, 4,4'-dichlorodiphenyl sulfone and 1,3-bis(4-chlorobenzoyl)benzene. Another organic dihalide used as an end-capping agent is more preferably 4,4'-difluorobenzophenone. Due to the addition of other organic dihalides, the terminal units of the copolymer can be terminated with halogen atoms, preferably fluorine atoms, which is understood to be a thermally stable copolymer.
[0061] Therefore, a preferred embodiment of the second aspect of the present invention is a process in which the polycondensation is stopped with lithium sulfate and in which the copolymer is end-capped by adding further 4,4'-difluorobenzophenone.
[0062] In another example of the second aspect, an additional step is performed. Once the desired degree of polycondensation is reached, the reaction is terminated by adding a stop agent if necessary, and the additive is added to the reaction mixture and stirred for at least 5 minutes. More preferably, the reaction mixture is stirred for 15 minutes after adding the additive, and even more preferably for at least 30 minutes.
[0063] In one embodiment, the additive is a polyaryletherketone PAEK, wherein the PAEK has a melting temperature at least 20°C higher than the melting temperature of the copolymer, as determined by differential scanning calorimetry as described in Example 33. More preferably, the PAEK has a melting temperature at least 50°C higher, or even more preferably at least 80°C higher than the melting temperature of the copolymer.
[0064] The PAEK may be selected from the following PAEK group: polyetheretherketone, polyetherketone, polyether.
[0065] For purified copolymers, melt viscosity (MV), used to estimate polymer molecular weight (and thus the degree of polycondensation), can be measured at 400 °C and 1,000 s -1 The viscosity of the copolymer was measured appropriately using a Malvern Instruments Rosand RH10 capillary rheometer at a shear rate of 1.50 mm (capillary diameter) x 8.0 mm (capillary length). The RH10 capillary rheometer was equipped with a tungsten carbide die of 0.5 mm (capillary diameter) x 8.0 mm (capillary length). About 5 grams of the copolymer was dried in an air circulating oven at 150°C for 3 hours. The extruder was equilibrated to 400°C. The dried polymer was loaded into the heating barrel of the extruder, a brass end (12 mm long x 9.92 ± 0.01 mm diameter) was placed on top of the polymer, and the piston and screw were manually turned until the seal of the pressure gauge just engaged the piston to help clear any trapped air. The polymer column was allowed to heat and melt for at least 10 minutes. After the preheating stage, the screw began to rotate, causing the molten polymer to be extruded through the die to form thin fibers at the desired shear rate, while the pressure (P) required to extrude the polymer was recorded. The melt viscosity is given by
[0066]
[0067] Where P = pressure / kN m -2
[0068] L = mold length / m
[0069] S = punching speed / ms -1
[0070] A=Cylinder cross-sectional area / m 2
[0071] r = mold radius / m
[0072] The relationship between shear rate and other parameters is given by:
[0073] Apparent wall shear rate = 4Q
[0074] πr 3
[0075] Where Q = volume flow rate / m 3 s -1 =SA.
[0076] Therefore, by adjusting the punch speed S, the -1 ) to measure the viscosity of the molten polymer.
[0077] The copolymer of the present invention suitably has a flow rate of 1000 s at 400°C as described above by capillary rheometer. -1 The median shear rate measured is at least 0.05 kNsm -2 , preferably at least 0.10 kNsm -2 , more preferably at least 0.15 kNsm -2 The copolymer may have a melt viscosity (MV) of 1000s -1 Measured less than 1.20kNsm -2 , suitably less than 1.00kNsm -2 Melt viscosity. 1000s -1 The measured melt viscosity can be used as a measure or indication of the molecular mass of the polymer.
[0078] Additive layer manufacturing technologies include filament fusion, laser sintering, powder bed fusion, ThermoMELT TM and particle fusion.
[0079] Powder bed fusion and filament fusion are examples of additive manufacturing processes for which the copolymers of the present invention are particularly useful. Powder bed fusion (also known as laser sintering or selective laser sintering - SLS) involves the use of a laser to melt and fuse polymer microparticles together as a building material for part molding into a three-dimensional part shape. No external forces (other than gravity) are applied to the powder, so the polymer is not subject to significant shear as it melts. Powder bed fusion is therefore a low shear process, and therefore requires a polymer with a low viscosity under low shear conditions to agglomerate the polymer microparticles. Using only low molecular weight polymers may not be sufficient to achieve the viscosity requirements, as high molecular weights are preferred for high mechanical strength.
[0080] In filament fusion, thin filaments of polymer are extruded through a print head onto a substrate to be used as a building material for building parts layer by layer. Although the polymer may experience significant shear at the extruder head, the consolidation and fusion processes that occur outside the print head are low shear processes. Therefore, when the polymer is in the molten state, it is desirable to have a polymer with a relatively low viscosity at low shear rates. However, it is desirable to maintain the polymer molecular weight at a level that ensures good mechanical properties and toughness.
[0081] In view of the combination of low Tm with high Tg, low dynamic viscosity at low shear rates and the ability to crystallize, the copolymers of the present invention are particularly useful as building materials for additively manufactured parts.
[0082] Therefore, the present invention also provides a method for producing a three-dimensional component by additive layer manufacturing from the copolymer of the first aspect of the present invention.
[0083] Another aspect of the present invention provides the use of the copolymer of the first aspect of the present invention as a building material in an additive manufacturing process.
[0084] In particular, the present invention also provides a method for manufacturing a three-dimensional component from a powder selectively sintered using electromagnetic radiation, wherein the powder comprises, essentially consists of, or consists of a copolymer according to the first aspect of the present invention.
[0085] The present invention also provides the use of a powder as a building material for selectively sintering the powder using electromagnetic radiation to produce a three-dimensional component from the powder, wherein the powder comprises a copolymer according to the first aspect of the invention, essentially consists of a copolymer according to the first aspect of the invention, or consists of a copolymer according to the first aspect of the invention.
[0086] The copolymer of the first aspect of the present invention may be compounded with one or more fillers. The filler may include a fibrous filler or a non-fibrous filler. The filler may include a fibrous filler and a non-fibrous filler. The fibrous filler may be continuous or discontinuous.
[0087] The fibrous filler may be selected from inorganic fibrous materials, non-melting and high-melting organic fibrous materials, such as aramid fibers and carbon fibers.
[0088] The fiber filler can be selected from glass fiber, carbon fiber, asbestos fiber, silica fiber, alumina fiber, zirconium oxide fiber, boron nitride fiber, silicon nitride fiber, boron fiber, fluorocarbon resin fiber and potassium titanate fiber. Preferred fiber fillers are glass fiber and carbon fiber. The fiber filler can include nanofibers.
[0089] The non-fibrous filler can be selected from mica, silica, talc, hydroxyapatite (or hydroxyapatite), alumina, kaolin, calcium sulfate, calcium carbonate, titanium oxide, titanium dioxide, zinc sulfide, ferrite, clay, glass powder, zinc oxide, nickel carbonate, iron oxide, quartz powder, magnesium carbonate, fluorocarbon resin, graphite (including graphite nanosheets and graphene), carbon black, carbon powder, nanotubes (such as carbon nanotubes) and / or barium sulfate. The non-fibrous filler can be introduced in the form of powder or flaky particles.
[0090] Preferably, if fillers are present, they may include or may be one or more fillers selected from the group consisting of glass fibers, carbon fibers, polyaramid fibers, carbon black, and fluorocarbon resins. More preferably, the fillers include or are glass fibers or carbon fibers. Such fillers preferably include or are glass fibers.
[0091] The filled copolymer composition may include, consist essentially of, or consist of at least 20 wt % or at least 40 wt % of filler. The filled composition may include, consist essentially of, or consist of 70 wt % or less, or 60 wt % or less of filler.
[0092] The present invention also provides a component comprising, essentially consisting of, or consisting of a copolymer according to the first aspect of the present invention or a filled copolymer composition as described above. For example, the component can be a film, a rod such as a rod, or a machined component. The component can be an injection molded component, a compression molded component, or an extruded component. Alternatively, the component can be formed using additive manufacturing techniques.
[0093] The present invention also provides a film or tape comprising a copolymer according to the first aspect of the invention or a composition consisting of a copolymer according to the first aspect of the invention. The film may be extruded and may have a thickness of 5 to 100 μm or preferably 5 to 50 μm.
[0094] The copolymers of the present invention are particularly useful for preparing shaped and molded housings for electronic devices, particularly portable electronic devices that can be easily dropped, such as portable smart phones and tablet computers.
[0095] For example, a housing formed from a composition for an electronic device is provided, the composition comprising, consisting essentially of, or consisting of the copolymer of the first aspect of the invention. Housings for electronic devices include housings for portable devices such as smart phones. The housing can be a molded housing. Alternatively, the housing can be formed by an additive manufacturing process. Because the copolymers of the present invention have a high resistance to brittle fracture, housings comprising, consisting essentially of, or consisting of the copolymers of the present invention are particularly suitable for withstanding the stresses and pressures of long-term daily use. In addition, housings comprising the PEEK-PEDEK copolymers of the present invention are more able to withstand defects formed during the manufacturing process of the housing, because minor manufacturing defects can cause cracks that can spread in the housing, and the copolymers of the present invention are resistant to brittle fracture.
[0096] The composition of the shell may comprise 30 to 100 wt% of the copolymer of the first aspect of the invention and 0 to 70 wt% of other ingredients, such as fillers, e.g. fiber fillers, glass fillers, colorants, etc. Preferably, the composition of the shell does not contain other PAEK or PEEK, more preferably does not contain other polymers.
[0097] The invention also provides a package comprising a copolymer according to the first aspect of the invention, preferably in powder, pellet and / or granular form.
[0098] The package may comprise at least 1 kg, suitably at least 5 kg, preferably at least 10 kg, more preferably at least 14 kg of polymeric material. The package may comprise 1000 kg or less, preferably 500 kg or less of polymeric material. Preferred packages comprise 10 to 500 kg of polymeric material.
[0099] The packaging may include packaging material (intended to be discarded or reused) and the desired material (suitably including a polymeric material). The packaging material preferably substantially completely seals the desired material. The packaging material may include a first container, such as a flexible container, such as a plastic bag, in which the desired material is arranged. The first container may be contained in a second container (such as a box, such as a carton).
[0100] The present invention also provides a tube or sleeve formed from a composition comprising or consisting of a copolymer according to the first aspect of the invention.
[0101] The invention also provides a process for forming a tube or sleeve by extruding a composition comprising or consisting of a copolymer according to the first aspect of the invention.
[0102] Specific embodiments of the present invention will now be described.
[0103] Copolymers were prepared as described in Examples 1 to 32. During the preparation process, the progress of copolymerization was monitored by measuring the torque applied to the reaction agitator. As the molecular weight of the copolymer (degree of polymerization) increased, the torque increased. As described below, when the target torque was reached, or after 60 minutes (if the target torque was not reached at this time), the reaction was terminated. As the polymer molecular weight increases, the solution viscosity in the reaction mixture also increases, resulting in an increase in the torque of the reaction agitator. Under similar reaction conditions for preparing PEEK, the target torque is expected to be about 0.15 to 0.45 kNsm -2 Examples 34 and 35 provide detailed descriptions of the procedures and tests performed on the copolymers of the examples.
[0104] The copolymers of Examples 1 to 3 are not according to the invention, whereas the copolymers of Examples 4 to 32 are according to the invention.
[0105] Example 1-0.5 mol polyetheretherketone PEEK-PEDEK copolymer (R PEEK :R PEDEK =90:10)
[0106] A 0.5-liter flanged bottle equipped with a ground glass lid, stirrer / stirrer guide, nitrogen inlet and outlet was charged with 4,4'-difluorobenzophenone (111.56 g, 0.511 mol), 1,4-dihydroxybenzene (49.55 g, 0.450 mol), 4,4'-dihydroxybiphenyl (9.31 g, 0.050 mol) and diphenyl sulfone (314.94 g) and purged with nitrogen for 1 hour. Next, the contents were heated to 150°C under a nitrogen blanket to form an almost colorless solution. While maintaining a nitrogen blanket, dry sodium carbonate (53.42 g, 0.504 mol) and potassium carbonate (2.764 g, 0.02 mol) were added, both of which were sieved through a 500 micron mesh size screen. The temperature was raised to 180°C at 1°C / min and maintained for 100 minutes. The temperature was increased at 0.5°C / min to 200°C; then the temperature was increased at 1°C / min to 305°C and maintained for about 60 minutes, or until the desired degree of polymerization was achieved as indicated by the rise in torque of the stirrer. The reaction mixture was then poured into a foil tray, cooled, ground and washed with 2 liters of acetone at 40 to 50°C, followed by warm water, until the conductivity of the waste water was <2 μS. The resulting polymer powder was dried in an air oven at 120°C for 12 hours.
[0107] Examples 2 to 3 - Preparation of other PEEK-PEDEK copolymers
[0108] The procedure described in Example 1 was repeated except that the amounts of 1,4-dihydroxybenzene and 4,4'-dihydroxybiphenyl were varied to provide a polyetheretherketone (PEEK)-biphenyl type polyetheretherketone (PEDEK) copolymer having the ratio of PEEK component to PEDEK component shown in Table 1.
[0109] Table 1
[0110] Example <![CDATA[R PEEK :R PEDEK ]]> 1,4-Dihydroxybenzene mass (g) 4,4'-Dihydroxybiphenyl mass (g) 2 75:25 41.29 23.38 3 60:40 33.03 37.24
[0111] Examples 4 to 9 - Including 1,2-dihydroxybenzene as a comonomer (providing R oPEEK Repeating unit) of PEEK- Preparation of oPEEK-PEDEK copolymer
[0112] The procedure described in Example 1 was repeated except that 1,2-dihydroxybenzene was used in combination with 1,4-dihydroxybenzene to vary the overall ratio of dihydroxybenzene to 4,4′-dihydroxybiphenyl to provide polyetheretherketone PEEK-oPEEK-PEDEK copolymers having PEEK:oPEEK:PEDEK repeating unit ratios as shown in Table 2.
[0113] Table 2
[0114]
[0115] Examples 10 to 13 - Including 1,3-dihydroxybenzene comonomer (providing R mPEEK Repeating unit) of PEEK- Preparation of mPEEK-PEDEK copolymer
[0116] The procedure described in Example 1 was repeated except that 1,3-dihydroxybenzene was used in combination with 1,4-dihydroxybenzene to vary the overall ratio of dihydroxybenzene to 4,4′-dihydroxybiphenyl to provide PEEK-mPEEK-PEDEK copolymers having the PEEK:mPEEK:PEDEK component ratios shown in Table 3.
[0117] Table 3
[0118]
[0119] Example 14 - Including 1,3-dihydroxybenzene comonomer (providing R mPEEK Repeating unit) and 1,2-dihydroxybenzene Polymerization monomer (providing R oPEEK Preparation of PEEK-mPEEK-oPEEK-PEDEK copolymers with repeating units
[0120] In this embodiment, 1,3-dihydroxybenzene and 1,2-dihydroxybenzene comonomers are used in combination with 1,4-dihydroxybenzene to provide R PEEK: R mPEEK: R oPEEK :R PEDEK =65 / 5 / 5 / 25 PEEK-mPEEK-oPEEK-PEDEK copolymer.
[0121] 4,4'-difluorobenzophenone (111.56 g, 0.511 mol), 1,4-dihydroxybenzene (35.79 g, 0.330 mol), 1,3-dihydroxybenzene (2.75 g, 0.03 mol), 1,2-dihydroxybenzene (2.75 g, 0.03 mol), 4,4'-dihydroxybiphenyl (23.28 g, 0.125 mol) and diphenyl sulfone (314.94 g) were added to a 0.5-liter flange bottle equipped with a ground glass lid, a stirrer / stirrer guide, a nitrogen inlet and outlet, and purged with nitrogen for 1 hour. Then, the contents were heated to 150° C. under a nitrogen blanket to form an almost colorless solution. While maintaining a nitrogen blanket, dry sodium carbonate (53.42 g, 0.504 mol) and potassium carbonate (2.764 g, 0.02 mol), both sieved through a 500 micron mesh size screen, were added. The temperature was raised to 180°C at 1°C / min and held for 100 minutes. The temperature was raised to 200°C at 0.5°C / min; the temperature was then raised to 305°C at 1°C / min and held for about 60 minutes, or until the desired degree of polymerization was achieved as indicated by the rise in torque of the agitator. The reaction mixture was then poured into a foil tray, cooled, ground, and washed with 2 liters of acetone at 40 to 50°C, followed by warm water, until the conductivity of the waste water was <2 μS. The resulting polymer powder was dried in an air oven at 120°C for 12 hours.
[0122] Example 15 - Including 1,2-dihydroxybenzene comonomer (providing R oPEEK Repeating unit) of PEEK-PEDEK copolymer Preparation of the polymer - Termination reaction using lithium salt and copolymer end-capping
[0123] In this embodiment, 1,2-dihydroxybenzene comonomer is used in combination with 1,4-dihydroxybenzene to provide R PEEK: R oPEEK :R PEDEK =65 / 10 / 25 PEEK-oPEEK-PEDEK copolymer.
[0124] Once the desired torque / MV was reached, the reaction was stopped by the addition of lithium sulfate followed by 4,4'-difluorobenzophenone to provide a copolymer with the following fluorobenzophenone end units:
[0125]
[0126] A 0.5-liter flanged bottle equipped with a ground glass lid, stirrer / stirrer guide, nitrogen inlet and outlet was charged with 4,4'-difluorobenzophenone (110.19 g, 0.505 mol), 1,4-dihydroxybenzene (35.79 g, 0.330 mol), 1,2-dihydroxybenzene (5.51 g, 0.05 mol), 4,4'-dihydroxybiphenyl (23.28 g, 0.125 mol) and diphenyl sulfone (303.00 g) and purged with nitrogen for 1 hour. Next, the contents were heated to 150° C. under a nitrogen blanket to form an almost colorless solution. While maintaining a nitrogen blanket, dry sodium carbonate (54.58 g, 0.515 mol) and potassium carbonate (0.35 g, 0.0025 mol) were added, both of which were sieved through a 500 micron mesh size screen. The temperature was raised to 270°C at 1°C / min and maintained until the desired torque was reached, and lithium sulfate (0.96 g, 0.00875 mol) and 4,4'-difluorobenzophenone (1.36 g, 0.00625 mol) were added. The reaction mixture was kept at 270°C for another 30 minutes. The reaction mixture was then poured into a foil tray, cooled, ground, and washed with 2 liters of acetone at a temperature of 40 to 50°C, followed by washing with warm water until the conductivity of the waste water was <2 μS. The resulting polymer powder was dried in an air oven at 120°C for 12 hours.
[0127] Example 16 - Including 1,3-dihydroxybenzene comonomer (providing R mPEEK )PEEK-mPEEK-PEDEK copolymer Preparation - Termination reaction using lithium salt and copolymer end-capping
[0128] In this embodiment, 1,3-dihydroxybenzene comonomer is used in combination with 1,4-dihydroxybenzene to provide R PEEK: R mPEEK :R PEDEK =65 / 10 / 25 PEEK-mPEEK-PEDEK copolymer.
[0129] Once the desired torque / MV was reached, the reaction was stopped by the addition of lithium sulfate followed by 4,4'-difluorobenzophenone to provide a copolymer with the following fluorobenzophenone end units:
[0130]
[0131] The detailed instructions are as follows.
[0132] A 0.5-liter flanged bottle equipped with a ground glass lid, stirrer / stirrer guide, nitrogen inlet and outlet was charged with 4,4'-difluorobenzophenone (110.19 g, 0.505 mol), 1,4-dihydroxybenzene (35.79 g, 0.330 mol), 1,3-dihydroxybenzene (5.51 g, 0.05 mol), 4,4'-dihydroxybiphenyl (23.28 g, 0.125 mol) and diphenyl sulfone (303.00 g) and purged with nitrogen for 1 hour. Next, the contents were heated to 150° C. under a nitrogen blanket to form an almost colorless solution. While maintaining a nitrogen blanket, dry sodium carbonate (54.58 g, 0.515 mol) and potassium carbonate (0.35 g, 0.0025 mol) were added, both of which were sieved through a 500 micron mesh size screen. The temperature was raised to 270°C at 1°C / min and maintained until the desired torque was reached, and lithium sulfate (0.96 g, 0.00875 mol) and 4,4'-difluorobenzophenone (1.36 g, 0.00625 mol) were added. The reaction mixture was kept at 270°C for another 30 minutes. The reaction mixture was then poured into a foil tray, cooled, ground, and washed with 2 liters of acetone at a temperature of 40 to 50°C, followed by washing with warm water until the conductivity of the waste water was <2 μS. The resulting polymer powder was dried in an air oven at 120°C for 12 hours.
[0133] Example 17 - Differential Scanning Calorimetry of Copolymers of Examples 1 to 16
[0134] Crystallinity (as reported in Table 2) can be assessed by several methods, such as density, IR spectroscopy, X-ray diffraction or differential scanning calorimetry. The DSC method was used to assess the crystallinity formed by the polymers of Examples 1 to 20 using a Mettler Toledo DSC1Star system with a FRS5 sensor.
[0135] The following DSC method was used to determine the glass transition temperature (Tg), melting temperature (Tm), and heat of fusion (Hm) of melting for the polymers of Examples 1 to 19.
[0136] A dried sample of each polymer was compression molded into an amorphous film by heating 7 g of the polymer in a mold at 50 bar pressure, 400°C for 2 minutes, and then quenching in cold water to produce a film with a size of 120×120 mm and a thickness of about 0.20 mm. An 8 mg+3 mg or 8 mg-3 mg sample of each film was scanned by DSC as follows:
[0137] Step 1, perform and record a preliminary thermal cycle by heating the sample from 50°C to 400°C at 20°C / min.
[0138] Step 2, hold for 5 minutes.
[0139] Step 3, cool at 50°C / min to the Tg recorded in the first cycle 1 To Tm 1 The midpoint (Tg 1 It is the point of maximum slope obtained during the glass transition when heated in step 1. Tm 1 is the temperature at which the melting endotherm reaches its maximum in step 1).
[0140] Step 4, keep for 3 hours
[0141] Step 5: Cool to 50°C at 50°C / min and hold for 5 minutes
[0142] Step 6, reheat from 50°C to 400°C at 20°C / min, and record the Tg, Tm and
[0143] According to the DSC trace obtained by scanning in step 6, the temperature Tg at which the endothermic slope is the largest during the glass transition is obtained. Tm is the temperature at which the melting endothermic reaches the maximum value.
[0144] The heat of fusion ( ) of melting is obtained by connecting the two points of the melting endotherm in step 6 that deviate from a relatively straight baseline above Tg. ). The integrated area under the endotherm as a function of time yields the enthalpy of the melting transition. The mass normalized heat of fusion is calculated by dividing the enthalpy by the mass of the sample (J / g). The level of crystallization (%) is determined by dividing the heat of fusion of the sample by 130 J / g. This value of 130 J / g is the heat of fusion of fully crystalline PEEK and is used as a reference value for this measurement.
[0145] The results are shown in Table 4 below.
[0146] Example 18 - Thermogravimetric Analysis of Polyaryletherketones of Examples 1 to 16
[0147] The thermal stability of a polymer can be measured by evaluating the temperature at which 5% by weight of the polymer mass is lost when the temperature is increased from room temperature to 1000°C in air at a constant rate (Td5). Td5 is suitably measured by thermogravimetric analysis (TGA). The TGA method is used to measure Td5 using a TA Instruments TGAQ5000 and a tared platinum sheet in air. The temperature is increased from room temperature to 1000°C at a rate of 50°C per minute, and when a loss of 0.1% weight of the sample is detected, the rate is reduced to 1°C per minute.
[0148] The results are shown in Table 4 below, where the examples are compared with the samples having the same total (R PEEK +R oPEEK +R mPEEK ):R PEDEK Other examples of ratios are grouped together.
[0149] Table 4
[0150]
[0151] From Table 4, we can see that by using R mPEEK and / or R oPEEK Unit Replacement Part R PEEK Unit, for a specific R PEEK :R PEDEK The PEEK-PEDEK copolymers were modified to result in:
[0152] i) Tm is significantly reduced;
[0153] ii) Tg is partially reduced;
[0154] iii) the crystallinity is partially reduced, but significant crystallinity is still present; and
[0155] iv) Little effect on Td5.
[0156] In summary, the copolymers provided by the present invention include [-ether-phenyl-ether-phenyl-carbonyl-phenyl-] (R PEEK ) and [ether-phenyl-phenyl-ether-phenyl-carbonyl-phenyl-] (R PEDEK ) repeating unit, by PEEK Unit part replaced by R oPEEK and / or R mPEEK The present invention discloses a copolymer having a lower melting temperature and a phenyl-ether unit, wherein the ether-phenyl-ether moiety is in the normal and meta positions instead of the para positions. The copolymer has crystallinity and a glass transition temperature similar to that of the prior art polymer without partial para substitution. The preparation method and use of the copolymer are also disclosed.
[0157] Example 19 - Including 1,2-dihydroxybenzene as a comonomer (providing R oPEEK Repeating unit) of PEEK- Preparation of oPEEK-PEDEK copolymer
[0158] The procedure described in Example 1 was repeated except that 1,2-dihydroxybenzene was used in combination with 1,4-dihydroxybenzene to change the overall ratio of dihydroxybenzene to 4,4′-dihydroxybiphenyl to provide polyetheretherketone PEEK-oPEEK-PEDEK copolymers having the PEEK:oPEEK:PEDEK repeat unit ratios shown in Table 5.
[0159] Table 5
[0160]
[0161] Table 6
[0162]
[0163] As shown in Table 6, the polymer material provided by Example 19 has a significantly lower Tm than the PEEK-PEDEK copolymer, a partially lower Tg than the PEEK-PEDEK copolymer, and a comparable crystallinity level.
[0164] Examples 20 and 21 - Including 1,2-dihydroxybenzene as a copolymer monomer (providing R oPEEK Repeating unit) Preparation of PEEK-oPEEK-PEDEK copolymers, adding Victrex ST45PF (PEKEKK) at the end of the reaction
[0165] In Example 20, the procedure described in Example 1 was repeated except that 1,2-dihydroxybenzene was used in combination with 1,4-dihydroxybenzene to change the overall ratio of dihydroxybenzene to 4,4′-dihydroxybiphenyl to provide a polyetheretherketone PEEK-oPEEK-PEDEK copolymer having the PEEK:oPEEK:PEDEK repeating unit ratio shown in Table 7.
[0166] In Example 21, a polymer material was prepared according to Example 19, and an additive was added to the polymer material at the end of the reaction to increase the crystallization rate of the polymer material. 10 minutes after the torque rise stopped, 7.59 grams of Victrex ST45PF (available from Victrex Manufacturing Limited, Victrex Technology Centre, Hillhouse International, Thornton Cleveleys, FY5 4QD, UK) was added to the polymer material. After stirring for another 10 minutes, the reaction mixture was poured into a foil tray, cooled, ground and washed according to the procedures in Example 1. Victrex ST45PF is polyetherketoneetherketoneketone PEKEKK.
[0167] Table 7
[0168]
[0169] The results are shown in Table 8 below.
[0170] Table 8
[0171]
[0172] Surprisingly, it was found that the additive Victrex ST45PF resulted in an increase in the crystallization rate, as shown by an increase in Tc. Without being bound by theory, it is believed that the ST45PF powder particles are nucleation sites, thereby increasing the crystallization rate of the polymer material through heterogeneous crystallization. The benefit of increasing the crystallization rate is that the polymer material can be used in various manufacturing processes, including processes that require fast crystallization properties, such as injection molding.
[0173] Embodiment 22
[0174] The procedure described in Example 8 was repeated on a larger scale using a 450 L jacketed steel vessel.
[0175] Diphenyl sulfone (99.6 kg) was charged into the container and melted. When the contents were melted and at 140 to 150°C, stirring was set at 20 rpm, and the following materials were added in sequence: 1,4-dihydroxybenzene (11.451 kg, 104.0 moles), 1,2-dihydroxybenzene (2.643 kg, 24.0 moles), 4,4'-dihydroxybiphenyl (5.959 kg, 32.0 moles), and 4,4'-difluorobenzophenone (35.715 kg, 163.7 moles). When the contents were at 140 to 150°C, a mixture of sodium carbonate (17.094 kg, 161.3 moles) and potassium carbonate (1.106 kg, 8.0 moles) pre-screened through a 500 μm mesh was added to the container.
[0176] The stirring rate was increased to 50 rpm and the content temperature was increased to 0.3 °C min- 1 Raise to 200℃, then at 1℃min -1 Raised to 305°C. The temperature was maintained at 305°C until sufficient viscosity was achieved. The molten mixture was discharged from the reactor in about 45 minutes and the solidified material was ground into a coarse powder (maximum size <2mm). The powder was transferred to a column pre-infiltrated with acetone until the leaching solvent no longer produced precipitation after the addition of water. The product was then washed with deionized water at 50°C to remove aqueous by-products. Once the conductivity of the leachate was <2μS measured using a conductivity probe, the remaining material in the column was discharged and dried in an air circulating oven at 150°C.
[0177] Embodiment 23
[0178] Example 22 was repeated but using a reduced charge of 4,4'-difluorobenzophenone of 35.505 kg.
[0179] Embodiment 24
[0180] Example 22 was repeated, but using a 76.439 kg charge of diphenyl sulfone.
[0181] Embodiment 25
[0182] Example 24 was repeated, but at the end of the polymerization, 2.42 kg of fine ST 45PF powder (PEKEKK) were added to the reaction mixture. The mixture was stirred for a further 30 minutes, then discharged and processed as previously described in Example 22.
[0183] Embodiment 26
[0184] Example 24 was repeated but using a reduced charge of 4,4'-difluorobenzophenone of 35.505 kg.
[0185] Embodiment 27
[0186] Example 25 was repeated but using a reduced charge of 35.505 kg of 4,4'-difluorobenzophenone.
[0187] Example 28 - Preparation of 12 kg of Example 22 by adding Victrex ST45PF (PEKEKK) during melt processing Polyaryletherketone
[0188] In Example 28, a polymer material was prepared according to Example 22. An additive was then added to the polymer material in a subsequent melt processing step to increase the crystallization rate of the polymer material. An amount of 600 g of Victrex ST45PF (available from Victrex Manufacturing Limited, Victrex Technology Centre, Hillhouse International, Thornton Cleveleys, FY5 4QD, UK) was added to 11.4 kg of the polymer material and fed to the rear feed section of a Coperion ZSK25 twin screw extruder through a separate loss-in-weight feeder at a barrel temperature of 310 to 320° C. The resulting mixture was then extruded into two laces having a diameter of 4 mm and cooled on a conveyor belt before being pelletized into pellets having a length of 2.0 to 4.0 mm.
[0189] Example 29 - Preparation of 12 kg of Example 23 by adding Victrex ST45PF (PEKEKK) during melt processing Polyaryletherketone
[0190] In Example 29, a polymer material was prepared according to Example 23. An additive was then added to the polymer material in a subsequent melt processing step to increase the crystallization rate of the polymer material. A quantity of 600 g of Victrex ST45PF (available from Victrex Manufacturing Limited, Victrex Technology Centre, Hillhouse International, Thornton Cleveleys, FY5 4QD, UK) was added to 11.4 kg of the polymer material and fed to the rear feed section of a Coperion ZSK25 twin screw extruder via a separate loss-in-weight feeder at a barrel temperature of 310 to 320° C. The resulting mixture was then extruded into two ribbons having a diameter of 4 mm and cooled on a conveyor belt before being pelletized into pellets having a length of 2.0 to 4.0 mm.
[0191] Example 30 - Preparation of 5 kg of the polymer of Example 22 by addition of Hytrel 5555HS (TPC-ET) during melt processing Aryl ether ketone
[0192] In Example 30, a polymer material was prepared according to Example 22. An additive was then added to the polymer material in a subsequent melt processing step to reduce the stiffness of the polymer material and improve its impact properties. A quantity of 500 g of Hytrel 5555HS (available from Dupont, 974 Centre Road, Wilmington, DE 19805, USA) was added to 4.5 kg of the polymer material and fed to the rear feed section of a Coperion ZSK25 twin screw extruder via a separate weight loss feeder at a barrel temperature of 290° C. The resulting mixture was then extruded into two ribbons having a diameter of 4 mm and cooled on a conveyor belt before being pelletized into pellets having a length of 2.0 to 4.0 mm.
[0193] Example 31 - Preparation of 5 kg of the polymer of Example 22 by addition of Hytrel 5555HS (TPC-ET) during melt processing Aryl ether ketone
[0194] In Example 31, a polymer material was prepared according to Example 22. An additive was then added to the polymer material in a subsequent melt processing step to reduce the stiffness of the polymer material and improve its impact properties. An amount of 1.0 kg of Hytrel 5555HS (available from Dupont, 974 Centre Road, Wilmington, DE 19805, USA) was added to 4.0 kg of the polymer material and fed to the rear feed section of a Coperion ZSK25 twin-screw extruder through a separate weight loss feeder at a barrel temperature of 290° C. The resulting mixture was then extruded into two ribbons having a diameter of 4 mm and cooled on a conveyor belt before being pelletized into pellets having a length of 2.0 to 4.0 mm.
[0195] Example 32 - Addition of Siltem 1500 (PEI-siloxane copolymer) and Ultem during melt processing 1000 (PEI) Preparation of 5 kg of polyaryletherketone of Example 22
[0196] In Example 32, a polymer material was prepared according to Example 22. Two additives were then added to the polymer material in a subsequent melt processing step to reduce the stiffness of the polymer material and improve its impact properties. 500 g of Siltema 1500 and 250 g of Ultema 1000 (both available from Sabic, SAUDI BASIC INDUSTRIES CORPORATION (HQ), PO Box 5101, Riyadh 11422, Saudi Arabia) were added to 4.25 kg of the polymer material and fed to the rear feed section of a Coperion ZSK25 twin screw extruder through a separate weight loss feeder at a barrel temperature of 290° C. The resulting mixture was then extruded into two ribbons with a diameter of 4 mm and cooled on a conveyor belt before being pelletized into pellets with a length of 2.0 to 4.0 mm.
[0197] Example 33 - Addition of Siltem 1500 (PEI-siloxane copolymer) and Ultem during melt processing 1000 (PEI) Preparation of 5 kg of polyaryletherketone of Example 22
[0198] In Example 33, a polymer material was prepared according to Example 22. Two additives were then added to the polymer material in a subsequent melt processing step to reduce the stiffness of the polymer material and improve its impact properties. 500 g of Siltema 1500 and 500 g of Ultema 1000 (both available from Sabic, SAUDI BASIC INDUSTRIES CORPORATION (HQ), PO Box 5101, Riyadh 11422, Saudi Arabia) were added to 4.0 kg of the polymer material and fed to the rear feed section of a Coperion ZSK25 twin screw extruder through a separate weight loss feeder at a barrel temperature of 290° C. The resulting mixture was then extruded into two ribbons with a diameter of 4 mm and cooled on a conveyor belt before being pelletized into pellets with a length of 2.0 to 4.0 mm.
[0199] Example 34 - Differential Scanning Calorimetry (DSC) of Examples 22, 23, 25, 27, 28 and 29
[0200] The melting temperature (Tm), crystallization temperature (Tc), glass transition temperature (Tg) and heat of fusion (ΔH) of Examples 22, 23, 25, 27, 28 and 29 were determined using another differential scanning calorimetry (DSC) according to ISO 11357. The instrument used was a TA Instruments Q200.
[0201] The thermal cycle is:
[0202] First thermal cycle: 20.0℃ from 50.0℃ to 320.0℃, isothermal for 5 minutes
[0203] · First cooling cycle*: 20.0℃ from 320.0℃ to 50.0℃, isothermal for 5 minutes
[0204] Second thermal cycle: 50.0℃ to 320.0℃ at 20.0℃, isothermal for 5 minutes
[0205] Tm is the peak temperature at which the melting endotherm reaches a maximum in the second thermal scan.
[0206] Tc is the peak temperature of the crystallization exotherm obtained from the first cold scan.
[0207] The glass transition temperature (Tg), onset and midpoint were determined in the second thermal scan.
[0208] The melting enthalpy ΔH was determined in the second thermal scan and the area was calculated by plotting a linear baseline from just above Tg (157°C) to a temperature above the last endotherm.
[0209] The mass normalized heat of fusion is calculated by dividing the enthalpy by the mass of the sample (J / g). The level of crystallinity (%) is determined by dividing the heat of fusion of the sample by 130 J / g. This value of 130 J / g is the heat of fusion of fully crystalline PEEK and is used as a reference value for this measurement.
[0210] Table 9 shows the glass transition temperature (Tg), melting temperature (Tm) and Tc measured during the cooling cycle, which is the temperature at which the crystallization exotherm reaches a minimum. The heat of fusion (ΔHm) of melting is obtained by connecting two points of the melting endotherm that deviate from a relatively straight baseline. The integrated area under the endotherm as a function of time yields the enthalpy of the melting transition (mJ). The mass normalized heat of fusion is calculated by dividing the enthalpy by the mass of the sample (J / g). The level of crystallization (%) is determined by dividing the heat of fusion of the sample by the heat of fusion of a fully crystalline polymer (130 J / g for copolymers).
[0211] As can be seen, the melting temperature of the copolymer is significantly lower than that of Victrex PEEK 150G and Victrex PEEK 450G. This creates a material that is easier to process at lower temperatures, while opening up the possibility of using additives in combination with the copolymer that are not suitable for PEEK polymers due to the higher processing temperatures required to process PEEK.
[0212] Table 9 - Material properties from DSC for Examples 22 and 23 and Comparative Examples
[0213] Tg(℃) Tm(℃) Tc(℃) Crystallinity(%) 150G 144 344 301 34.7 Embodiment 22 147 282 222 22 450G 144 343 290 32.8 Embodiment 23 147 278 207 15.9
[0214] Examples 25, 27, 28 and 29 are copolymer compositions to which Victrex ST45PF is added (Victrex ST45PF is polyetherketoneetherketoneketone PEKEKK). Victrex ST45PF has a melting temperature of about 387°C. By adding ST45PF, the inventors were able to produce polymer materials with reduced crystallization times, as shown in Table 10. As a result, the composition crystallizes much faster than the copolymer itself. One benefit of increasing the crystallization rate of the copolymer is that when making parts from the copolymer, the number of molding cycles can be increased, thereby increasing the number of parts produced per minute.
[0215] Table 10 - Crystallization behavior from Examples 25, 27, 28 and 29
[0216]
[0217] Example 35 - Rheological Measurements
[0218] The melt viscosity of PAEK copolymers can be measured by capillary rheometer using an RH10 capillary rheometer (Malvern Instruments Rosand RH10 Capillary Rheometer) equipped with a 0.5 mm (capillary diameter) × 8.0 mm (capillary length) tungsten carbide die. About 5 grams of copolymer were dried in an air circulating oven at 150°C for 3 hours. The extruder was equilibrated to 400°C. The dried polymer was loaded into the heated barrel of the extruder, the brass end (12 mm long × 9.92 ± 0.01 mm diameter) was placed on the top of the polymer, and the piston and screw were manually turned until the seal of the pressure gauge just engaged the piston to help clear any trapped air. The polymer column was allowed to heat and melt for at least 10 minutes. After the preheating stage, the screw began to rotate, causing the molten polymer to be extruded through the die at the desired shear rate to form thin fibers, while the pressure (P) required to extrude the polymer was recorded. The melt viscosity is given by
[0219]
[0220] Where P = pressure / kN m -2
[0221] L = mold length / m
[0222] S = punching speed / ms -1
[0223] A=Cylinder cross-sectional area / m 2
[0224] r = mold radius / m
[0225] The relationship between shear rate and other parameters is expressed by the following equation:
[0226] Apparent wall shear rate = 4Q / πr 3
[0227] Where Q = volume flow rate / m 3 s -1 =SA.
[0228] Therefore, by adjusting the punch speed S, the -1 ) to measure the viscosity of the molten polymer.
[0229] Figure 1 and Figure 2 The shear viscosity behavior of Examples 22 and 23 using the method described in Example 35 above is shown. Comparative examples are also shown, including comparative shear rheology information for Victrex 150G and Victrex 450G (available from Victrex Manufacturing Limited, Victrex Technology Centre, Thornton Cleveleys, UK). Comparative examples from other PAEK suppliers are also shown (e.g., KT880 from Solvay Speciality Polymers USA, LLC, 4500 McGinnis Ferry Road, Alpharetta, Georgia, USA, and L4000 from Evonik Industries AG, Rellinghauser Straβe 1-11, 45128 Essen, Germany). Examples 22 and 23 show flow properties between comparative polyetheretherketones.
[0230] The low shear rate viscosity of polymer materials (0.006s -1 to 628.319s -1 ) can be measured using a rotational rheometer, using TA Instruments TM Discovery Hybrid Rheometer-2 (DHR-2) rotational rheometer. The rheometer is equipped with an environmental test chamber (ETC), 25 mm stainless steel parallel plates and a 25 mm stainless steel stepped lower ETC plate. 1.6 grams of copolymer was dried in an air circulation oven at 150°C for about 3 hours. The extruder was equilibrated to the test temperature (usually 300-400°C).
[0231] The dried copolymer was loaded into the melt ring wrapped around the stepped portion of the lower plate. Once the temperature of the chamber returned to the test temperature, a delay of 3 minutes was sufficient to melt the copolymer, upon which the melt ring was removed. The gap between the two plates was closed at a rate of 200 μm / s until the gap size was 1075 μm. After a further delay of 2 minutes, the excess polymer material was removed from the gap using a 6 mm trimming tool. Once trimmed, the gap was closed again at a rate of 200 μm / s to 1000 μm before starting the test.
[0232] The viscosity is given by:
[0233]
[0234] in:
[0235] M = torque / Nm -1
[0236] K σ = stress constant
[0237] Ω = motor angular velocity / rad s -1
[0238] K γ = strain constant.
[0239] For parallel plates,
[0240] in:
[0241] r = radius of the plate / m
[0242] h = gap size / m.
[0243] For parallel plates,
[0244] in:
[0245] r = radius of the plate / m.
[0246] In order to determine the shear viscosity over a range of shear rates, a dynamic oscillation experiment was performed. The torque was kept constant and the frequency was swept logarithmically from high to low (usually from 100 Hz to 0.01 Hz), taking 5 points per order of magnitude. The complex viscosity was determined as:
[0247]
[0248] in:
[0249] G*=complex modulus / Pa
[0250] ω = angular frequency / rad s -1 .
[0251] Complex viscosity can be converted to viscosity via the Cox-Merz rule, giving viscosity as a function of shear rate.
[0252] COX-Merz rule for linear polymers: η*(ω)=η(γ)@γ=ω
[0253] Where γ = shear rate / s -1 .
[0254] Figure 2 The rheological properties of Examples 22 and 23 are shown in comparison with Victrex PEEK 150G, Victrex PEEK 450G and Victrex PEEK 650G (all available from Victrex Manufacturing Limited).The copolymers according to the invention show similar rheological behavior to known PEEK.
[0255] Example 36 - Mechanical Properties
[0256] The mechanical properties of the compositions of Examples 22, 23, 26, 30 and 32 were tested at 23° C. using a Type 1A (ISO 3167) test bar according to ISO standards: tensile properties ISO 527, flexural properties ISO 178 and impact strength properties ISO 180 / A.
[0257] Table 11 shows the tensile mechanical properties of Examples 22, 23 and 26. The copolymers show good tensile strength properties close to Victrex PEEK 450G.
[0258] Table 11 - Mechanical properties
[0259] ISO tensile modulus, (Young's) GPa ISO tensile strength, MPa 450G 3.7 98 Embodiment 22 3.5 90 Embodiment 23 3.4 82 Embodiment 26 3.1 90
[0260] Table 12 shows the mechanical properties of immiscible blends comprising the copolymer and the elastomer Hytrel 5555HS (TPC-ET). By incorporating small amounts of Hytrel 5555HS (TPC-ET) in the composition, improved impact resistance is observed.
[0261] Table 12 - Mechanical Properties of Immiscible Blend Compositions
[0262]
[0263] Table 13 shows the mechanical properties of immiscible blends comprising copolymers and the elastomers Siltem and Ultem. By incorporating small amounts of Siltem and Ultem in the composition, improved impact resistance is observed.
[0264] Table 13 - Mechanical Properties of Miscible Blend Compositions
[0265]
[0266] Emphasis is placed on all materials and documents related to the present application which are filed concurrently with or prior to this specification and which are open to public inspection with this specification, and the contents of all these materials and documents are incorporated herein by reference.
[0267] All features disclosed in this specification (including any accompanying claims and drawings), and / or all steps of any method or process so disclosed, may be combined in any combination, except combinations where at least some of such features and / or steps are mutually exclusive.
[0268] Unless otherwise expressly stated, each feature disclosed in this specification (including any attached claims and drawings) may be replaced by alternative features for the same, equivalent or similar purposes. Therefore, unless otherwise expressly stated, each feature disclosed is only an example of a general series of equivalent or similar features.
[0269] The present invention is not limited to the detailed description of the foregoing embodiments. The present invention extends to any novel one or any novel combination of the features disclosed in this specification (including any attached claims and drawings), or to any novel one or any novel combination of the steps of any method or process disclosed in this manner.
Claims
1. A copolymer consisting of a repeating unit of formula I and a repeating unit and a terminal unit of formula II, -O-Ph-O-Ph-CO-Ph-I wherein the molar ratio of the repeating unit of formula I to the repeating unit of formula II is 55:45 to 95:5; and wherein the repeating units of formula I consist of 50 to 90 mol % of repeating units of formula III and 10 to 50 mol % of repeating units of formula IV, repeating units of formula V or a mixture thereof, The repeating unit of formula IV is And the repeating unit of formula V is 2. The copolymer according to claim 1, wherein The molar ratio of the repeating unit of formula I to the repeating unit of formula II is 60:40 to 90:
10.
3. The copolymer according to claim 1, wherein The molar ratio of the repeating unit of formula I to the repeating unit of formula II is 70:30 to 90:
10.
4. The copolymer according to claim 1, wherein The molar ratio of the repeating unit of formula I to the repeating unit of formula II is 80:20 to 90:
10.
5. The copolymer according to any one of claims 1 to 4, wherein The repeating units of formula I consist of a combination of 65 to 90 mol % of repeating units of formula III and 10 to 35 mol % of repeating units of formula IV, repeating units of formula V, or a mixture thereof.
6. The copolymer according to claim 5, wherein The repeating unit of formula I consists of a combination of 80 to 90 mol % of the repeating unit of formula III and 10 to 20 mol % of the repeating unit of formula IV, the repeating unit of formula V or a mixture thereof.
7. The copolymer according to claim 1, wherein The molar ratio of the repeating unit of formula I to the repeating unit of formula II is 90:10 to 80:20, and wherein the repeating unit of formula I consists of a combination of 80 to 90 mol % of the repeating unit of formula III and 10 to 20 mol % of the repeating unit of formula IV, the repeating unit of formula V or a mixture thereof.
8. The copolymer according to claim 1, wherein The copolymer does not include repeating units of formula IV.
9. The copolymer according to claim 1, wherein The copolymer does not include repeating units of formula V.
10. The copolymer according to claim 1, wherein The terminal unit is identical to the repeating unit of the copolymer but terminates with a terminal -OH or -F moiety.
11. The copolymer according to claim 10, wherein In addition to the terminal units which are identical to the repeating units of the copolymer but terminated with a terminal -OH or -F moiety, the terminal units also include As a terminal unit.
12. A method for producing a copolymer according to any one of the preceding claims, the method comprising polycondensing 4,4'-difluorobenzophenone with a mixture of dihydroxy compounds consisting of 1,4-dihydroxybenzene, 4,4'-dihydroxybiphenyl and at least one of 1,3-dihydroxybenzene and 1,2-dihydroxybenzene; wherein the dihydroxy compounds are in the molar proportion required to provide the copolymer according to claim 1; wherein the molar ratio of (4,4'-difluorobenzophenone) / (dihydroxy compound) is from 1.005 to 1.05; and The polycondensation is carried out in the presence of particulate sodium carbonate and potassium carbonate in an aromatic sulfone solvent.
13. The method according to claim 12, wherein: The polycondensation is stopped with a lithium salt and wherein the copolymer is end-capped by adding further 4,4'-difluorobenzophenone.
14. The method according to claim 12 or 13, wherein: a) after polycondensation, adding an additive to the reaction mixture and stirring for at least 5 minutes; and optionally, wherein the additive is polyaryletherketone PAEK, the PAEK having a melting temperature at least 20°C higher than the melting temperature of the copolymer as measured by differential scanning calorimetry, wherein the PAEK comprises 0.1% to 10% by weight of the total weight of the reaction mixture; or b) after the purification step, adding an additive to the copolymer in a melt compounding process to form a composition; and optionally, wherein the additive is polyaryletherketone PAEK, the PAEK having a melting temperature at least 20°C higher than the melting temperature of the copolymer as measured by differential scanning calorimetry, wherein the PAEK accounts for 0.1% to 10% of the total weight of the composition.
15. Use of a copolymer according to any one of claims 1 to 11 as a building material in an additive manufacturing process.
16. A method for manufacturing a three-dimensional component from powders selectively sintered using electromagnetic radiation, wherein: The powder comprises or consists of the copolymer according to any one of claims 1 to 11.
17. A powder as a building material for selective sintering of powders by means of electromagnetic radiation to produce three-dimensional parts from powders, the powder comprising or consisting of a copolymer as claimed in any one of claims 1 to 11.
18. A molded or extruded part comprising or consisting of a copolymer as claimed in any one of claims 1 to 11.
19. A method for reducing isothermal crystallization time, wherein: The isothermal crystallization time is determined by differential scanning calorimetry, the method comprising: a) selecting a copolymer according to any one of claims 1 to 11, and selecting a polyaryletherketone (PAEK) having a melting temperature at least 20°C higher than the melting temperature of the copolymer, and melt processing the copolymer and the PAEK to form a composition, wherein the copolymer comprises 90% to 99.9% by weight of the composition and the PAEK comprises 0.1% to 10% by weight of the composition.