A microwave-guided in-situ gallium metal oxide-coated ternary positive electrode material and preparation method thereof
By coating the ternary cathode material with in-situ gallium metal oxide guided by microwaves, the structural stability and electrolyte erosion problems of nickel-rich ternary layered transition metal oxides in lithium-ion batteries are solved, and the transport of Li+ is promoted. Improved battery cycle and rate performance.
Patent Information
- Application Number
- CN202310082441.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-02-08
AI Technical Summary
Nickel-rich ternary layered transition metal oxides have problems such as poor structural stability, electrolyte erosion, and increased internal resistance in lithium-ion batteries, which affect their commercial application, and existing inorganic non-gallium metal oxide coating materials It hinders the transmission of Li+ and affects battery performance.
A method for preparing microwave-guided in-situ gallium metal oxide-coated ternary cathode material, by coating the surface of the ternary cathode material with a single layer of inorganic gallium metal oxide and synthesizing it using a microwave hydrothermal reaction method to enhance the stability of the material. and structural uniformity to promote Li+ transport.
It effectively avoids the side reaction between the ternary cathode material and the electrolyte, improves the cycle performance and rate performance of the battery, and improves the stability and performance of the lithium-ion battery.
Smart Images

Figure BDA0004067840050000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery positive electrode, and in particular to a microwave-guided in-situ gallium metal oxide-coated ternary positive electrode material and a preparation method thereof. Background Art
[0002] In recent years, with the demand for high energy density batteries, batteries have become thinner and lighter. Nickel (Ni)-rich ternary layered transition metal oxides (LiNi x Co y M 1-x-y O 2 , M=Mn or Al) has become a hot topic in current research due to its superior energy density and low cost. However, the application of Ni-rich ternary layered transition metal oxides mainly faces the following three problems: (1) Due to the occupation of Li by transition metals + Vacancies cause the lattice to distort, resulting in poor structural stability of the material; (2) the erosion of the electrolyte causes some transition metals in the material to dissolve; (3) after the decomposition of the electrolyte at the positive electrode, a SEI film will be formed, resulting in increased internal resistance. It is precisely because of the existence of these defects that the commercial application of Ni-rich ternary layered transition metal oxides is subject to certain restrictions.
[0003] At present, the main electrolyte lithium salt in lithium-ion batteries is lithium hexafluorophosphate (LiPF 6 ), LiPF 6 The thermal stability is poor and it is easy to undergo hydrolysis reaction with water to generate hydrogen fluoride (HF). HF will corrode the positive electrode material, dissolve the transition metal ions in the material, cause the crystal phase change, and deteriorate the battery performance. By coating a layer of inorganic non-gallium metal oxide on the surface of the ternary layered transition metal oxide material, the side reactions between the electrolyte and the ternary positive electrode material can be effectively reduced, thereby improving the stability of the lithium-ion battery during the cycle. Currently, inorganic non-metallic oxides, fluorides, phosphates, etc. are mainly used as coating materials for ternary layered transition metal oxides, including: silicon dioxide, cobalt oxide, molybdenum oxide, zirconium oxide, zinc oxide, aluminum oxide, aluminum fluoride, manganese phosphate, etc. Although they can well protect the positive electrode material from being corroded by the electrolyte, most of them are not conductive, which to a certain extent hinders Li + Transport on the surface of the positive electrode material, thus affecting the performance of the lithium battery. Summary of the invention
[0004] The coating materials based on the ternary layered transition metal oxides in the background technology hinder the Li + In order to solve the technical problem that the transmission on the surface of the positive electrode material affects the performance of the lithium battery, the present invention proposes a microwave-guided in-situ gallium metal oxide-coated ternary positive electrode material and a preparation method thereof.
[0005] A ternary cathode material coated with in-situ gallium metal oxide guided by microwave and a preparation method thereof proposed by the present invention include the following steps:
[0006] S1. Mix a ternary cathode material precursor, a lithium source, deionized water, ethanol, and ethyl acetoacetate evenly to obtain a mixed solution;
[0007] S2. Add a gallium source to the mixed solution and perform a microwave hydrothermal reaction under microwave conditions;
[0008] S3. Filter the mixed solution after the microwave hydrothermal reaction to obtain a product, wash and dry the product, and then sinter it to obtain a ternary cathode material coated with inorganic gallium metal oxide.
[0009] In a preferred embodiment of the present invention, in step S1, the ternary cathode material precursor, the lithium source, deionized water, ethanol, and ethyl acetoacetate are mixed evenly in an ultrasonic microwave synergistic chemical reactor. The temperature of the ultrasonic microwave synergistic chemical reactor is 150-180 °C, and the mixing time is 5-10 h.
[0010] In a preferred embodiment of the present invention, in step S1, the chemical formula of the ternary cathode material precursor is Ni x Co y Mn z (OH) 2 , where: 0.4 < x < 1, 0 < y < 0.4, 0 < z < 1, and x + y + z = 1; preferably, 0.6 ≤ x < 1, 0.05 ≤ y < 0.2, 0.05 ≤ z < 0.2, and x + y + z = 1.
[0011] In a preferred embodiment of the present invention, in step S1, the lithium source is lithium acetate, and the molar ratio of the sum of Ni, Co, and Mn elements in the ternary cathode material precursor to Li in the lithium source is 1:1.01-1.10; preferably, the molar ratio of the sum of Ni, Co, and Mn elements in the ternary cathode material precursor to Li in the lithium source is 1:1.02-1.06.
[0012] In a preferred embodiment of the present invention, in step S1, the volume ratio of deionized water, ethanol, and ethyl acetoacetate is 1:1:1-3; preferably, the volume ratio of deionized water, ethanol, and ethyl acetoacetate is 1:1:2.
[0013] In a preferred embodiment of the present invention, in step S2, the gallium source is gallium isopropoxide, and the coating amount is 500-2000 ppm; preferably, the coating amount is 1000-1500 ppm.
[0014] In a preferred embodiment of the present invention, in step S2, the temperature of the microwave hydrothermal reaction is 100-200°C, and the reaction time is 5-20h; preferably, the temperature of the microwave hydrothermal reaction is 150-180°C, and the reaction time is 5-10h.
[0015] In a preferred embodiment of the present invention, in step S3, the washing is performed several times using ethanol, the drying temperature is 50-100°C, and the drying time is 2-6h; preferably, the drying temperature is 60-80°C, and the drying time is 3-5h.
[0016] In a preferred embodiment of the present invention, in step S3, the sintering is carried out in an air atmosphere or an oxygen atmosphere, the sintering temperature is 400-1000°C, and the sintering time is 5-20h; preferably, the sintering temperature is 500-700°C, and the sintering time is 10-10h.
[0017] The present invention also provides a microwave-guided in-situ gallium metal oxide-coated ternary positive electrode material, which is prepared by the above-mentioned preparation method.
[0018] The present invention proposes a microwave-guided in-situ gallium metal oxide-coated ternary cathode material preparation method. By coating a layer of inorganic gallium metal oxide on the surface of the ternary cathode material, the side reaction between the ternary cathode material and the electrolyte can be effectively avoided, thereby enhancing the stability of the material and improving the cycle performance of the battery; the microwave hydrothermal synthesis method can directly supply energy to the molecules without obvious temperature gradient. The system is uniform and the particle size is uniformly distributed, which can effectively improve the structural uniformity and stability of the ternary cathode material. At the same time, the inorganic gallium metal oxide coating can well promote the Li + transmission, improving the cycle performance and rate performance of lithium-ion batteries. DETAILED DESCRIPTION
[0019] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0020] Embodiment 1:
[0021] A microwave-guided in-situ gallium metal oxide-coated ternary positive electrode material and a preparation method thereof, comprising the following steps:
[0022] S1. Add a mixed solvent of deionized water, ethanol and ethyl acetoacetate into an ultrasonic microwave synergistic chemical reactor. The volume ratio of deionized water, ethanol and ethyl acetoacetate is 500 mL: 500 mL: 1000 mL. Then, 300 g of NCM60-05-35 precursor (the molar ratio of Ni, Co and Mn is 60%, 5% and 35%) and 221 g of CH3 COOLi is evenly dispersed in the above solvents, and the mixture is evenly mixed by using the rapid selective heating of microwaves and the principle of ultrasonic oscillation to obtain a mixed solution;
[0023] S2, adding 1.06g of gallium isopropoxide to the mixed solution, stirring evenly, and then charging the solution into a microwave hydrothermal synthesis reactor, setting the temperature to 180°C, and keeping the temperature for 15h;
[0024] S3. Collect the samples after the insulation in a beaker, wash them with ethanol, and then put them in an oven for drying. The oven temperature is set to 80°C and the drying time is 5 hours. Put the dried samples into a sagger and then into a muffle furnace. Heat the temperature to 850°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with an air flow rate of 0.6m 3 / h; the sintered sample is crushed and sieved to obtain the lithium metagallate-coated ternary positive electrode material.
[0025] Embodiment 2:
[0026] A microwave-guided in-situ gallium metal oxide-coated ternary positive electrode material and a preparation method thereof, comprising the following steps:
[0027] S1. Add a mixed solvent of deionized water, ethanol and ethyl acetoacetate into an ultrasonic microwave synergistic chemical reactor. The volume ratio of deionized water, ethanol and ethyl acetoacetate is 500 mL: 500 mL: 1000 mL. Then, 300 g of NCM60-05-35 precursor (the molar ratio of Ni, Co and Mn is 60%, 5% and 35%) and 221 g of CH 3 COOLi is evenly dispersed in the above solvents, and the mixture is evenly mixed by using the rapid selective heating of microwaves and the principle of ultrasonic oscillation to obtain a mixed solution;
[0028] S2, adding 2.12g of gallium isopropoxide to the mixed solution, stirring evenly, and then charging the solution into a microwave hydrothermal synthesis reactor, setting the temperature to 180°C, and keeping the temperature for 15h;
[0029] S3. Collect the samples after the insulation in a beaker, wash them with ethanol, and then put them in an oven for drying. The oven temperature is set to 80°C and the drying time is 5 hours. Put the dried samples into a sagger and then into a muffle furnace. Heat the temperature to 850°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with an air flow rate of 0.6m 3 / h; the sintered sample is crushed and sieved to obtain the lithium metagallate-coated ternary positive electrode material.
[0030] Embodiment 3:
[0031] A microwave-guided in-situ gallium metal oxide-coated ternary positive electrode material and a preparation method thereof, comprising the following steps:
[0032] S1. Add a mixed solvent of deionized water, ethanol and ethyl acetoacetate into an ultrasonic microwave synergistic chemical reactor. The volume ratio of deionized water, ethanol and ethyl acetoacetate is 500 mL: 500 mL: 1000 mL. Then, 300 g of NCM60-05-35 precursor (the molar ratio of Ni, Co and Mn is 60%, 5% and 35%) and 221 g of CH 3 COOLi is evenly dispersed in the above solvents, and the mixture is evenly mixed by using the rapid selective heating of microwaves and the principle of ultrasonic oscillation to obtain a mixed solution;
[0033] S2, adding 1.59 g of gallium isopropoxide to the mixed solution, stirring evenly, and then charging the solution into a microwave hydrothermal synthesis reactor, setting the temperature to 180° C. and keeping the temperature for 15 h;
[0034] S3. Collect the samples after the insulation in a beaker, wash them with ethanol, and then put them in an oven for drying. The oven temperature is set to 80°C and the drying time is 5 hours. Put the dried samples into a sagger and then into a muffle furnace. Heat the temperature to 850°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with an air flow rate of 0.6m 3 / h; the sintered sample is crushed and sieved to obtain the lithium metagallate-coated ternary positive electrode material.
[0035] Embodiment 4:
[0036] A microwave-guided in-situ gallium metal oxide-coated ternary positive electrode material and a preparation method thereof, comprising the following steps:
[0037] S1. Add a mixed solvent of deionized water, ethanol and ethyl acetoacetate into an ultrasonic microwave synergistic chemical reactor. The volume ratio of deionized water, ethanol and ethyl acetoacetate is 500 mL: 500 mL: 1000 mL. Then, 300 g of NCM60-05-35 precursor (the molar ratio of Ni, Co and Mn is 60%, 5% and 35%) and 221 g of CH 3 COOLi is evenly dispersed in the above solvents, and the mixture is evenly mixed by using the rapid selective heating of microwaves and the principle of ultrasonic oscillation to obtain a mixed solution;
[0038] S2, adding 1.06g of gallium isopropoxide to the mixed solution, stirring evenly, and then charging the solution into a microwave hydrothermal synthesis reactor, setting the temperature to 180°C, and keeping the temperature for 15h;
[0039] S3. Collect the samples after the insulation in a beaker, wash them with ethanol, and then put them in an oven for drying. The oven temperature is set to 80°C and the drying time is 5 hours. Put the dried samples into a sagger and then into a muffle furnace. Heat the temperature to 850°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with an air flow rate of 0.6m 3 / h; the sintered sample is crushed and sieved to obtain the lithium metagallate-coated ternary positive electrode material.
[0040] Embodiment 5:
[0041] A microwave-guided in-situ gallium metal oxide-coated ternary positive electrode material and a preparation method thereof, comprising the following steps:
[0042] S1. Add a mixed solvent of deionized water, ethanol and ethyl acetoacetate into an ultrasonic microwave synergistic chemical reactor. The volume ratio of deionized water, ethanol and ethyl acetoacetate is 500 mL: 500 mL: 1000 mL. Then, 300 g of NCM60-05-35 precursor (the molar ratio of Ni, Co and Mn is 60%, 5% and 35%) and 221 g of CH 3 COOLi is evenly dispersed in the above solvents, and the mixture is evenly mixed by using the rapid selective heating of microwaves and the principle of ultrasonic oscillation to obtain a mixed solution;
[0043] S2, adding 1.06g of gallium isopropoxide to the mixed solution, stirring evenly, and then charging the solution into a microwave hydrothermal synthesis reactor, setting the temperature to 180°C, and keeping the temperature for 15h;
[0044] S3. Collect the samples after the insulation in a beaker, wash them with ethanol, and then put them in an oven for drying. The oven temperature is set to 80°C and the drying time is 5 hours. Put the dried samples into a sagger and then into a muffle furnace. Heat the temperature to 750°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with an air flow rate of 0.6m 3 / h; the sintered sample is crushed and sieved to obtain the lithium metagallate-coated ternary positive electrode material.
[0045] Comparative Example 1:
[0046] S1. Add a mixed solvent of deionized water, ethanol and ethyl acetoacetate into an ultrasonic microwave synergistic chemical reactor, wherein the volume ratio of deionized water, ethanol and ethyl acetoacetate is 500 mL: 500 mL: 1000 mL, then evenly disperse 300 g of NCM60-05-35 precursor (the molar ratio of Ni, Co and Mn is 60%, 5% and 35%) and 221 g of CH3COOLi into the above solvent, and mix them evenly by using the rapid selective heating of microwaves and the principle of ultrasonic oscillation to obtain a mixed solution;
[0047] S2, the mixed solution was placed into a microwave hydrothermal synthesis reactor, the temperature was set to 180°C, and the insulation time was 15h;
[0048] S3. Collect the samples after the insulation in a beaker, wash them with ethanol, and then put them in an oven for drying. The oven temperature is set to 80°C and the drying time is 5 hours. Put the dried samples into a sagger and then into a muffle furnace. Heat the temperature to 850°C at a heating rate of 2°C / min and keep it warm for 15 hours. At the same time, compressed air is continuously introduced during the entire reaction process with an air flow rate of 0.6m 3 / ; The sintered sample is crushed and sieved to obtain the ternary positive electrode material.
[0049] The positive electrode materials obtained in Example 1, Example 2, Example 3, Example 4, Example 5, and Comparative Example 1 were respectively prepared with conductive carbon black and PVDF in a ratio of 90:5:5, and NMP was used as a solvent to mix them evenly, and then they were evenly coated on aluminum foil to make button batteries to test their electrochemical properties: the test was carried out at room temperature 25°C, and the first five weeks were charged and discharged at 0.2C / 0.2C, 0.33C / 0.33C, 1C / 1C, 2C / 2C, and 5C / 5C, and then charged and discharged at 1C / 1C, and cycled 50 times. All test voltage ranges were between 2.8-4.45V, and the button battery performance data are shown in Table 1:
[0050] Table 1
[0051]
[0052] It can be seen from the results in Table 1 that by coating a single layer of inorganic gallium metal oxide on the surface of the ternary positive electrode material, the side reaction between the ternary positive electrode material and the electrolyte can be effectively avoided, thereby enhancing the stability of the material and improving the cycle performance of the battery.
[0053] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a microwave-guided in-situ gallium metal oxide-coated ternary cathode material, characterized in that: The following steps are involved: S1. Evenly mix the ternary cathode material precursor, lithium source, deionized water, ethanol, and ethyl acetoacetate to obtain a mixed solution; S2, adding a gallium source to the mixed solution, and performing a microwave hydrothermal reaction under microwave conditions; S3, filtering the mixed solution after the microwave hydrothermal reaction to obtain a product, washing the product, drying it, and then sintering it to obtain a ternary positive electrode material coated with an inorganic gallium metal oxide; In step S1, the ternary cathode material precursor, lithium source, deionized water, ethanol, and ethyl acetoacetate are uniformly mixed in an ultrasonic-microwave-assisted chemical reactor. The temperature of the ultrasonic-microwave-assisted chemical reactor is 150-180° C., and the mixing time is 5-10 hours. In step S2, the temperature of the microwave hydrothermal reaction is 150-180° C., and the reaction time is 5-10 h; In step S3, sintering is performed in an air atmosphere at a sintering temperature of 400-1000° C. and a sintering time of 5-20 h; In step S1, the chemical formula of the ternary cathode material precursor is Ni x Co y Mn z (OH)2, of which: 0.4 <x<1,0<y<0.4,0<z<1,x+y+z=1。 2. The method for preparing the microwave-guided in-situ gallium metal oxide-coated ternary cathode material according to claim 1, characterized in that: In step S1, the lithium source is lithium acetate, and the molar ratio of the sum of Ni, Co, and Mn elements in the ternary positive electrode material precursor to Li in the lithium source is 1:1.01~1.
10.
3. The method for preparing the microwave-guided in-situ gallium metal oxide-coated ternary cathode material according to claim 1, characterized in that: In step S1, the volume ratio of deionized water, ethanol, and ethyl acetoacetate is 1:1:1-3.
4. The method for preparing a microwave-guided in-situ gallium metal oxide-coated ternary cathode material according to claim 1, characterized in that: In step S2, the gallium source is gallium isopropoxide, and the coating amount is 500-2000 ppm.
5. The method for preparing a microwave-guided in-situ gallium metal oxide-coated ternary cathode material according to claim 1, characterized in that: In step S3, the washing is performed by using ethanol for several times, the drying temperature is 50-100° C., and the drying time is 2-6 hours.
6. A microwave-guided in-situ gallium metal oxide-coated ternary cathode material, prepared by the preparation method according to any one of claims 1 to 5.