Resin composition

By using thermoplastic plastomers with appropriate acid values ​​and acid-modified polyolefin resins in the resin composition, combined with hollow particles of highly cross-linkable monomers, the problem of reduced physical properties of the resin composition during the molding process is solved and achieved. High mechanical strength and lightweight molded body.

CN116234869BActive Publication Date: 2024-10-11ZEON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180064582.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2021-09-28
Publication Date
2024-10-11
Estimated Expiration
2041-09-28

AI Technical Summary

Technical Problem

Resin compositions containing resin and hollow particles are prone to decrease in physical properties such as tensile strength and flexural strength during the molding process.

Method used

A thermoplastic elastomer with an acid value of less than 3.0 mgKOH/g and an acid-modified polyolefin resin with an acid value of 3.5 mgKOH/g or more are used. The shell of the hollow particles contains 30 to 100 parts by mass of cross-linkable monomer units, and the acid The weight average molecular weight of the modified polyolefin-based resin is 15,000 or more. The combination of these components forms good interfacial adhesion and suppresses a decrease in physical properties.

Benefits of technology

It forms good interface adhesion in the molded body, improves the mechanical strength, prevents the hollow particles from being broken, extends the applicable temperature and pressure range of the molding process, suppresses the decrease in physical properties, and realizes a lightweight molded body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004136850590000321
    Figure BDA0004136850590000321
  • Figure BDA0004136850590000361
    Figure BDA0004136850590000361
  • Figure HDA0004136850630000011
    Figure HDA0004136850630000011
Patent Text Reader

Abstract

The present invention provides a resin composition that suppresses the reduction of physical properties when a molded body is formed even if hollow particles are included. The resin composition of the present invention comprises a thermoplastic plastomer having an acid value of less than 3.0 mgKOH / g, hollow particles, and an acid-modified polyolefin resin having an acid value of 3.5 mgKOH / g or more, wherein the hollow particles have a shell containing a resin and a hollow part surrounded by the shell, and the resin contains a polymer containing 30 to 100 parts by mass of a crosslinking monomer unit in 100 parts by mass of all monomer units.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, and more particularly, to a resin composition containing hollow particles. Background Art

[0002] Hollow particles (hollow resin particles) are particles with a cavity inside. Compared with solid particles that are substantially filled with resin, they can scatter light well and reduce the transmittance of light. Therefore, hollow particles are widely used as organic pigments and masking agents with excellent optical properties such as opacity and whiteness in water-based paints, paper coating compositions, etc., and are also used as lightweight agents and heat-insulating agents for resins, coatings, etc. used in various fields such as automobiles, electrical, electronic, and construction.

[0003] The applicant disclosed a resin composition containing a thermoplastic plastomer and hollow resin particles in Patent Document 1. The hollow resin particles contained in the resin composition disclosed in Patent Document 1 have high porosity and are lightweight, and the shell is formed by a resin with a high crosslinking monomer ratio, so the thermoplasticity of the shell is low, and the hollow resin particles have high mechanical strength even at high temperatures and are not easily broken. Therefore, the change in the porosity of the hollow resin particles of the resin composition disclosed in Patent Document 1 during molding processing is small, and by using the resin composition, it can be stably molded into a lightweight molded body.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent document 1: International Publication No. 2020 / 066704. Summary of the invention

[0007] Problem that the invention aims to solve

[0008] However, conventional resin compositions containing a resin and hollow particles have a problem of reduced physical properties such as tensile strength and flexural strength when formed into a molded body, depending on the type of resin or the production conditions of the resin composition or the molded body, compared with resin compositions not containing hollow particles.

[0009] In view of the above-mentioned actual situation, an object of the present invention is to provide a resin composition in which the deterioration of physical properties when formed into a molded body is suppressed even when the resin composition contains hollow particles.

[0010] Solutions for solving problems

[0011] The present invention provides a resin composition, comprising a thermoplastic plastomer having an acid value of less than 3.0 mgKOH / g, hollow particles, and an acid-modified polyolefin resin having an acid value of 3.5 mgKOH / g or more.

[0012] The hollow particles have a shell composed of a resin and a hollow portion surrounded by the shell, and the resin contains a polymer containing 30 to 100 parts by mass of a crosslinkable monomer unit in 100 parts by mass of all monomer units.

[0013] In the resin composition of the present invention, the content of the acid-modified polyolefin-based resin is preferably 10 to 150 parts by mass based on 100 parts by mass of the hollow particles.

[0014] In the resin composition of the present invention, the acid-modified polyolefin-based resin preferably has a weight average molecular weight of 15,000 or more.

[0015] In the resin composition of the present invention, the acid-modified polyolefin-based resin is preferably a carboxylic acid-modified polyolefin-based resin.

[0016] In the resin composition of the present invention, the thermoplastic plastomer is preferably a polyolefin-based resin.

[0017] Effects of the Invention

[0018] The present invention can provide a resin composition in which the degradation of physical properties when formed into a molded body is suppressed even if the composition contains hollow particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic diagram showing one embodiment of a method for producing hollow particles used in the present invention.

[0020] Figure 2 Schematic diagram showing one embodiment of the suspension in the suspension preparation step. DETAILED DESCRIPTION

[0021] In addition, in the present invention, "to" in a numerical range means that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0022] In the present invention, (meth)acrylate refers to acrylate and methacrylate, (meth)acrylic acid refers to acrylic acid and methacrylic acid, and (meth)acryloyl refers to acryloyl and methacryloyl, respectively.

[0023] Hereinafter, the resin composition of the present invention and the molded article of the resin composition of the present invention will be described in order.

[0024] 1. Resin composition

[0025] The resin composition of the present invention is characterized by comprising: a thermoplastic plastomer having an acid value of less than 3.0 mgKOH / g, hollow particles, and an acid-modified polyolefin resin having an acid value of 3.5 mgKOH / g or more.

[0026] The hollow particles have a shell composed of a resin and a hollow portion surrounded by the shell, and the resin contains a polymer containing 30 to 100 parts by mass of a crosslinkable monomer unit in 100 parts by mass of all monomer units.

[0027] Compared with the resin combination that does not comprise hollow particles, the resin combination that comprises resin and hollow particles in the past, when being made into molded body, physical properties such as tensile strength, flexural strength, flexural elastic modulus tend to reduce.It can be considered that in the molded body of the resin combination that comprises resin and hollow particles in the past, because the interface adhesion between resin and hollow particles is low, the interface strength between resin and hollow particles is relatively low, therefore physical properties such as intensity relative to external force are reduced.

[0028] In this regard, the resin composition of the present invention comprises an acid-modified polyolefin resin in combination in a thermoplastic plastomer and hollow particles as resins. In the acid-modified polyolefin resin, the polarity of the polyolefin part is relatively low, and the polarity of the acid-modified part is relatively high. On the other hand, compared with hollow particles, thermoplastic plastomers are usually low in polarity. Therefore, the polyolefin part of the acid-modified polyolefin resin has good affinity with the thermoplastic plastomer, and the acid-modified part of the acid-modified polyolefin resin has good affinity with the hollow particles. It can be inferred that in the resin composition of the present invention comprising such an acid-modified polyolefin resin, a thermoplastic plastomer and hollow particles, the acid-modified polyolefin resin easily enters between the thermoplastic plastomer and the hollow particles, and in the molded body of the resin composition of the present invention, it is easy to form a structure in which the thermoplastic plastomer is present around the hollow particles via the acid-modified polyolefin resin. In the molded body, the adhesion between the hollow particles and the acid-modified polyolefin resin, and the adhesion between the thermoplastic plastomer and the acid-modified polyolefin resin are good, so it can be inferred that the molded body of the resin composition of the present invention is less likely to produce relatively low-strength areas, resulting in the suppression of degradation of physical properties.

[0029] In addition, the hollow particles included in the resin composition of the present invention have a high ratio of crosslinkable monomer units in the shell, so the thermoplasticity of the shell is low, and the mechanical strength is also high even at high temperatures. Therefore, even under high temperature and high pressure environments during the molding of the resin composition of the present invention, the hollow particles are not easily broken, and the change in the porosity of the hollow particles is also small.

[0030] Therefore, in the resin composition of the present invention, regardless of the molding conditions such as extrusion molding and injection molding, the crushing of hollow particles during molding is suppressed, and by using the resin composition of the present invention, a lightweight molded product can be molded.

[0031] Furthermore, since the hollow particles contained in the resin composition of the present invention are not easily broken even under a high-temperature and high-pressure environment, the range of selectable molding processing conditions for the resin composition of the present invention is wide.

[0032] Hereinafter, the thermoplastic plastomer, the hollow particles and the acid-modified polyolefin-based resin contained in the resin composition of the present invention will be described in order.

[0033] [Thermoplastic plastic]

[0034] The resin composition of the present invention contains a thermoplastic plastomer as a resin.

[0035] A plastomer is a material that usually shows no or almost no elastic deformation and has the property of being easily plastically deformed. On the other hand, an elastomer is a material that has the property of instantly deforming in response to an external force and returning to its original shape in a short time when the external force is removed, which is completely opposite to the former.

[0036] In the present invention, the term "thermoplastic plastomer" refers to a polymer having the property of being easily deformed by flow by heating and being solidified into the deformed shape by cooling.

[0037] In the present invention, as a thermoplastic plastomer, the following material can be typically used: in a tensile test, when the original size is taken as 100%, it can be stretched to 200% by a small external force at room temperature (20°C), and even if the external force is removed, the size will not recover to less than 130%. Specifically, the small external force refers to an external force with a tensile strength of 1 to 100 MPa. In more detail, as a thermoplastic plastomer, the following polymer can be used: according to the tensile permanent deformation test of JIS K 6262-1997, in a tensile test at 20°C, it can be stretched to twice the distance between the scale lines of the dumbbell-shaped No. 4 test piece specified in JIS K 6251-1993 before stretching without breaking, and after being stretched to twice the distance between the scale lines before stretching and kept for 60 minutes, the tensile external force is removed, and after 5 minutes, the tensile permanent deformation is 30% or more.

[0038] As the thermoplastic plastomer, a wide range of thermoplastic resins that can be used for conventionally known molding processes can be used, for example: polyvinyl chloride; polyvinylidene chloride; polyvinyl alcohol; ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, ethylene-methyl (meth)acrylate copolymer, ethylene-ethyl (meth)acrylate copolymer, and ethylene-butyl (meth)acrylate copolymer; polyethylene resins such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ultra-low-density polyethylene (ULDPE), medium-density polyethylene, and high-density polyethylene (HDPE); polypropylene homopolymer (PP homopolymer), random polypropylene (PP) and polypropylene copolymer. Polypropylene resins such as propylene (random PP), block polypropylene (block PP), polybutylene resins, polycycloolefins, and propylene-α-olefin copolymers; styrene copolymers such as styrene-acrylonitrile copolymers and styrene-butadiene-acrylonitrile copolymers; polystyrene; polyterpene; polyacetal; polymethyl (meth)acrylate; cellulose acetate; polycarbonate; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; thermoplastic polyurethane; polytetrafluoroethylene resin (PTFE); ionomer resins such as ethylene ionomers, polyurethane ionomers, styrene ionomers, and fluorine ionomers; polyacetal; polyphenylene sulfide, etc. These thermoplastic plastomers can be used alone or in combination of two or more.

[0039] The thermoplastic plastomer contained in the resin composition of the present invention preferably contains a polyolefin resin from the viewpoint of good affinity with the acid-modified polyolefin resin and from the viewpoint of improving the mechanical strength when a molded article is formed.

[0040] Here, the polyolefin resin in the present invention includes a polymer of an olefin, a copolymer of two or more olefins, and a copolymer of one or more olefins and one or more other monomers. In addition, in the polyolefin resin as a copolymer of one or more olefins and one or more other monomers, the copolymerization ratio of olefins is preferably 50 mass % or more.

[0041] Examples of the polyolefin resin include the above-mentioned polyethylene resin, polypropylene resin, polybutene resin, polycycloolefin, and propylene-α-olefin copolymer. Among them, polyethylene resin, polypropylene resin, and propylene-α-olefin copolymer are preferred, and polypropylene resin is particularly preferred.

[0042] Here, for example, the polyethylene resin may be a polyethylene resin obtained by copolymerizing a small amount of an olefin or other monomer other than ethylene. The same is true for the polypropylene resin and the polybutene resin, which may be a polypropylene resin and a polybutene resin obtained by copolymerizing a small amount of an olefin or other monomer other than propylene or butene. The propylene-α-olefin copolymer may be a copolymer of propylene and an α-olefin other than propylene, or a propylene-α-olefin copolymer obtained by copolymerizing a small amount of other monomers. Here, the small amount of copolymerization may be, for example, a copolymerization ratio of 10% by mass or less, or may be 5% by mass or less.

[0043] As the olefin used in the synthesis of the polyolefin resin, an olefin having 2 to 30 carbon atoms is preferred, at least one selected from olefins having 2 to 4 carbon atoms and α-olefins having 5 to 30 carbon atoms is more preferred, and at least one selected from α-olefins having 2 to 10 carbon atoms is further preferred.

[0044] Examples of other monomers other than olefins that can be used in the synthesis of polyolefin-based resins include monomers having 4 to 30 carbon atoms and having an unsaturated bond copolymerizable with olefins, and specific examples thereof include vinyl acetate and the like.

[0045] In the propylene-α-olefin copolymer, the copolymerization ratio of propylene and α-olefin is not particularly limited, and the copolymerization ratio of propylene is preferably 50 to 90% by mass, and more preferably 70 to 90% by mass. In addition, as the α-olefin used in the propylene-α-olefin copolymer, α-olefins having 2 to 6 carbon atoms are preferred, and ethylene and butene are particularly preferred.

[0046] In addition, the acid value of thermoplastic plastomer is less than 3.0mgKOH / g, preferably less than 2.5mgKOH / g. The thermoplastic plastomer having an acid value less than the above-mentioned upper limit value is not easily affected by humidity environment due to water absorption, stable chemical properties, excellent electrical properties, excellent in dielectric constant and power factor in high frequency region, but low in affinity with hollow particles, therefore, in the case of the resin combination in the past for comprising hollow particles, the physical property when resin combination is made into molded body is easily decreased. On the other hand, in resin combination of the present invention, even if the thermoplastic plastomer having an acid value less than the above-mentioned upper limit value is used, the physical property reduction when molded body can be suppressed.

[0047] The lower limit of the acid value of the thermoplastic plastomer is not particularly limited, and may be 0 mgKOH / g or more.

[0048] In the present invention, the acid value of the resin is a value measured in the following order (i) to (iii) according to 3.1 neutralization titration method of JIS K0070.

[0049] (i) 1 g of a measurement sample is dissolved in 100 g of xylene adjusted to 100°C.

[0050] (ii) Titration was performed at the same temperature using phenolphthalein as an indicator with a 0.1 mol / L potassium hydroxide ethanol solution (trade name: 0.1 mol / L ethanolic potassium hydroxide solution, manufactured by Wako Pure Chemical Industries, Ltd.).

[0051] (iii) The amount of potassium hydroxide required for titration is converted into mg, and the acid value (unit: mgKOH / g) is calculated.

[0052] In addition, the solubility parameter (SP value) of the thermoplastic plastomer is preferably 13 (cal / cm 3 ) 1 / 2 Below, more preferably 12 (cal / cm 3 ) 1 / 2 Below, more preferably 10 (cal / cm 3 ) 1 / 2 Thermoplastic plasticizers with an SP value below the above-mentioned upper limit value are less susceptible to humidity environmental influences due to their small water absorption, excellent electrical properties, excellent in terms of dielectric constant and power factor in high-frequency regions, but low in affinity with hollow particles, and therefore, in the case of a conventional resin composition for containing hollow particles, the physical property when the resin composition is made into a molded body is easily reduced. On the other hand, in the resin composition of the present invention, even if a thermoplastic plasticizer with an SP value below the above-mentioned upper limit value is used, the physical property reduction when the molded body is made can be suppressed.

[0053] The lower limit of the SP value of the thermoplastic plastomer is not particularly limited, but is preferably 6 (cal / cm 3 ) 1 / 2 More preferably, 7 (cal / cm 3 ) 1 / 2 above.

[0054] In addition, 1(cal / cm 3 ) 1 / 2 Can be converted to 2.05(J / cm 3 ) 1 / 2 or 2.05(MPa) 1 / 2 .

[0055] In the present invention, the SP value of the resin is a value obtained by the method described in "Polymer Handbook Fourth Edition" compiled by J. Brandrup et al., published by John Wiley & Sons, Inc., 1999, p. 675-714. For cases not described in the above literature, the SP value (δ) is calculated from the statistics (ΣG) of the molar gravitational constant (G), the molecular weight (M) and the specific gravity (d) according to the following formula based on the molar gravitational constant of various atomic groups proposed by Small.

[0056] δ=∑G / V=d∑G / M (δ: SP value, V: specific volume, M: molecular weight, d: specific gravity)

[0057] In the resin composition of the present invention, the content of the thermoplastic plastomer is not particularly limited, and is generally 50 to 95% by mass, preferably 60 to 90% by mass. When the content of the thermoplastic plastomer is above the above lower limit, the moldability of the resin composition is excellent, and the mechanical strength of the obtained molded body can be improved. When the content of the thermoplastic plastomer is below the above upper limit, the hollow particles and the acid-modified polyolefin resin can be fully contained, and therefore, the physical property reduction when the resin composition is made into a molded body can be suppressed, and the mechanical strength can be improved. In addition, the lightweight effect of the molded body is also excellent.

[0058] [Hollow particles]

[0059] The hollow particles contained in the resin composition of the present invention are particles having a shell (outer shell) containing a resin and a hollow portion surrounded by the shell.

[0060] In the present invention, the hollow part is a hollow space clearly distinguishable from the shell of the hollow particle formed of the resin material. The shell of the hollow particle may have a porous structure, in which case the hollow part has a size clearly distinguishable from a plurality of tiny spaces uniformly dispersed in the porous structure.

[0061] Hollow particles may also have one or more hollow parts. In addition, the shell of the hollow particle and, in the case of having two or more hollow parts, the partition wall separating the adjacent hollow parts may be porous. In order to maintain a good balance between the high porosity of the hollow particle and the mechanical strength of the hollow particle, the particle preferably has only one hollow part.

[0062] The hollow part of the hollow particles can be confirmed by, for example, SEM observation of a particle cross section or by direct TEM observation of the particles.

[0063] Furthermore, the hollow part of the hollow particles is preferably filled with a gas such as air.

[0064] Generally, hollow particles include: hollow particles whose shells do not have communicating holes connecting the hollow part with the external space of the particle; and hollow particles whose shells have one or more communicating holes, and the hollow part is connected to the outside of the particle via the communicating holes. Although it also depends on the size of the hollow particles, the diameter of the communicating holes is usually about 10 to 500 nm. In addition, hollow particles sometimes have crack-like shell defects that are extremely large compared to the size of the particles. Although it also depends on the size of the hollow particles, cracks with a length of more than 1 μm usually significantly deteriorate the strength of the hollow particles, and are therefore considered to be shell defects.

[0065] The hollow particles contained in the resin composition of the present invention preferably have 5 or less hollow particles having continuous pores or shell defects among 100 hollow particles in SEM observation, from the viewpoint that the hollow particles are not easily broken during molding of the resin composition.

[0066] The lower limit of the porosity of the hollow particles is preferably 50% or more, more preferably 53% or more, further preferably 55% or more, further preferably 58% or more, and particularly preferably 60% or more. When the porosity of the hollow particles is above the above lower limit, the hollow particles can be lightweight due to the high proportion of the hollow portion. The upper limit of the porosity of the hollow particles is preferably 90% or less, preferably 85% or less, and more preferably 80% or less. When the porosity of the hollow particles is below the above upper limit, the strength reduction of the hollow particles can be suppressed.

[0067] The porosity of the hollow particles was calculated from the apparent density D1 and the true density D0 of the hollow particles according to the following formula (0).

[0068] Formula (0)

[0069] Porosity (%) = I00 - [apparent density D1] / [true density D0] × 100

[0070] The method for measuring the apparent density D1 of the hollow particles is as follows.

[0071] First, in a volume of 100cm 3 Fill the volumetric flask to about 30 cm 3 The mass of the hollow particles was accurately weighed. Next, the volumetric flask filled with the hollow particles was filled with isopropyl alcohol to the mark while being careful not to mix in bubbles. The mass of isopropyl alcohol added to the volumetric flask was accurately weighed, and the apparent density D1 (g / cm 3 ).

[0072] Formula (I)

[0073] Apparent density D1 = [mass of hollow particles] / (100-[mass of isopropyl alcohol] / [specific gravity of isopropyl alcohol at the measurement temperature])

[0074] The apparent density D1 corresponds to the specific gravity of the entire hollow particle when the hollow portion is regarded as a part of the hollow particle.

[0075] The true density D0 of the hollow particles is determined as follows. After the hollow particles are crushed in advance, 3 A volumetric flask is filled with about 10 g of hollow particle fragments, and the mass of the filled fragments is accurately weighed. Then, isopropanol is added to the volumetric flask in the same manner as the above-mentioned apparent density measurement, and the mass of isopropanol is accurately weighed. Based on the following formula (II), the true density D0 (g / cm 3 ).

[0076] Formula (II)

[0077] True density D0 = [mass of hollow particle fragments] / (100 - [mass of isopropanol] / [specific gravity of isopropanol at the measurement temperature])

[0078] The true density D0 corresponds to the specific gravity of only the shell portion of the hollow particle. As can be seen from the above measurement method, when calculating the true density D0, the hollow portion is not considered as a part of the hollow particle.

[0079] The hollow particles preferably do not show a glass transition temperature (Tg) below 250° C. Since the hollow particles do not show a glass transition temperature (Tg) below 250° C., it can be determined that the hollow particles are not easily deformed or broken when heated.

[0080] The glass transition temperature can be measured by differential scanning calorimetry (DSC).

[0081] The lower limit of the volume-based average particle size (volume average particle size) of the hollow particles is preferably 1.0 μm or more, more preferably 3.0 μm or more, further preferably 4.0 μm or more, and particularly preferably 4.5 μm or more, and the upper limit is preferably 60.0 μm or less, more preferably 55.0 μm or less, and further preferably 50.0 μm or less.

[0082] When the volume average particle size of the hollow particles is 1.0 μm or more, the desired porosity can be obtained, so the hollow particles can be lightweight. In addition, when the volume average particle size of the hollow particles is 60.0 μm or less, the hollow particles are not easily broken, so they have high compressive strength.

[0083] The particle size distribution (volume average particle size (Dv) / number average particle size (Dn)) of the hollow particles is not particularly limited, and may be, for example, 1.00 to 2.50. By setting the particle size distribution to 2.50 or less, particles having small deviations between particles in compressive strength characteristics and heat resistance can be obtained. In addition, by setting the particle size distribution to 2.50 or less, when manufacturing products such as molded bodies described later, products with uniform thickness can be manufactured.

[0084] The volume average particle size (Dv) and number average particle size (Dn) of the hollow particles can be measured by, for example, a laser diffraction particle size distribution measuring device to measure the particle size of each hollow particle, and the number average and volume average are calculated, respectively, and the obtained values ​​are used as the number average particle size (Dn) and volume average particle size (Dv) of the particles. The particle size distribution is the value of the volume average particle size divided by the number average particle size.

[0085] The shape of the hollow particles is not particularly limited as long as a hollow portion is formed inside, and examples thereof include spherical, ellipsoidal, and irregular shapes, etc. Among these, a spherical shape is preferred from the viewpoint of easy production.

[0086] The average roundness of the hollow particles may be 0.950 to 0.995.

[0087] In the present invention, roundness is defined as the value obtained by dividing the circumference of a circle having a projection area equal to that of the particle image by the circumference of the projection image of the particle. In addition, the average roundness in the present invention is used as a simple method for quantitatively expressing the shape of the hollow particles, and is an index indicating the degree of concavity and convexity of the hollow particles. When the hollow particles are ideally spherical, the average roundness shows 1, and the more complex the surface shape of the hollow particles is, the smaller the value of the average roundness is.

[0088] The lower limit of the thickness of the shell of the hollow particles of the present invention is preferably 0.1 μm or more, more preferably 0.2 μm or more, and further preferably 0.3 μm or more, and the upper limit is preferably 6 μm or less, more preferably 5 μm or less, and further preferably 4 μm or less. By making the thickness of the shell of the hollow particles above the above lower limit, the strength of the shell is improved. On the other hand, since the shell of the hollow particles of the present invention has a dense structure that is not easily penetrated by acetone, even if the thickness of the shell is as thin as below the above lower limit, the strength of the hollow particles is excellent and not easily broken.

[0089] In addition, the inner diameter r of the hollow particles is calculated by the following formula (1) using the volume average particle diameter R and the porosity of the hollow particles, and the shell thickness of the hollow particles is calculated by the following formula (2) using the inner diameter r and the volume average particle diameter R. In addition, the porosity in the following formula (1) is a numerical value expressed as a ratio.

[0090] 4 / 3π×(R / 2) 3 × porosity = 4 / 3π×(r / 2)3 Formula (1)

[0091] Shell thickness = (Rr) / 2 Formula (2)

[0092] The difference between the calculated shell thickness and the average value of the shell thickness actually measured at 20 locations is usually within ±10% of these average values, and therefore the calculated shell thickness can be regarded as the shell thickness of the hollow particle.

[0093] The thickness of the shell at each location of the hollow particle used to determine the average value of the thickness of the shell at 20 locations can be measured by, for example, observing fragments of the shell obtained by cutting the hollow particle with a SEM.

[0094] An example of an image of the shape of hollow particles is a bag formed of a thin film and inflated with gas, and its cross-sectional view is as described below. Figure 1 The hollow particle 100 in FIG. 1 is shown in FIG. 1 . In this example, a thin membrane is provided on the outside, and the inside is filled with gas.

[0095] The shape of the hollow particles can be confirmed by, for example, SEM, TEM, etc. Furthermore, the shape of the inside of the hollow particles can be confirmed by, for example, SEM, TEM, etc. after the particles are cut into discs by a known method.

[0096] <Shell composition>

[0097] The hollow particles contained in the resin composition of the present invention have a shell composed of a resin, and the resin contains a polymer containing 30 to 100 parts by mass of a crosslinkable monomer unit in 100 parts by mass of all monomer units.

[0098] The polymerizable monomers as the raw materials of the above-mentioned polymers at least include crosslinking monomers, and further may include non-crosslinking monomers. Here, the polymerizable monomers refer to compounds having functional groups capable of addition polymerization (sometimes referred to as polymerizable functional groups in the present invention). In the present invention, as polymerizable monomers, compounds having ethylenically unsaturated bonds as functional groups capable of addition polymerization are generally used. As functional groups capable of addition polymerization, it may be the ethylenically unsaturated bond itself, or it may be a group containing an ethylenically unsaturated bond, specifically, vinyl, (meth) acrylic group, ethylene and allyl groups, etc. may be cited.

[0099] In the present invention, a non-crosslinkable monomer refers to a polymerizable monomer having only one polymerizable functional group, and a crosslinkable monomer refers to a polymerizable monomer having two or more polymerizable functional groups and forming a crosslinked bond in a resin by a polymerization reaction.

[0100] (Crosslinking monomer unit)

[0101] As a cross-linking monomer derived from a cross-linking monomer unit, there is no particular restriction as long as it has two or more polymerizable functional groups. As a cross-linking monomer, for example, divinylbenzene, divinylbiphenyl, divinylnaphthalene, diallyl phthalate, allyl (meth)acrylate, vinyl (meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, 2-hydroxy-3-(meth)acrylate propyl (meth)acrylate and other difunctional cross-linking monomers having two polymerizable functional groups; trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate and other trifunctional or more cross-linking monomers having three or more polymerizable functional groups. These cross-linking monomers can be used alone or in combination of two or more.

[0102] As the crosslinking monomer, it is particularly preferred to use a hydrophilic crosslinking monomer having a solubility of 0.3 g / L or more in distilled water at 20°C. The shell of the hollow particles contains a hydrophilic crosslinking monomer unit, which has an excellent effect of suppressing the reduction in physical properties when the resin composition of the present invention is made into a molded body. Examples of the hydrophilic crosslinking monomer include ethylene glycol dimethacrylate, diethylene glycol diacrylate, allyl methacrylate, vinyl methacrylate, and 2-hydroxy-3-methacrylic acid propyl acrylate.

[0103] In all monomer units of 100 parts by mass of the above-mentioned polymer, the content of the cross-linking monomer unit is 30 to 100 parts by mass, and the lower limit is preferably 35 parts by mass or more, more preferably 40 parts by mass or more, and further preferably 45 parts by mass or more. The upper limit of the content of the cross-linking monomer unit can be less than 100 parts by mass, or less than 90 parts by mass, or less than 80 parts by mass. By making the content of the cross-linking monomer unit above the above lower limit, the mechanical properties of the shell can be improved, the strength of the hollow particles can be improved, and the crushing and porosity reduction of the hollow particles during the molding process of the resin composition can be suppressed. In the case where the content of the cross-linking monomer unit is less than 100 parts by mass, the above-mentioned polymer combination includes a cross-linking monomer unit and a non-cross-linking monomer unit. The cross-linking monomer can link the non-cross-linking monomers to each other by having a plurality of polymerizable functional groups. Therefore, in the case where the combination includes a cross-linking monomer unit and a non-cross-linking monomer unit, the strength and heat resistance of the shell can sometimes be improved.

[0104] The content of each polymerizable monomer unit can be determined by calculating the ratio of each polymerizable monomer fed to the polymerization reaction from the amount of each polymerizable monomer fed during the polymerization and the amount of each polymerizable monomer remaining at the end of the polymerization.

[0105] (Non-crosslinking monomer)

[0106] As the non-crosslinking monomer, for example, a monovinyl monomer can be preferably used. In the present invention, a monovinyl monomer is a compound having a carbon-carbon double bond that can be polymerized. As the monovinyl monomer, for example: (meth)acrylate esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, glycidyl (meth)acrylate, and (meth)acrylate-2-hydroxyethyl (meth)acrylate and (meth)acrylic acid and other (meth)acrylic acid monovinyl monomers; aromatic vinyl monomers such as styrene, vinyltoluene and α-methylstyrene; monoolefin monomers such as ethylene, propylene and butene, etc. These non-crosslinking monomers can be used alone or in combination of two or more.

[0107] Among them, from the viewpoint of reactivity and heat resistance, a (meth)acrylic monovinyl monomer is preferred, and at least one selected from butyl acrylate and methyl methacrylate is more preferred.

[0108] As the non-crosslinking monomer, it is particularly preferred to use a hydrophilic non-crosslinking monomer having a solubility of 0.3 g / L or more in distilled water at 20° C. When the shell of the hollow particle contains a hydrophilic non-crosslinking monomer unit, the strength of the hollow particle is improved.

[0109] As the hydrophilic non-crosslinking monomer, among the above-mentioned monovinyl monomers, for example, alkyl (meth)acrylates having an alkyl group with 1 to 5 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate; non-crosslinking monomers containing polar groups, such as (meth)acrylic acid, glycidyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate. As the hydrophilic non-crosslinking monomer, further examples include (meth)acrylamides and their derivatives, such as (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; and (meth)acrylonitrile.

[0110] As non-crosslinking monomers containing polar groups, non-crosslinking monomers containing polar groups selected from carboxyl, hydroxyl, sulfonic acid, amino, polyoxyethylene and epoxy groups can be cited. As non-crosslinking monomers containing carboxyl, in addition to the above-mentioned (meth) acrylic acid, olefinic unsaturated carboxylic acid monomers such as crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, butene tricarboxylic acid can also be cited. As non-crosslinking monomers containing hydroxyl groups, in addition to the above-mentioned (meth) acrylic acid-2-hydroxyethyl ester, for example, (meth) acrylic acid-2-hydroxypropyl ester, (meth) acrylic acid-4-hydroxybutyl ester, etc. can also be cited. As non-crosslinking monomers containing sulfonic acid groups, for example, styrene sulfonic acid, etc. can be cited. As non-crosslinking monomers containing amino groups, for example, dimethylaminoethyl (meth) acrylic acid, diethylaminoethyl (meth) acrylic acid, etc. can be cited. As non-crosslinking monomers containing polyoxyethylene, for example, the above-mentioned (meth) acrylic acid methoxy polyethylene glycol ester, etc. can be cited. Examples of the non-crosslinkable monomer containing an epoxy group include allyl glycidyl ether, 4-hydroxybutyl acrylate glycidyl ether, and the like in addition to the above-mentioned glycidyl (meth)acrylate.

[0111] As the hydrophilic non-crosslinking monomer, from the viewpoint of a high effect of improving the strength of the hollow particles, at least one selected from (meth)acrylic acid and alkyl (meth)acrylates having an alkyl group having 1 to 5 carbon atoms is particularly preferred, at least one selected from (meth)acrylic acid and alkyl (meth)acrylates having an alkyl group having 1 to 4 carbon atoms is more preferred, and at least one selected from (meth)acrylic acid and methyl (meth)acrylate is further preferred.

[0112] In 100 parts by mass of all monomer units of the above-mentioned polymer, the content of non-crosslinked monomer units is 0 to 70 parts by mass. In addition, all monomer units of the above-mentioned polymer refer to the total of crosslinked monomer units and non-crosslinked monomer units in the above-mentioned polymer. In the case where the above-mentioned polymer contains non-crosslinked monomer units, the lower limit of the content of non-crosslinked monomer units is preferably 3 parts by mass or more, more preferably 10 parts by mass or more, further preferably 15 parts by mass or more, particularly preferably 20 parts by mass or more, and the upper limit is preferably 65 parts by mass or less, more preferably 60 parts by mass or less, further preferably 55 parts by mass or less, and particularly preferably 45 parts by mass or less. By making the above-mentioned polymer contain non-crosslinked monomer units and the content of non-crosslinked monomer units is above the above-mentioned preferred lower limit, the strength and heat resistance of the shell can be improved, and by making the content of non-crosslinked monomer units below the above-mentioned upper limit, it can be made to fully contain crosslinked monomer units, so that the mechanical properties of the shell can be improved and the hollow particles can be suppressed from breaking.

[0113] The content of the polymer contained in the shell of the hollow particles is not particularly limited, but is usually 80% by mass or more, preferably 90% by mass or more, from the viewpoint of excellent strength of the hollow particles.

[0114] In addition, the shell of the hollow particle may contain a small amount of resin different from the above polymer. As the resin different from the above polymer, for example, a polymer having a non-crosslinking monomer unit content greater than 70% by mass, a polyurethane resin, a polyurethane acrylic resin, an epoxy resin, an epoxy acrylic resin, etc. can be cited. In the shell of the hollow particle, the content of the resin different from the above polymer is preferably 20% by mass or less, more preferably 10% by mass or less.

[0115] Furthermore, the shell of the hollow particles may contain additives, etc., in addition to the resin, as necessary. Examples of the additives that may be contained in the shell of the hollow particles include the particle size control agent described below.

[0116] The content of the particle size control agent in the shell of the hollow particles is appropriately adjusted depending on the type thereof and is not particularly limited, but is preferably 0.0001 to 10% by mass, and more preferably 0.001 to 8% by mass.

[0117] <Content of hollow particles>

[0118] In the resin composition of the present invention, the content of the hollow particles is not particularly limited, and is preferably 5 to 50% by mass, more preferably 5 to 30% by mass, and further preferably 5 to 15% by mass. By making the content of the hollow particles above the above lower limit, the lightweight effect of the resin composition brought by the hollow particles can be improved. By making the content of the hollow particles below the above upper limit, the thermoplastic plastomer and the acid-modified polyolefin resin can be fully contained in the resin composition, so that the physical property reduction when the molded body is made can be suppressed, and the mechanical strength can be improved.

[0119] <Method for producing hollow particles>

[0120] Hereinafter, one embodiment of the method for producing hollow particles will be described, but the method for producing hollow particles of the present invention is not necessarily limited to the following embodiment and is not particularly limited.

[0121] One embodiment of the method for producing hollow particles comprises:

[0122] a step of preparing a mixed solution containing a polymerizable monomer, an oil-soluble polymerization initiator, a hydrocarbon solvent, a dispersion stabilizer, and an aqueous medium (mixed solution preparing step);

[0123] A step of preparing a suspension in which droplets of a monomer composition containing a polymerizable monomer and a hydrocarbon solvent are dispersed in an aqueous medium by suspending the mixed liquid (suspension preparation step);

[0124] a step of preparing a precursor composition including precursor particles enclosing a hydrocarbon-based solvent by polymerizing the suspension (polymerization step);

[0125] A step of obtaining precursor particles by solid-liquid separation of the precursor composition (solid-liquid separation step); and

[0126] A step of obtaining hollow particles by removing the hydrocarbon solvent contained in the precursor particles (solvent removal step).

[0127] In the present invention, hollow particles whose hollow parts are filled with a hydrocarbon solvent may be considered as intermediates of hollow particles whose hollow parts are filled with a gas and may be referred to as “precursor particles.” In the present invention, a “precursor composition” refers to a composition containing precursor particles.

[0128] As described above, the present embodiment includes (1) a mixed solution preparation process, (2) a suspension preparation process, (3) a polymerization process, (4) a solid-liquid separation process, and (5) a solvent removal process. The processes of the present embodiment are not limited to these five processes, and may further include processes other than these processes. In addition, as long as it is technically feasible, two or more of the above-mentioned processes and other additional processes may be performed simultaneously as one process, or the order may be changed. For example, the preparation of the mixed solution and the suspension may be performed simultaneously in one process by adding materials for preparing the mixed solution while suspending the mixed solution at the same time.

[0129] Figure 1 This is a schematic diagram showing an example of the production method of the present invention. Figure 1 (1) to (5) in the figure correspond to the above steps (1) to (5). The white arrows between the figures indicate the order of the steps. Figure 1 The schematic diagrams are only for explanation, and the manufacturing method of the present invention is not limited to the manufacturing method shown in the figures. In addition, the structure, size and shape of the materials used in each manufacturing method of the present invention are not limited to the structure, size and shape of the various materials in these figures.

[0130] Figure 1 (1) is a cross-sectional schematic diagram showing an embodiment of a mixed solution in a mixed solution preparation process. As shown in the figure, the mixed solution includes an aqueous medium 1 and a low-polarity material 2 dispersed in the aqueous medium 1. Here, the low-polarity material 2 refers to a material with low polarity that is difficult to mix with the aqueous medium 1. In the present invention, the low-polarity material 2 includes a polymerizable monomer and a hydrocarbon solvent.

[0131] Figure 1(2) is a cross-sectional schematic diagram showing an embodiment of a suspension in a suspension preparation process. The suspension includes an aqueous medium 1 and droplets 10 of a monomer composition dispersed in the aqueous medium 1. Although the droplets 10 of the monomer composition include polymerizable monomers and a hydrocarbon solvent, the distribution in the droplets is not uniform. The droplets 10 of the monomer composition have the following structure: the hydrocarbon solvent 4a and the material 4b other than the hydrocarbon solvent including the polymerizable monomer are phase-separated, the hydrocarbon solvent 4a is biased to exist in the center, the material 4b other than the hydrocarbon solvent is biased to exist on the surface side, and a dispersion stabilizer (not shown) is attached to the surface.

[0132] Figure 1 (3) is a cross-sectional schematic diagram showing an embodiment of a composition (precursor composition) obtained by a polymerization process and comprising precursor particles containing a hydrocarbon-based solvent in a hollow portion. The composition comprises an aqueous medium 1, and precursor particles 20 containing a hydrocarbon-based solvent 4a in a hollow portion dispersed in the aqueous medium 1. The shell 6 forming the outer surface of the precursor particle 20 is formed by polymerization of the polymerizable monomer in the droplets 10 of the above-mentioned monomer composition.

[0133] Figure 1 (4) is a schematic cross-sectional view showing an embodiment of precursor particles containing a hydrocarbon solvent in the hollow portion after the solid-liquid separation step. Figure 1 (4) shows that from the above Figure 1 The state (3) is the state after removing the aqueous medium 1.

[0134] Figure 1 (5) is a schematic cross-sectional view showing one embodiment of the hollow particles after the solvent removal step. Figure 1 (5) shows that from the above Figure 1 The state (4) is a state after the hydrocarbon solvent 4a is removed. By removing the hydrocarbon solvent from the precursor particle containing the hydrocarbon solvent in the hollow part, the hollow particle 100 having the hollow part 8 filled with gas inside the shell 6 can be obtained.

[0135] Hereinafter, the above five steps and other steps will be described in sequence.

[0136] (1) Mixed solution preparation process

[0137] This step is a step of preparing a mixed solution containing a polymerizable monomer, an oil-soluble polymerization initiator, a hydrocarbon solvent, a dispersion stabilizer, and an aqueous medium. From the viewpoint of appropriately adjusting the particle size of the droplets of the monomer composition and the thickness of the shell of the obtained hollow particles, the mixed solution preferably further contains a particle size control agent.

[0138] The polymerizable monomer is as described in the above-mentioned <Shell Composition> of the Hollow Particles. In addition to the polymerizable monomer described in the above-mentioned <Shell Composition> of the Hollow Particles, the mixed liquid may contain other polymerizable compounds.

[0139] (Particle size control agent)

[0140] The mixed liquid preferably contains a particle size control agent for appropriately adjusting the particle size of the droplets of the monomer composition. This allows the particle size and shell thickness of the obtained hollow particles to be appropriately adjusted, and hollow particles that are not easily broken even with high porosity can be obtained.

[0141] As a particle size control agent, for example, at least one selected from rosin acid, higher fatty acids and their metal salts, or a polar resin described later can be used. These particle size control agents can appropriately adjust the particle size of the droplets of the monomer composition containing polymerizable monomers and hydrocarbon solvents in the suspension preparation process described later. In the suspension preparation process, droplets of the monomer composition are formed in the aqueous medium by the action of a dispersion stabilizer. In the droplets of the monomer composition, materials other than the hydrocarbon solvent containing polymerizable monomers are phase-separated from the hydrocarbon solvent, the hydrocarbon solvent tends to exist in the center, and the materials other than the hydrocarbon solvent tend to exist on the surface side. In the case where the mixed liquid contains a particle size control agent, it is inferred that it has the following structure: the particle size control agent tends to exist near the surface of the droplets of the monomer composition, and the dispersion stabilizer is attached to the surface of the droplets. Such a distribution structure of materials is formed according to the different affinity of each material to the aqueous medium. It can be considered that, because the mixed liquid contains a particle size control agent, the droplets of the monomer composition in the suspension present a distribution structure of the material as described above, and an interaction between the dispersion stabilizer and the particle size control agent occurs on the surface of the droplets. Therefore, the dispersion stabilizer causes the dispersibility of the droplets to change, and the particle size of the droplets of the monomer composition can be appropriately adjusted.

[0142] The particle size control agent is preferably at least one selected from abietic acid, higher fatty acids, and metal salts thereof, and more preferably at least one selected from abietic acid and alkali metal salts thereof, from the viewpoint of being able to appropriately adjust the particle size of the droplets with a small content.

[0143] The rosin acid preferably used as the particle size control agent can be obtained from rosins such as rosin, tall oil rosin and wood rosin.

[0144] Components contained in abietic acid obtained from these rosins include, for example, abietic acid, dehydroabietic acid, palustric acid, isopimaric acid, pimaric acid, etc. The component ratio of abietic acid is not fixed and varies depending on the type of rosin, the pine species of the raw material, the production area, and the like.

[0145] As the rosin acid and its metal salt used in the present invention, rosin acid and its alkali metal salt containing 50% by mass of abietic acid such as abietic acid, dehydroabietic acid, palustric acid, and hydrogenated products thereof are preferred.

[0146] The higher fatty acid used as the particle size control agent is preferably a higher fatty acid having 10 to 25 carbon atoms excluding the carbon atom in the carboxyl group. Examples of preferred higher fatty acids include lauric acid (CH3(CH2) 10 COOH), tridecanoic acid (CH3(CH2) 11 COOH), myristic acid (CH3(CH2) 12 COOH), pentadecanoic acid (CH3(CH2) 13 COOH), palmitic acid (CH3(CH2) 14 COOH), heptadecanoic acid (CH3(CH2) 15 COOH), stearic acid (CH3(CH2) 16 COOH), arachidic acid (CH3(CH2) 18 COOH), behenic acid (CH3(CH2) 20 COOH) and tetracosanoic acid (CH3(CH2) 22 COOH) etc.

[0147] Examples of the metal used in the metal salt of rosin acid or higher fatty acid include alkali metals such as Li, Na, and K, and alkaline earth metals such as Mg and Ca. Alkali metals are particularly preferred, and at least one selected from Li, Na, and K is more preferred.

[0148] When at least one selected from rosin acid, higher fatty acids and metal salts thereof is used as a particle size control agent, the total content of rosin acid, higher fatty acids and metal salts thereof is preferably 0.0001 mass parts or more and 0.1 mass parts or less relative to 100 mass parts of polymerizable monomers, more preferably 0.001 mass parts or more and 0.01 mass parts or less, and further preferably 0.0015 mass parts or more and 0.006 mass parts or less. By making the above content above the above lower limit, it is easy to control the particle size and shell thickness of the hollow particles, and the strength of the hollow particles can be improved. On the other hand, by making the above content below the above upper limit, the content ratio of the polymerizable monomer can be suppressed from decreasing, and therefore, the strength of the shell can be suppressed from decreasing, and the crushing of the hollow particles can be further suppressed.

[0149] The polar resin preferably used as the particle size control agent is a polymer containing a repeating unit containing a heteroatom, and specifically, acrylic resins, polyester resins, vinyl resins containing a heteroatom, and the like are mentioned.

[0150] The polar resin may be a homopolymer or copolymer of a monomer containing a heteroatom, or a copolymer of a monomer containing a heteroatom and a monomer not containing a heteroatom. When the polar resin is a copolymer of a monomer containing a heteroatom and a monomer not containing a heteroatom, from the viewpoint of easily controlling the particle size of the hollow particles, the proportion of the monomer unit containing a heteroatom in 100% by mass of all repeating units constituting the copolymer is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more.

[0151] Examples of heteroatom-containing monomers used in the polar resin include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, acrylic acid, methacrylic acid, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and propylene glycol. The monomers having a (meth)acryloyl group include (meth)acrylic acid glycidyl ester, 4-hydroxybutyl acrylate glycidyl ether, (meth)acrylic acid monovinyl monomers; aromatic vinyl monomers containing heteroatoms such as halogenated styrene and styrene sulfonic acid; carboxylic acid vinyl ester monomers such as vinyl acetate; halogenated vinyl monomers such as vinyl chloride; vinylidene halide monomers such as vinylidene chloride; vinyl pyridine monomers; carboxyl group-containing monomers such as ethylenically unsaturated carboxylic acid monomers such as crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, butenetricarboxylic acid; epoxy group-containing monomers such as allyl glycidyl ether, etc. These heteroatom-containing monomers can be used alone or in combination of two or more.

[0152] Examples of heteroatom-free monomers used in polar resins include aromatic vinyl monomers that do not contain heteroatoms, such as styrene, vinyltoluene, α-methylstyrene, and p-methylstyrene; monoolefin monomers such as ethylene, propylene, and butene; and diene monomers such as butadiene and isoprene. These heteroatom-free monomers can be used alone or in combination of two or more.

[0153] Among the above-mentioned polar resins, from the viewpoint of high compatibility with the above-mentioned polymerizable monomer and easy control of the particle size of the hollow particles, it is preferred that the total mass of (meth)acrylic acid monovinyl monomer units in 100% by mass of all repeating units constituting the resin is preferably 50% by mass or more, more preferably 70% by mass or more, and further preferably 90% by mass or more of acrylic resins, and it is particularly preferred that all repeating units constituting the resin are formed of (meth)acrylic acid monovinyl monomer units.

[0154] From the viewpoint of easily controlling the particle size of the hollow particles, the polar resin preferably contains a polar group-containing monomer unit containing a polar group selected from a carboxyl group, a hydroxyl group, a sulfonic acid group, an amino group, a polyoxyethylene group and an epoxy group. As the polar group-containing monomer used in the polar resin, for example, the same polar group-containing monomer as the non-crosslinking monomer containing the polar group that the above-mentioned polymerizable monomer can contain can be cited. The polar group-containing monomer can be used alone or in combination of two or more. As the polar group contained in the polar group-containing monomer unit contained in the polar resin, carboxyl and hydroxyl groups are preferred from the viewpoint of being able to control the particle size with a small amount of addition.

[0155] When the polar resin contains a polar group-containing monomer unit, it is preferred that the polar group is located at the end of the main chain or side chain, or is bonded to the main chain or side chain in a pendant state, from the viewpoint of easily configuring the polar resin on the outer surface of the hollow particles and easily controlling the particle size of the hollow particles.

[0156] In the case where the polar resin does not contain the above-mentioned polar group-containing monomer unit, from the viewpoint of high compatibility with the above-mentioned polymerizable monomer and easy control of the particle size of the hollow particles, the above-mentioned heteroatom-containing monomer unit contained in the polar resin preferably contains a monomer unit derived from an alkyl (meth)acrylate, wherein, from the viewpoint of high polarity, it is preferred to contain a monomer unit derived from an alkyl (meth)acrylate in which the number of carbon atoms of the alkyl group is preferably 3 or less, the alkyl group is more preferably methyl or ethyl, and the alkyl group is further preferably methyl.

[0157] From the viewpoint of high compatibility with the polymerizable monomer and easy control of the particle size of the hollow particles, the acrylic resin used as the polar resin is preferably a polymer or copolymer of a polymerizable monomer for a polar resin containing 50% by mass or more of methyl methacrylate when the total mass of the polymerizable monomer for a polar resin is taken as 100% by mass. In addition, in the present invention, the polymerizable monomer used in the synthesis of the polar resin is referred to as a polymerizable monomer for a polar resin.

[0158] The polar resin can be obtained, for example, by using a polymerizable monomer for a polar resin containing the heteroatom-containing monomer and polymerizing it by a polymerization method such as solution polymerization and emulsion polymerization.

[0159] Furthermore, when the polar resin is a copolymer, the copolymer may be any of a random copolymer, a block copolymer, and a graft copolymer, and is preferably a random copolymer.

[0160] Furthermore, from the viewpoint of improving solubility, it is preferred that the polar resin be pulverized more finely.

[0161] The number average molecular weight (Mn) of the polar resin is not particularly limited, and is preferably in the range of 3000 to 20000, more preferably in the range of 4000 to 17000, and further preferably in the range of 6000 to 15000, as measured by a polystyrene conversion value measured by gel permeation chromatography (GPC) using tetrahydrofuran. By making the number average molecular weight (Mn) of the polar resin above the lower limit value or more, the solubility of the polar resin is improved, and the particle size of the hollow particles is easily controlled. By making the number average molecular weight (Mn) of the polar resin above the upper limit value or less, the strength reduction of the shell can be suppressed.

[0162] When using polar resin as particle size control agent, relative to 100 parts by mass of polymerizable monomer, the content of polar resin is preferably 0.1 parts by mass and 10 parts by mass or less, more preferably 0.3 parts by mass and 8.0 parts by mass or less, further preferably 0.5 parts by mass and 8.0 parts by mass or less. By making the above content above the above lower limit, it is easy to control the particle diameter of hollow particles and the thickness of the shell, and the strength of hollow particles can be improved. On the other hand, by making the above content below the above upper limit, the ratio of the content of polymerizable monomer can be suppressed to reduce, therefore, the strength of the shell can be suppressed to reduce, and the crushing of hollow particles can be further suppressed.

[0163] (Oil-soluble polymerization initiator)

[0164] In the present embodiment, a suspension polymerization method using an oil-soluble polymerization initiator is adopted instead of an emulsion polymerization method using a water-soluble polymerization initiator.

[0165] The oil-soluble polymerization initiator is not particularly limited as long as it is a lipophilic polymerization initiator having a solubility in water of 0.2 mass % or less. Examples of the oil-soluble polymerization initiator include benzoyl peroxide, lauroyl peroxide, tert-butyl peroxy-2-ethylhexanoate, 2,2'-azobis(2,4-dimethylvaleronitrile), and azobisisobutyronitrile.

[0166] When the total mass of the polymerizable monomer is set to 100 parts by mass, the content of the oil-soluble polymerization initiator is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and further preferably 1 to 5 parts by mass. When the above content of the oil-soluble polymerization initiator is 0.1 parts by mass or more, the polymerization reaction is easy to proceed sufficiently. On the other hand, when the above content of the oil-soluble polymerization initiator is 10 parts by mass or less, after the polymerization reaction is completed, the risk of the oil-soluble polymerization initiator remaining is small, and as a result, the risk of carrying out an unexpected side reaction is also small.

[0167] (Hydrocarbon solvents)

[0168] The hydrocarbon solvent in this embodiment has a function of forming a hollow space inside the particles.

[0169] In the suspension preparation step described below, a suspension in which monomer droplets containing a hydrocarbon solvent are dispersed in an aqueous medium can be obtained. In the suspension preparation step, phase separation occurs in the monomer droplets, and as a result, the hydrocarbon solvent with low polarity tends to gather inside the monomer droplets. Finally, in the monomer droplets, the hydrocarbon solvent is distributed inside according to their respective polarities, and other materials other than the hydrocarbon solvent are distributed around them.

[0170] In the polymerization step described below, a precursor composition including precursor particles containing a hydrocarbon solvent can be obtained. That is, the hydrocarbon solvent is concentrated inside the particles, and hollows formed by the hydrocarbon solvent are formed inside the obtained polymer particles (precursor particles).

[0171] The type of hydrocarbon solvent is not particularly limited. Examples of the hydrocarbon solvent include highly volatile solvents such as benzene, toluene, xylene, butane, pentane, hexane, heptane, and cyclohexane.

[0172] The hydrocarbon solvent used in the present embodiment preferably has a relative dielectric constant of 3 or less at 20° C. The relative dielectric constant is one of the indicators indicating the polarity of a compound. When the relative dielectric constant of the hydrocarbon solvent is sufficiently small to be 3 or less, it is considered that phase separation rapidly proceeds in the monomer droplets and hollows are easily formed.

[0173] Examples of solvents having a relative dielectric constant of 3 or less at 20° C. are as follows. The values ​​in parentheses are relative dielectric constants.

[0174] Heptane (1.9), cyclohexane (2.0), benzene (2.3), toluene (2.4).

[0175] Regarding the relative dielectric constant at 20° C., reference can be made to the values ​​and other technical information recorded in known literature (e.g., Chemical Society of Japan, "Basic Handbook of Chemistry", revised 4th edition, Maruzen Co., Ltd., published on September 30, 1996, pages II-498 to II-503). As a method for measuring the relative dielectric constant at 20° C., for example, a relative dielectric constant test performed according to 23 of JISC 2101:1999 and measuring at a temperature of 20° C. can be cited.

[0176] The hydrocarbon solvent used in this embodiment may be a hydrocarbon compound having 5 to 7 carbon atoms. The hydrocarbon compound having 5 to 7 carbon atoms can be easily encapsulated in the precursor particles during the polymerization step and can be easily removed from the precursor particles during the solvent removal step. Among them, the hydrocarbon solvent is preferably a hydrocarbon compound having 6 carbon atoms.

[0177] When the total mass of the polymerizable monomer is set to 100 parts by mass, the content of the hydrocarbon solvent is preferably 70 to 900 parts by mass, more preferably 150 to 700 parts by mass, and further preferably 200 to 500 parts by mass. When the above content of the hydrocarbon solvent is 70 parts by mass or more, the porosity of the obtained hollow particles becomes larger. On the other hand, when the above content of the hydrocarbon solvent is 900 parts by mass or less, the mechanical properties of the obtained hollow particles are mostly excellent, and the risk of not being able to maintain the hollow is small.

[0178] (Dispersion Stabilizer)

[0179] The dispersion stabilizer is an agent that disperses the droplets of the monomer composition in the aqueous medium in the suspension preparation process. In the present invention, from the viewpoint of easily controlling the particle size of the droplets in the suspension, narrowing the particle size distribution of the obtained hollow particles, and preventing the shell from becoming too thin and preventing the strength of the hollow particles from decreasing, it is preferred to use an inorganic dispersion stabilizer as the dispersion stabilizer. In particular, when an inorganic dispersion stabilizer is used in combination with the above-mentioned particle size control agent, the effect brought about by the inorganic dispersion stabilizer is easily exerted.

[0180] Examples of the inorganic dispersion stabilizer include sulfates such as barium sulfate and calcium sulfate; carbonates such as barium carbonate, calcium carbonate, and magnesium carbonate; phosphates such as calcium phosphate; metal oxides such as aluminum oxide and titanium oxide; inorganic compounds such as metal hydroxides such as aluminum hydroxide, magnesium hydroxide, calcium hydroxide, barium hydroxide, and iron hydroxide. These inorganic dispersion stabilizers can be used alone or in combination of two or more.

[0181] Among the above-mentioned inorganic dispersion stabilizers, the above-mentioned poorly water-soluble inorganic metal salts such as sulfates, carbonates, phosphates and metal hydroxides are preferred, metal hydroxides are more preferred, and magnesium hydroxide is particularly preferred.

[0182] In the present invention, the poorly water-soluble inorganic metal salt is preferably an inorganic metal salt having a solubility of 0.5 g or less in 100 g of water.

[0183] The content of the dispersion stabilizer is not particularly limited, and is preferably 0.5 to 10 parts by mass, more preferably 1.0 to 8.0 parts by mass, relative to 100 parts by mass of the total mass of the polymerizable monomer and the hydrocarbon solvent. By making the content of the dispersion stabilizer above the lower limit, the droplets of the monomer composition can be fully dispersed in the suspension without merging. On the other hand, by making the content of the dispersion stabilizer below the upper limit, the viscosity of the suspension can be prevented from increasing during granulation, avoiding the undesirable situation that the suspension cannot pass through the granulator.

[0184] The content of the dispersion stabilizer is usually 2 parts by mass or more and 15 parts by mass or less, and more preferably 3 parts by mass or more and 8 parts by mass or less, based on 100 parts by mass of the aqueous medium.

[0185] (Water-based media)

[0186] In the present embodiment, the aqueous medium refers to any one of water, a hydrophilic solvent, or a mixture of water and a hydrophilic solvent.

[0187] The hydrophilic solvent in this embodiment is not particularly limited as long as it is fully miscible with water and does not phase separate. Examples of the hydrophilic solvent include alcohols such as methanol and ethanol, tetrahydrofuran (THF), and dimethyl sulfoxide (DMSO).

[0188] Among aqueous media, water is preferably used from the viewpoint of its high polarity. When a mixture of water and a hydrophilic solvent is used, it is extremely important that the polarity of the mixture as a whole does not become too low from the viewpoint of forming monomer droplets. For example, the mixing ratio (mass ratio) of water and the hydrophilic solvent may be water: hydrophilic solvent = 99:1 to 50:50.

[0189] The mixed solution prepared in this step is a composition in a state where the above-mentioned polymerizable monomer, oil-soluble polymerization initiator, hydrocarbon-based solvent, dispersion stabilizer and aqueous medium are simply mixed and appropriately stirred. In this mixed solution, the oil phase containing the above-mentioned polymerizable monomer, oil-soluble polymerization initiator and hydrocarbon-based solvent is dispersed in the aqueous medium in a particle size of about several mm. The dispersion state of these materials in the mixed solution can be observed with the naked eye depending on the type of material.

[0190] In this step, the mixed solution can be prepared by mixing an oil phase containing a polymerizable monomer, an oil-soluble polymerization initiator and a hydrocarbon solvent with an aqueous phase containing a dispersion stabilizer and an aqueous medium. By mixing the oil phase and the aqueous phase in this way, particles with a uniform composition can be formed.

[0191] (2) Suspension preparation process

[0192] This step is a step of preparing a suspension in which droplets of a monomer composition containing a polymerizable monomer and a hydrocarbon solvent are dispersed in an aqueous medium by suspending the above-mentioned mixed liquid.

[0193] In the suspension prepared in this step, droplets of a monomer composition containing the above-mentioned polymerizable monomer, oil-soluble polymerization initiator and hydrocarbon solvent and having a volume average particle size of about 1 to 60 μm are uniformly dispersed in the aqueous medium. Such droplets of the monomer composition are difficult to observe with the naked eye, but can be observed by a known observation device such as an optical microscope.

[0194] Figure 2 The figure is a schematic diagram showing one embodiment of the suspension in the suspension preparation process. Figure 2 The cross section of the droplet 10 of the monomer composition is schematically shown. Figure 2 It is only a schematic diagram, and the suspension in the present invention is not necessarily limited to Figure 2 Suspension shown. Figure 2 A part of Figure 1 (2).

[0195] Figure 2 2 shows a state where droplets 10 of a monomer composition and polymerizable monomer 4c dispersed in an aqueous medium 1 are dispersed in an aqueous medium 1. The droplets 10 are formed by surrounding an oil-soluble monomer composition 4 with a dispersion stabilizer 3.

[0196] The monomer composition contains an oil-soluble polymerization initiator 5, a polymerizable monomer, and a hydrocarbon solvent (neither of which are shown in the figure).

[0197] The droplets 10 are fine oil droplets containing the monomer composition 4, and the oil-soluble polymerization initiator 5 generates polymerization initiation radicals inside the fine oil droplets. Therefore, precursor particles having a target particle size can be produced without excessively growing the fine oil droplets.

[0198] In the suspension polymerization method using such an oil-soluble polymerization initiator, there is no chance for the polymerization initiator to come into contact with the polymerizable monomer 4c dispersed in the aqueous medium 1. Therefore, by using an oil-soluble polymerization initiator, in addition to the target resin particles having a hollow portion, the generation of unnecessary polymer particles such as dense particles having a small particle size can be suppressed.

[0199] In the suspension preparation step, the method for forming droplets of the monomer composition is not particularly limited, and examples thereof include methods using an apparatus capable of strong stirring, such as an (in-line) emulsifying disperser (manufactured by Ohira Kiko Co., Ltd., trade name: Milder) or a high-speed emulsifying disperser (manufactured by Primix Co., Ltd., trade name: TKHOMOMIXER MARK II).

[0200] As described above, in this step, since phase separation occurs in the droplets of the monomer composition, the hydrocarbon solvent with low polarity tends to concentrate inside the droplets. As a result, the hydrocarbon solvent is distributed inside the obtained droplets, and materials other than the hydrocarbon solvent are distributed around the obtained droplets.

[0201] Alternatively, in the suspension preparation process, the suspension can also be prepared by a membrane emulsification method. In the case of preparing a suspension by a membrane emulsification method, for example, in the mixed solution preparation process, an oil phase containing a polymerizable monomer, an oil-soluble polymerization initiator and a hydrocarbon solvent, and an aqueous phase containing a dispersion stabilizer and an aqueous medium are prepared separately, and the suspension is prepared by a membrane emulsification method. The membrane emulsification method refers to a method in which a dispersed phase liquid is extruded into a continuous phase through the pores of a porous membrane, thereby obtaining a suspension in which tiny droplets of the dispersed phase are dispersed in a continuous phase. Here, the dispersed phase refers to a liquid phase dispersed in the form of tiny droplets, and the continuous phase refers to a liquid phase surrounded by the dispersed phase droplets. In the present embodiment, as long as the membrane emulsification method using the above-mentioned oil phase as the dispersed phase and the above-mentioned aqueous phase as the continuous phase, any one of the direct membrane emulsification method and the membrane emulsification method accompanied by pre-emulsification can be used.

[0202] In the membrane emulsification method, a membrane emulsification system (e.g., model: MN-20, manufactured by SPG Technology Co., Ltd.) and a membrane having a specific pore size are used. Examples of porous membranes that can be used in the membrane emulsification method include inorganic porous membranes such as Shirasu porous glass membrane (SPG membrane), and organic porous membranes such as PTFE membrane.

[0203] The pore size of the porous membrane in the membrane emulsification method determines the particle size of the obtained microdroplets. Although it depends on the components in the dispersed phase, the particle size of the microdroplets will affect the number average particle size of the obtained hollow particles. Therefore, the selection of the pore size of the porous membrane is important. For example, when using a Shirasu porous glass membrane (SPG membrane), it is preferred to select a pore size of 0.1 to 5.0 μm as the membrane.

[0204] In the suspension preparation step using the membrane emulsification method, the suspension is prepared by membrane emulsification using the membrane emulsification system and the porous membrane with the oil phase as a dispersed phase and the water phase as a continuous phase.

[0205] In addition, the suspension preparation step in the present embodiment is not limited to the above-mentioned method.

[0206] (3) Polymerization process

[0207] This step is a step of preparing a precursor composition in which precursor particles containing a hydrocarbon solvent are dispersed in an aqueous medium by polymerizing the above-mentioned suspension. The precursor particles are formed by polymerization of polymerizable monomers contained in droplets of the monomer composition.

[0208] The polymerization method is not particularly limited, and examples thereof include intermittent (batch), semi-continuous, and continuous methods. The polymerization temperature is preferably 40 to 80° C., more preferably 50 to 70° C. The polymerization reaction time is preferably 1 to 20 hours, more preferably 2 to 15 hours.

[0209] In the polymerization step, since the shell parts of the droplets of the monomer composition containing the hydrocarbon solvent inside are polymerized, as described above, a hollow space formed by the hydrocarbon solvent is formed inside the obtained precursor particles.

[0210] (4) Solid-liquid separation process

[0211] This step is a step of obtaining precursor particles by solid-liquid separation of the above-mentioned precursor composition.

[0212] The method for solid-liquid separation of the precursor composition is not particularly limited as long as it is a method for separating the solid component comprising the precursor particles from the liquid component comprising the aqueous medium, and known methods can be used. As the method for solid-liquid separation, for example, centrifugation, filtration and static separation can be enumerated, wherein, centrifugation or filtration can be used, and from the viewpoint of the simplicity of operation, centrifugation can also be used.

[0213] After the solid-liquid separation step and before the solvent removal step described below, an arbitrary step such as a pre-drying step may be performed. As the pre-drying step, for example, a step of pre-drying the solid component obtained after the solid-liquid separation step by a drying device such as a dryer or a dryer such as a hand dryer may be mentioned.

[0214] (5) Solvent Removal Process

[0215] This step is a step of obtaining hollow particles by removing the hydrocarbon solvent contained in the precursor particles.

[0216] The hydrocarbon solvent contained in the precursor particles may be removed in the form of gas or liquid.

[0217] In this process, "in gas" strictly refers to an environment in which there is no liquid component outside the precursor particles, and an environment in which there is only a very small amount of liquid component outside the precursor particles to the extent that it does not affect the removal of the hydrocarbon-based solvent. "In gas" can be expressed as a state in which the precursor particles are not present in the slurry, and can also be expressed as a state in which the precursor particles are present in the dry powder.

[0218] The method for removing the hydrocarbon solvent in the precursor particles is not particularly limited, and a known method can be used. In addition, as a method for removing the hydrocarbon solvent in the precursor particles in a gas, for example, a reduced pressure drying method, a heating drying method, a gas flow drying method, or a combination of these methods can be cited.

[0219] In particular, when a heating drying method is used, the heating temperature needs to be above the boiling point of the hydrocarbon solvent and below the highest temperature at which the shell structure of the hollow particles is not broken. Therefore, depending on the composition of the shell in the precursor particles and the type of the hydrocarbon solvent, the heating temperature can be, for example, 50 to 250° C., 100 to 240° C., or 150 to 220° C. In addition, the heating time can be 1 to 24 hours, preferably 2 to 15 hours, and more preferably 3 to 10 hours.

[0220] By the drying operation in the gas, the hydrocarbon solvent inside the precursor particles is replaced by the external gas, and as a result, hollow particles whose hollow parts are filled with the gas can be obtained.

[0221] The drying environment is not particularly limited, and examples thereof include air, oxygen, nitrogen, argon, and vacuum environments. Alternatively, hollow particles whose interiors are temporarily vacuumed may be obtained by once filling the interior of the hollow particles with a gas and then drying under reduced pressure.

[0222] As another method, instead of performing solid-liquid separation on the slurry-like precursor composition obtained in the polymerization step, the hydrocarbon solvent contained in the precursor particles may be replaced with the aqueous medium of the slurry in the slurry containing the precursor particles and the aqueous medium to remove the hydrocarbon solvent.

[0223] In this method, the hydrocarbon solvent included in the precursor particles can be removed by bubbling an inert gas in the precursor composition at a temperature equal to or higher than the boiling point of the hydrocarbon solvent minus 35° C.

[0224] Here, the above-mentioned hydrocarbon solvent is a mixed solvent containing multiple hydrocarbon solvents. When it has multiple boiling points, the boiling point of the hydrocarbon solvent in the solvent removal process is the boiling point of the solvent with the highest boiling point among the solvents contained in the mixed solvent, that is, the highest boiling point among the multiple boiling points.

[0225] From the viewpoint of reducing the residual amount of the hydrocarbon solvent in the hollow particles, the temperature at which the inert gas is bubbled in the precursor composition is preferably a temperature higher than the temperature at which 30°C is subtracted from the boiling point of the hydrocarbon solvent, and more preferably a temperature higher than the temperature at which 20°C is subtracted from the boiling point of the hydrocarbon solvent. In addition, the temperature at the time of bubbling is usually a temperature higher than the polymerization temperature in the above-mentioned polymerization step. Although not particularly limited, the temperature at the time of bubbling can be 50°C or higher and 100°C or lower.

[0226] The inert gas for bubbling is not particularly limited, and examples thereof include nitrogen and argon.

[0227] The bubbling conditions can be appropriately adjusted according to the type and amount of the hydrocarbon solvent so as to remove the hydrocarbon solvent contained in the precursor particles. The conditions are not particularly limited and may be, for example, bubbling the inert gas at 1 to 3 L / min for 1 to 10 hours.

[0228] This method can obtain an aqueous slurry in which an aqueous medium is enclosed in precursor particles. The hollow particles obtained by solid-liquid separation of the slurry are dried to remove the aqueous medium in the hollow particles, thereby obtaining hollow particles in which the hollow part is occupied by gas.

[0229] A method is compared in which, after solid-liquid separation of a slurry-like precursor composition, hydrocarbon solvent in the precursor particles is removed in a gas, thereby obtaining hollow particles whose hollow parts are filled with gas; and a method in which, in a slurry comprising precursor particles and an aqueous medium, the hydrocarbon solvent enclosed in the precursor particles is replaced with the aqueous medium of the slurry, solid-liquid separation is performed, and the aqueous medium in the precursor particles is removed in a gas, thereby obtaining hollow particles whose hollow parts are filled with gas. The former method has the advantage that the hollow particles are not easily broken in the step of removing the hydrocarbon solvent, and the latter method has the advantage that the residual hydrocarbon solvent is reduced by bubbling using an inert gas.

[0230] In addition, when the hydrocarbon solvent contained in the precursor particles is replaced with water, if the water of the same volume as the hydrocarbon solvent separated from the particles does not enter the particles, there is a problem that the obtained hollow particles are broken. As a method to prevent this problem, for example, it can be considered to remove the hydrocarbon solvent after making the pH of the slurry 7 or more and swelling the shell of the particles with alkali. In this case, the shell of the particle acquires flexibility, so the replacement of the hydrocarbon solvent and water inside the particle proceeds rapidly.

[0231] (6) Others

[0232] As steps other than the above-mentioned (1) to (5), for example, the following (6-a) cleaning step and the following (6-b) hollow portion re-replacement step may be added.

[0233] (6-a) Cleaning process

[0234] The washing step is a step of washing by adding an acid or an alkali in order to remove the residual dispersion stabilizer in the precursor composition containing the precursor particles before the above-mentioned solvent removal step. When the dispersion stabilizer used is an inorganic dispersion stabilizer soluble in acid, it is preferred to wash by adding an acid to the precursor composition containing the precursor particles. On the other hand, when the dispersion stabilizer used is an inorganic compound soluble in alkali, it is preferred to wash by adding an alkali to the precursor composition containing the precursor particles.

[0235] In addition, when an inorganic dispersion stabilizer soluble in acid is used as a dispersion stabilizer, an acid is added to the precursor composition containing the precursor particles, and the pH is preferably adjusted to 6.5 or less, and more preferably adjusted to 6 or less. As the acid to be added, inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as formic acid and acetic acid can be used, and sulfuric acid is particularly preferred from the viewpoint of high removal efficiency of the dispersion stabilizer and small burden on the manufacturing equipment.

[0236] (6-b) Re-replacement step of hollow portion

[0237] The re-replacement process of the hollow part is a process of replacing the gas or liquid inside the hollow particle with other gas or liquid. By such replacement, the environment inside the hollow particle can be changed, or molecules can be selectively confined inside the hollow particle, or the chemical structure inside the hollow particle can be modified according to the application.

[0238] [Acid-modified polyolefin resin]

[0239] The resin composition of the present invention contains an acid-modified polyolefin resin. The acid-modified polyolefin resin is a resin in which an acidic group is introduced into the polyolefin resin.

[0240] As the polyolefin resin used in the acid-modified polyolefin resin, there can be mentioned the same type of polyolefin resin as the polyolefin resin used as the thermoplastic plastomer, and preferably a polyolefin resin having a weight average molecular weight within the preferred range described below is used. As the polyolefin resin used in the acid-modified polyolefin resin, polyethylene resins, polypropylene resins, and propylene-α-olefin copolymers are preferred, and polypropylene resins are particularly preferred from the viewpoint of good affinity with the above-mentioned preferred thermoplastic plastomer.

[0241] As the acid-modified polyolefin-based resin used in the resin composition of the present invention, it is preferred that a carboxylic acid-modified polyolefin-based resin is one in which a carboxyl group or a carboxylic acid anhydride group is introduced as an acidic group.

[0242] The carboxylic acid-modified polyolefin resin can be obtained by adding at least one selected from α,β-unsaturated carboxylic acid and its anhydride to the system during or after the polymerization of the polyolefin resin. It can be a method in which α,β-unsaturated carboxylic acid and its anhydride are introduced into the main chain of the polyolefin resin by addition reaction to form a chemical bond between the polyolefin resin and the α,β-unsaturated carboxylic acid and its anhydride; it can also be a method in which the α,β-unsaturated carboxylic acid and its anhydride are dispersed in the polyolefin resin instead of forming a chemical bond between the polyolefin resin and the α,β-unsaturated carboxylic acid and its anhydride; or it can also have these methods in combination.

[0243] Examples of the α,β-unsaturated carboxylic acid and its anhydride include (meth)acrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, and anhydrides thereof. Among them, maleic anhydride and maleic acid are preferred, and maleic anhydride is more preferred.

[0244] As a method for introducing an acidic group into a polyolefin-based resin, in addition to the above-mentioned method, a known method of acid-modifying a resin can be adopted.

[0245] The lower limit of the weight average molecular weight of the acid-modified polyolefin resin contained in the resin composition of the present invention is preferably 10,000 or more, more preferably 15,000 or more, further preferably 20,000 or more, further preferably 30,000 or more, and particularly preferably 40,000 or more, and the upper limit of the weight average molecular weight is preferably 60,000 or less, more preferably 55,000 or less, and further preferably 50,000 or less. When the weight average molecular weight of the acid-modified polyolefin resin is greater than the lower limit and less than the upper limit, the affinity of the thermoplastic plastomer with the hollow particles is improved, and it is easy to suppress the reduction of physical properties when the resin composition is made into a molded body.

[0246] In the present invention, the weight average molecular weight of a resin is a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0247] In addition, the acid value of the acid-modified polyolefin resin is more than 3.5 mgKOH / g, preferably more than 10 mgKOH / g, more preferably more than 15 mgKOH / g, and more preferably more than 20 mgKOH / g. If the acid value of the acid-modified polyolefin resin is more than the above lower limit, the thermoplastic plastomer has good affinity with the hollow particles, and therefore, it is possible to suppress the reduction of physical properties when the resin composition is made into a molded body. The upper limit of the acid value of the acid-modified polyolefin resin is not particularly limited, and from the viewpoint of affinity with the thermoplastic plastomer, it is preferably less than 150 mgKOH / g, more preferably less than 100 mgKOH / g, more preferably less than 80 mgKOH / g, more preferably less than 60 mgKOH / g, more preferably less than 50 mgKOH / g, and particularly preferably 30 mgKOH / g.

[0248] In the resin composition of the present invention, the content of the acid-modified polyolefin resin is not particularly limited, and is preferably 10 to 150 parts by mass, more preferably 20 to 100 parts by mass, and further preferably 30 to 70 parts by mass relative to 100 parts by mass of the hollow particles. When the content of the acid-modified polyolefin resin is above the above lower limit, the effect of suppressing the reduction of physical properties when the molded body is made and improving the mechanical strength is excellent. When the content of the acid-modified polyolefin resin is below the above upper limit, the thermoplastic plastomer and the hollow particles can be fully contained, and therefore, a resin composition with excellent strength after being lightened can be made.

[0249] [Other additives]

[0250] The resin composition of the present invention may contain additives such as ultraviolet absorbers, colorants, heat stabilizers, fillers, etc., in addition to the above-mentioned thermoplastic plastomer, hollow particles and acid-modified polyolefin resin, as required, within the range not impairing the effects of the present invention.

[0251] Furthermore, the resin composition of the present invention may further contain organic or inorganic fibers such as carbon fibers, glass fibers, aramid fibers, and polyethylene fibers.

[0252] Examples of uses of the resin composition of the present invention include the same uses as the uses of the molded article described below.

[0253] [Method for producing resin composition]

[0254] The method for manufacturing resin combination of the present invention can use the method used in the manufacture of previous resin combination, and is not particularly limited. For example, each component such as the above-mentioned thermoplastic plastomer, hollow particles, acid-modified polyolefin resin and other additives added as required can be mixed, and then melt-kneaded to obtain resin combination of the present invention.

[0255] Melt kneading can be performed by a known method without particular limitation, and can be performed using, for example, a melt kneading machine such as a single-screw extruder, a twin-screw extruder, a Banbury mixer, a heating roll, or various kneaders.

[0256] The temperature during melt kneading is not particularly limited as long as it is a temperature at which the thermoplastic plastomer used can be melted, but is preferably 250° C. or less from the viewpoint of suppressing the breakage of the hollow particles. When the resin composition of the present invention is made into pellets, the resin composition can be formed into pellets by a known molding method such as extrusion molding, injection molding, etc. after melt kneading.

[0257] 2. Molding

[0258] The molded body of the resin composition of the present invention is suppressed because the hollow particles contained in the molded body are crushed, so it is a molded body that suppresses the decrease in porosity and is lightweight. As a molding method for obtaining the molded body of the resin composition of the present invention, hollow particles that are not easily broken are used, therefore, the molding method performed under heating and pressurizing conditions such as injection molding and compression molding can be appropriately used. And then, it is possible to use known molding methods such as extrusion molding, hollow molding, calendering molding, inflation molding, blow molding, stretch molding and solution casting.

[0259] The molded body of the resin composition of the present invention may be in any shape such as a sheet, film, plate, tube, or other various three-dimensional shapes. In addition, when the molded body includes fibers, the fibers in the molded body may be in the form of a nonwoven fabric.

[0260] Examples of uses of the molded article of the resin composition of the present invention include light reflective materials, heat insulating materials, sound insulating materials, and low-dielectric components used in various fields such as automobiles, electrical, electronic, construction, aviation, and aerospace, food containers, shoes such as sports shoes and sandals, home appliance parts, bicycle parts, stationery, tools, and the like.

[0261] Example

[0262] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples. In addition, parts and % are based on mass unless otherwise specified.

[0263] As acid-modified polyolefin resins, PP1 (maleic anhydride-modified polypropylene, manufactured by Sanyo Chemical Co., Ltd., trade name: UMEX 1001) and PP2 (maleic anhydride-modified polypropylene, manufactured by Sanyo Chemical Co., Ltd., trade name: UMEX 1010) were prepared.

[0264] In addition, as an unmodified polyolefin-based resin for comparison, PP3 (low-molecular-weight polypropylene, manufactured by Sanyo Chemical Co., Ltd., trade name: VISCOL 660-P) was prepared.

[0265] Table 1 shows the types of resins used as raw materials, the types of acids used for acid modification, acid values, and weight average molecular weights (Mw) of these acid-modified polyolefin resins and comparative unmodified polyolefin resins.

[0266] [Table 1]

[0267] Table 1

[0268]

[0269] [Manufacturing Example 1: Manufacture of Hollow Particles]

[0270] (1) Mixed solution preparation process

[0271] First, the following materials are mixed to prepare an oil phase.

[0272] 100 parts of ethylene glycol dimethacrylate

[0273] 3 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (oil-soluble polymerization initiator, manufactured by Wako Pure Chemical Industries, Ltd., trade name: V-65)

[0274] 0.0044 parts of rosin acid

[0275] 187 parts of cyclohexane

[0276] Next, in a stirring tank, at room temperature, to an aqueous solution of 7.8 parts of magnesium chloride (water-soluble polymetallic salt) dissolved in 225 parts of ion exchange water, an aqueous solution of 5.5 parts of sodium hydroxide (alkali metal hydroxide) dissolved in 55 parts of ion exchange water was slowly added under stirring to prepare a magnesium hydroxide colloid (water-insoluble metal hydroxide colloid) dispersion to form an aqueous phase.

[0277] A mixed liquid is prepared by mixing the obtained aqueous phase and oil phase.

[0278] (2) Suspension preparation process

[0279] The mixed solution obtained in the mixed solution preparation step was suspended by stirring at 4000 rpm for 1 minute in a disperser (manufactured by Primix, trade name: HOMOMIXER) to prepare a suspension in which droplets of the monomer composition containing cyclohexane were dispersed in water.

[0280] (3) Polymerization process

[0281] The suspension obtained in the suspension preparation step was stirred for 4 hours in a nitrogen atmosphere at a temperature of 65° C. to perform a polymerization reaction. Through the polymerization reaction, a precursor composition containing precursor particles containing cyclohexane was prepared.

[0282] (4) Cleaning process and solid-liquid separation process

[0283] The precursor composition obtained in the above polymerization step was washed with dilute sulfuric acid (25°C, 10 minutes) to a pH of 5.5 or less. Then, after separating the water by filtration, 200 parts of ion exchange water were added again to re-slurry, and the water washing treatment (washing, filtration, dehydration) was repeated several times at room temperature (25°C), and the solid component was separated by filtration. The obtained solid component was dried at a temperature of 40°C in a dryer to obtain precursor particles containing cyclohexane.

[0284] (5) Solvent Removal Process

[0285] The precursor particles obtained in the solid-liquid separation step were heated in a vacuum dryer at 200°C for 6 hours under vacuum conditions to remove the hydrocarbon solvent in the hollows, thereby obtaining hollow particles of Production Example 1. The volume average particle size of the obtained hollow particles was 10.6 μm, and the porosity was 65%. In addition, the obtained hollow particles were confirmed to be spherical and have a hollow portion based on the results of observation with a scanning electron microscope and the value of the porosity.

[0286] [Example 1]

[0287] 85 parts of polypropylene (manufactured by Mitsubishi Chemical Corporation, trade name: MA1B, specific gravity: 0.90 g / cm2) as a thermoplastic plastomer was mixed with a stirrer. 3 , acid value 0mgKOH / g, SP value 8.0(cal / cm 3 ) 1 / 2 ), 10 parts of the hollow particles obtained in Production Example 1, and 15 parts (50 parts relative to 100 parts of the hollow particles) of the above-mentioned PP1 as an acid-modified polypropylene resin are mixed to obtain the resin composition of Example 1.

[0288] Next, the obtained resin composition was kneaded and extruded by a twin-screw kneading machine (product name "TEM-35B", manufactured by Toshiba Machine Co., Ltd.) under the following kneading conditions to form pellets, thereby obtaining pellets of the resin composition.

[0289] <Mixing conditions>

[0290] The screw diameter is 37mm, L / D=32

[0291] The screw speed is 250rpm

[0292] Resin temperature is 190℃

[0293] Feed rate is 6kg / hour

[0294] The obtained pellets of the resin composition were heated at 80° C. for 6 hours to be dried, and then, using an injection molding apparatus, a molded body having a size of 80 mm×10 mm×4 mm in thickness was obtained under the following molding conditions.

[0295] <Molding conditions>

[0296] Cylinder temperature: 200℃

[0297] Mold temperature: 70℃

[0298] Injection pressure: 70MPa

[0299] [Examples 2 to 5, Comparative Examples 1 to 3]

[0300] In Example 1, except that the type or addition amount of the thermoplastic plastomer or the type or addition amount of the acid-modified polyolefin resin was changed according to Table 2, the same procedure as in Example 1 was carried out to obtain resin compositions and molded bodies of Examples 2 to 5 and Comparative Examples 1 to 3.

[0301] [Reference Example 1]

[0302] A molded article of Reference Example 1 was obtained in the same manner as in Example 1 except that the polypropylene (PP) used as the thermoplastic plastomer in Examples 1 to 4 was used instead of the resin composition obtained in Example 1.

[0303] [Reference Example 2]

[0304] A molded article of Reference Example 2 was obtained in the same manner as in Example 1 except that the high-density polyethylene (HDPE) used as the thermoplastic plastomer in Example 5 was used instead of the resin composition obtained in Example 1.

[0305] [evaluate]

[0306] The following physical properties were measured for the molded products obtained in each of the Examples, Comparative Examples, and Reference Examples.

[0307] (1) Tensile strength

[0308] According to JIS-K7161-2, a tensile test was performed using a multipurpose test piece as a test piece at a test speed of 50 mm / min, a chuck distance of 115 mm, a test environment of 23° C., and 50% RH to measure the tensile strength.

[0309] (2) Bending strength

[0310] According to JIS K7171, a portion cut out from the central parallel portion of a multipurpose test piece was used as a test piece, and a bending test was performed at a test speed of 2 mm / min, a support distance of 64 mm, and a test environment of 23° C. and 50% RH to measure the bending strength.

[0311] (3) Flexural modulus

[0312] The bending test was carried out under the same conditions as those for measuring the above-mentioned bending strength, and the bending modulus was measured.

[0313] [Table 2]

[0314]

[0315] In Table 2, PP is polypropylene (manufactured by Mitsubishi Chemical Corporation, trade name: MA1B, specific gravity 0.90 g / cm 3 , acid value 0mgKOH / g, SP value 8.0(cal / cm 3 ) 1 / 2 ), HDPE is high-density polyethylene (manufactured by Mitsubishi Chemical Corporation, trade name: NOVATEC HD HJ590N, specific gravity 0.96 g / cm 3 , acid value 0mgKOH / g, SP value 8.0(cal / cm 3 ) 1 / 2 ).

[0316] The resin compositions obtained in Examples 1 to 4 and Comparative Examples 1 to 2 all contain polypropylene as a thermoplastic plastomer and hollow particles. However, the tensile strength, flexural strength and flexural modulus of the resin composition of Comparative Example 1 not containing an acid-modified polyolefin resin and the resin composition of Comparative Example 2 containing an unmodified low molecular weight polypropylene instead of an acid-modified polyolefin resin when formed into a molded body are greatly reduced compared to the molded body of the polypropylene shown in Reference Example 1. On the other hand, the tensile strength, flexural strength and flexural modulus of the resin compositions of Examples 1 to 4 containing an acid-modified polyolefin resin when formed into a molded body are almost not reduced, or are slightly improved compared to the molded body of the polypropylene shown in Reference Example 1, and even if hollow particles are contained, the reduction in physical properties when formed into a molded body is suppressed.

[0317] The resin compositions obtained in Example 5 and Comparative Example 3 both contain high-density polyethylene as a thermoplastic plastomer and hollow particles. However, the tensile strength, flexural strength and flexural modulus of the resin composition of Comparative Example 3 containing unmodified low-molecular-weight polypropylene instead of the acid-modified polyolefin resin when formed into a molded body are greatly reduced compared with the molded body of the high-density polyethylene shown in Reference Example 2. On the other hand, the tensile strength, flexural strength and flexural modulus of the resin composition of Example 5 containing the acid-modified polyolefin resin when formed into a molded body are almost not reduced, or are slightly improved compared with the molded body of the high-density polyethylene shown in Reference Example 2, and even if hollow particles are contained, the reduction in physical properties when formed into a molded body is suppressed.

[0318] Description of Reference Numerals

[0319] 1: Water-based medium 2: Low polarity material

[0320] 3: Dispersion stabilizer 4: Monomer composition

[0321] 4a: Hydrocarbon solvent 4b: Materials other than hydrocarbon solvent

[0322] 4c: polymerizable monomer dispersed in an aqueous medium 5: oil-soluble polymerization initiator

[0323] 6: Shell 8: Hollow part

[0324] 10: Droplets of monomer composition 20: Precursor particles

[0325] 100: Hollow particles

Claims

1. A resin composition comprising a thermoplastic plastomer having an acid value of less than 3.0 mgKOH / g, hollow particles, and an acid-modified polyolefin resin having an acid value of 3.5 mgKOH / g or more, The hollow particles have a shell composed of a resin and a hollow part surrounded by the shell, and the resin contains a polymer containing 30 to 100 parts by mass of a crosslinkable monomer unit in 100 parts by mass of all monomer units. The solubility parameter (SP value) of the thermoplastic plastomer is 13 (cal / cm 3 ) 1 / 2 Hereinafter, the content of the thermoplastic plastomer is 50 to 95% by mass. The crosslinkable monomer from which the crosslinkable monomer unit is derived is a hydrophilic crosslinkable monomer having a solubility of 0.3 g / L or more in distilled water at 20° C., The content of the acid-modified polyolefin-based resin is 10 to 150 parts by mass based on 100 parts by mass of the hollow particles.

2. The resin composition according to claim 1, wherein The acid-modified polyolefin-based resin has a weight average molecular weight of 15,000 or more.

3. The resin composition according to claim 1 or 2, wherein The acid-modified polyolefin-based resin is a carboxylic acid-modified polyolefin-based resin.

4. The resin composition according to claim 1 or 2, wherein The thermoplastic plastic is a polyolefin resin.