A composite corrosion inhibitor for electrolyte of alkaline aluminum-air battery
By using an electrolyte composite corrosion inhibitor composed of hydroxyethyl cellulose and potassium stannate in aluminum-air batteries, the problem of poor electrochemical performance of the aluminum anode is solved, achieving higher battery activity and life, and is suitable for large-scale applications .
Patent Information
- Application Number
- CN202310243459.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-03-14
AI Technical Summary
Existing aluminum-air batteries suffer from poor electrochemical performance due to the high hydrogen overpotential and high self-discharge rate of the aluminum anode, which hinders their commercial application.
An electrolyte composite corrosion inhibitor composed of hydroxyethyl cellulose and potassium stannate is used, combined with ingredients such as carboxymethyl cellulose, ethanol or ethylene glycol, to form an electrolyte for alkaline aluminum air batteries. Through synergistic effects Inhibit the self-corrosion of aluminum anodes and improve their activity and battery performance.
It significantly reduces the self-corrosion rate of the aluminum anode, increases the discharge voltage and power density, extends the life of the battery, and reduces the preparation cost, making it suitable for large-scale applications.
Smart Images

Figure CN116288365B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemistry, and in particular relates to an electrolyte composite corrosion inhibitor for alkaline aluminum-air batteries. Background Art
[0002] Metal-air batteries, as an emerging energy storage technology, have received increasing research attention in electric vehicles, consumer electronics, and stationary power plants. Unlike traditional batteries that store reagents inside the battery, metal-air batteries abandon the bulky cathode chamber and adopt an air-breathing structure to utilize oxygen in the air, which greatly reduces the overall weight of the battery and frees up space. Therefore, they are also considered to be a hybrid of traditional batteries and fuel cells.
[0003] Generally speaking, metal-air batteries consist of a suitable electrolyte, a metal anode, an air cathode, and a separator that disconnects the anode and cathode. The metal anode can be an alkali metal (such as Li, Mg), the metal with the highest earth content (such as Al), or a first-row transition metal with good electrochemical equivalence (such as Zn). They have a high theoretical energy density, about 3-30 times higher than that of lithium-ion batteries. Among them, aluminum-air batteries have the highest volumetric energy density of 21954Wh·L -1 (Mass energy density is 8100Wh·kg -1 ), expanding its potential applications in numerous fields, such as from small-scale applications in wearable devices to large-scale applications in electric vehicles.
[0004] However, the current aluminum anodes do not show satisfactory performance because their high hydrogen overpotential (passivation film formation) and high self-discharge rate (parasitic corrosion of aluminum-based anodes) seriously affect their electrochemical performance and hinder the commercialization of aluminum-air batteries. Adding corrosion inhibitors to the electrolyte is an effective way to improve the above problems. However, existing corrosion inhibitors (such as single potassium stannate additives) sacrifice anode activity while inhibiting the self-corrosion of aluminum anodes, which makes the discharge performance of aluminum-air batteries far from the goal of commercialization. Summary of the invention
[0005] The purpose of the present invention is to solve the problem of poor electrochemical performance of aluminum anode of aluminum-air battery, and provide an electrolyte composite corrosion inhibitor for alkaline aluminum-air battery. The electrolyte composite corrosion inhibitor is composed of a corrosion inhibitor, a thickener, a stabilizer and an inorganic additive. The corrosion inhibitor is mainly composed of hydroxyethyl cellulose (HEC) and potassium stannate, the thickener includes carboxymethyl cellulose and hydroxypropyl methyl cellulose, and the stabilizer includes ethanol, ethylene glycol or glycerol and an inorganic additive KI. The HEC and potassium stannate composite corrosion inhibitor has a synergistic effect, can effectively inhibit the self-corrosion of the aluminum anode, can greatly reduce the self-corrosion reaction rate of the battery, and the discharge voltage is also greatly improved, and has the characteristics of simple component composition, low cost, safety and compliance with environmental protection requirements. The thickener and stabilizer can ensure that HEC is uniform and stable during the electrolyte configuration process, and the inorganic additive can increase the conductivity of the electrolyte, and can also promote the large-scale adsorption of HEC on the surface of the aluminum anode.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A composite electrolyte corrosion inhibitor for alkaline aluminum-air batteries, comprising a corrosion inhibitor, a thickener, a stabilizer and an inorganic additive; the corrosion inhibitor comprises hydroxyethyl cellulose and potassium stannate, and the amount of hydroxyethyl cellulose used is 1 to 7 g·L -1 The amount of potassium stannate used is 3 to 18 g·L -1 . The specific preparation method is: prepare a hydroxyethyl cellulose aqueous solution, after the hydroxyethyl cellulose is completely dissolved, add a thickener, a stabilizer and an inorganic additive in sequence, stir and dissolve again, and finally add potassium stannate and stir until completely dissolved to obtain an electrolyte composite corrosion inhibitor; heating and stirring treatment is performed during the dissolution of the hydroxyethyl cellulose to increase the dissolution rate. It should be noted that the stabilizer must be added after the corrosion inhibitor and the thickener. The above stirring method is a conventional stirring method in the field, and technicians in this field can make a reasonable choice according to process requirements.
[0008] Furthermore, the potassium stannate is anhydrous potassium stannate or potassium stannate trihydrate.
[0009] Furthermore, the concentration of the hydroxyethyl cellulose is 2 to 5 g·L -1 , more preferably 3 g·L -1 Other values not listed within the numerical range also apply.
[0010] Furthermore, the concentration of potassium stannate is 9 to 15 g·L -1 , more preferably 12 g·L -1 . 3g·L -1 , 6g·L -1 , 9g·L -1 , 12g·L -1, 15g·L -1 or 18 g L -1 The same applies.
[0011] Furthermore, the thickener is hydroxypropyl methylcellulose and carboxymethyl cellulose, and hydroxypropyl methylcellulose is more preferred.
[0012] Furthermore, the stabilizer is ethanol, ethylene glycol and glycerol, and more preferably ethylene glycol.
[0013] Furthermore, the electrolyte of the alkaline aluminum-air battery contains sodium hydroxide or potassium hydroxide. The alkaline aqueous electrolyte can not only control the hydrogen evolution rate of the aluminum alloy anode, but also make the aluminum alloy anode have a higher electrochemical activity (i.e., a higher discharge voltage), which is of great significance for improving battery performance and extending discharge life, and is conducive to the large-scale promotion and application of aluminum-air batteries.
[0014] Furthermore, the concentration of the sodium hydroxide or potassium hydroxide is 1-7 mol·L -1 , for example, it can be 1 mol·L -1 , 2mol·L -1 , 3mol·L -1 , 4mol·L -1 , 5mol·L -1 , 6mol·L -1 or 7 mol·L -1 , but not limited to the listed values, other values not listed in the numerical range are also applicable. The maximum addition amount of the corrosion inhibitor does not exceed one thousandth of the mass of soda ash.
[0015] The beneficial effects of the present invention compared to the prior art are:
[0016] (1) The electrolyte corrosion inhibitor of the present invention utilizes the synergistic effect of hydroxyethyl cellulose and potassium stannate to form a tin layer with uniform porosity on the surface of the aluminum anode, which can not only significantly reduce the hydrogen evolution self-corrosion rate of the aluminum anode, but also significantly shift the open circuit potential and the working potential of the aluminum anode under the condition of impressed current to the negative direction, thereby improving the anode efficiency and making the aluminum anode have good corrosion resistance and high electrochemical activity, so as to meet the requirements of high current density discharge of alkaline aluminum-air batteries.
[0017] (2) The alkaline aqueous electrolyte for the aluminum-air battery of the present invention can not only control the problem of excessively rapid hydrogen evolution corrosion in the alkaline aluminum-air battery, but also ensure that the battery electrolyte remains active, which is of great significance for improving battery performance and extending discharge life, and is conducive to large-scale promotion and application.
[0018] (3) The preparation method of the aluminum-air battery electrolyte of the present invention is simple, easy, low-cost and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The power density curve of aluminum anode in alkaline aqueous electrolyte with different types of corrosion inhibitors added;
[0020] Figure 2 50mA·cm -2 Constant current discharge curve of single cells containing different types of corrosion inhibitors at current density. DETAILED DESCRIPTION
[0021] The technical solution of the present invention is further illustrated below through the drawings and embodiments, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0022] Hydroxyethyl cellulose (HEC) is a white powdery solid at room temperature. Hydroxyethyl cellulose has electronegative O-heteroatoms, heterocycles and alkyl chain groups. Its polar groups can be adsorbed on the surface of the aluminum anode, thereby inhibiting corrosion. Potassium stannate is an inorganic corrosion inhibitor that can inhibit hydrogen evolution and reduce the polarization of the aluminum anode, causing the aluminum anode potential to shift negatively. This is because potassium stannate will form a metal Sn layer on the surface of the aluminum anode after dissolution:
[0023]
[0024] However, when potassium stannate is used alone as a corrosion inhibitor, the tin layer deposited on the surface of the aluminum anode is uneven and has a high porosity, so it cannot play a good corrosion inhibition role. Through the synergistic effect of potassium stannate and hydroxyethyl cellulose, the addition of hydroxyethyl cellulose promotes the deposition of tin on the surface of the aluminum anode, thereby significantly changing the interface properties of Al / electrolyte, not only reducing polarization by activating the passivation layer, but also significantly improving the operating voltage and power density of the alkaline aluminum-air battery; moreover, the addition of hydroxyethyl cellulose enhances the geometric coverage effect of the tin layer, inhibits the aggregation and shedding of tin, is conducive to the uniform deposition and adsorption of tin, and makes the tin layer uniform and stable. Therefore, the present invention utilizes hydroxyethyl cellulose and potassium stannate to form an electrolyte corrosion inhibitor, so that a uniform porous layered structure can be formed on the surface of the aluminum anode.
[0025] Embodiment 1:
[0026] A method for preparing an alkaline aqueous electrolyte for an aluminum-air battery: adding a hydroxyethyl cellulose aqueous solution to a potassium hydroxide solution at room temperature, and after the hydroxyethyl cellulose is completely dissolved, adding a thickener, a stabilizer and an inorganic additive in sequence, stirring and dissolving again, and finally adding potassium stannate and stirring until completely dissolved to obtain an electrolyte composite corrosion inhibitor; heating and stirring treatment is performed during the dissolution of the hydroxyethyl cellulose to increase the dissolution rate. The amount of the hydroxyethyl cellulose used is 3g·L-1 The amount of potassium stannate used is 12 g·L -1 The concentration of potassium hydroxide is 4 mol·L -1 In this embodiment, hydroxyethyl cellulose and potassium stannate work together to have a better corrosion inhibition effect than a single corrosion inhibitor, and also greatly improve the activity of the aluminum anode.
[0027] Comparative Example 1:
[0028] A method for preparing an alkaline aqueous electrolyte for an aluminum-air battery: adding a formulated amount of an electrolyte slow-release agent to a potassium hydroxide solution at room temperature, and stirring until the mixture is uniform. The concentration of hydroxyethyl cellulose in the electrolyte corrosion inhibitor is 3 g·L -1 , the concentration of potassium hydroxide is 4 mol·L -1 .
[0029] Comparative Example 2:
[0030] A method for preparing an alkaline aqueous electrolyte for an aluminum-air battery: adding a formulated amount of an electrolyte slow-release agent to a potassium hydroxide solution at room temperature, and stirring until the mixture is uniform. The concentration of sodium stannate in the electrolyte corrosion inhibitor is 12 g·L -1 , the concentration of potassium hydroxide is 4 mol·L -1 .
[0031] Comparative Example 3:
[0032] An alkaline aqueous electrolyte for an aluminum-air battery, wherein the alkaline aqueous electrolyte is 4 mol·L -1 of potassium hydroxide solution.
[0033] Use Xinwei battery testing equipment to collect data, specific data information such as Figure 1 and 2 As shown, from Figure 1 It can be seen that with the increase of current density, the aluminum anode without corrosion inhibitor added at 110 mA cm -2 The maximum power density (79.5 mW cm -2 ), the aluminum anode with hydroxyethyl cellulose and potassium stannate added at 130 mA cm -2 and 135 mA cm -2 The maximum power density (105.5 and 112.3 mW·cm -2 ); Aluminum anode with composite corrosion inhibitor added at 140mA·cm -2 The power density reached 118 mW cm -2 .from Figure 2 As can be seen, at 50 mA cm -2The constant current discharge test was carried out at a current density of . The stable discharge voltage of the aluminum anode without corrosion inhibitor was only 1.1V, while the stable discharge voltages of the aluminum anode with the addition of hydroxyethyl cellulose, potassium stannate and composite corrosion inhibitor were 1.17V, 1.2V and 1.5V. This shows that the addition of corrosion inhibitor activates the aluminum anode, reduces the self-corrosion of the aluminum anode, and increases the discharge voltage and power density of the aluminum anode. Moreover, the composite corrosion inhibitor with the addition of hydroxyethyl cellulose and potassium stannate has a higher discharge voltage and power density. This is because of the synergistic effect of potassium stannate and hydroxyethyl cellulose. The addition of hydroxyethyl cellulose promotes the deposition of tin on the surface of the aluminum anode; moreover, the addition of hydroxyethyl cellulose enhances the geometric coverage effect of the tin layer, inhibits the aggregation and shedding of tin, is conducive to the uniform deposition and adsorption of tin, and makes the tin layer uniform and stable.
Claims
1. An electrolyte for an alkaline aluminum-air battery, characterized in that: The electrolyte comprises a corrosion inhibitor, a thickener, a stabilizer and an inorganic additive; the corrosion inhibitor comprises hydroxyethyl cellulose and potassium stannate, and the amount of hydroxyethyl cellulose used is 2-5 g·L -1 The amount of potassium stannate used is 9-15 g·L -1 ; The inorganic additive is KI; the thickener is hydroxypropyl methylcellulose; the electrolyte also contains sodium hydroxide or potassium hydroxide.
2. The electrolyte for alkaline aluminum-air battery according to claim 1, characterized in that: The potassium stannate is anhydrous potassium stannate or potassium stannate trihydrate.
3. The electrolyte for alkaline aluminum-air battery according to claim 1, characterized in that: The stabilizer includes ethanol, ethylene glycol or glycerol.
4. The electrolyte for alkaline aluminum-air battery according to claim 1, characterized in that: The concentration of the sodium hydroxide or potassium hydroxide is 1-7 mol·L -1 .
Citation Information
Patent Citations
Aluminum-air battery electrolyte, aluminum-air battery and manufacturing method thereof
CN107275720A