PU coating combination system and its coating body and application

By using high-functional polyisocyanate and hydroxyl components in PU coatings, the crosslinking point density is improved, and the problem of insufficient chemical resistance and hardness of traditional coating films is solved, and higher sunscreen and friction resistance are achieved. Improved production efficiency.

CN116410651BActive Publication Date: 2024-11-22SHANGHAI PHICHEM MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111679665.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-31
Publication Date
2024-11-22
Estimated Expiration
2041-12-31

AI Technical Summary

Technical Problem

The chemical resistance of multi-layer coatings of traditional automotive interior plastic parts, especially the poor sunscreen resistance, and the paint film has insufficient hardness and friction resistance, which cannot meet the manufacturer's testing requirements.

Method used

High-functional polyisocyanate (NCO functionality ≥10, NCO content ≥25%) is used as the curing agent, combining hydroxyl components and additives to form a PU coating combination system, improve crosslinking point density, and improve coating density and performance.

Benefits of technology

Significantly improve the chemical resistance of the coating, especially sunscreen resistance, increase the hardness and friction resistance of the paint film, while shortening the baking time, reducing energy consumption, and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0003453646420000091
    Figure BDA0003453646420000091
  • Figure BDA0003453646420000156
    Figure BDA0003453646420000156
Patent Text Reader

Abstract

The present invention relates to a PU coating combination system, which uses a high-functionality and high-NCO content polyisocyanate (NCO functionality ≥ 10, NCO content ≥ 25%) as a curing agent, and synergistically acts with components such as hydroxyl components and leveling agents, and can greatly improve the crosslinking point density without increasing or reducing the amount of curing agent, thereby significantly improving the density of the paint film, so that the chemical resistance of the paint film, especially the resistance to sunscreen, is significantly improved, the hardness and friction resistance of the paint film are also improved to a certain extent, and still maintain good adhesion, and there is no phenomenon such as orange peel. The present invention also relates to a coating body, including a topcoat film layer and a primer film layer made of the PU coating combination system. It also relates to the application of the PU coating combination system and the coating body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coatings, and in particular to a PU coating combination system and a coating body and application thereof. Background Art

[0002] In recent years, products involved in the automotive, mobile phone, home appliance and other industries often need to be coated on the surface to increase performance and aesthetics. First, apply a primer on the surface of the substrate, and then continue to apply a topcoat for decoration and protection. This is a common form of coating, among which polyurethane (PU) coatings can be used for plastic substrates. For coating products (or paint film products), there are certain requirements in terms of abrasion resistance, hardness, appearance, adhesion, chemical resistance and other properties.

[0003] Taking automobile interior plastic parts as an example, traditional automobile interior plastic parts multilayer coatings mostly use PU resin as the supporting material, and diisocyanate curing agents establish a cross-linked network between the molecular chains of the resin polymer. Specifically, the commonly used curing agents for PU topcoats in traditional automobile interior plastic parts multilayer coatings are diisocyanates or their oligomers (the main component is their trimers). For example, diisocyanates can be hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), etc. These diisocyanate curing agents carry ≤3 isocyanate groups (NCO) in their molecules, that is, the NCO functionality is ≤3, and can be coupled with the side chain hydroxyl groups of the resin molecules to form cross-linking points between the resin molecules. Commonly used diisocyanate trimer curing agents include: Covestro N3580BA, Asahi Kasei TKA100, Covestro N3390, Digo T1890E, Covestro Z4470, and Covestro N75.

[0004] However, the chemical resistance, especially sunscreen resistance, of these multi-layer coating products for automotive interior plastic parts is poor. The hardness and abrasion resistance of the paint films are also average, which cannot meet the testing requirements of various manufacturers on a large scale.

[0005] Therefore, it is necessary to further develop PU coatings with improved chemical resistance, hardness and wear resistance, as well as good adhesion. Summary of the invention

[0006] Based on this, one of the objects of the present invention is to provide a PU coating combination system with improved chemical resistance, hardness and wear resistance, and a coated body and application thereof.

[0007] The above-mentioned object of the invention can be achieved through the following technical solutions.

[0008] In a first aspect of the present invention, a PU coating system is provided, comprising component A1, component B1 and component C1;

[0009] Based on 100% by mass, the component A1 comprises:

[0010] Hydroxyl content 40% to 80%;

[0011] Leveling agent 0.6% to 2.5%; and

[0012] Mixed solvent 15% to 60%;

[0013] Wherein, the hydroxyl content of the hydroxyl component is 3% to 8%;

[0014] The component B1 comprises polyisocyanate; wherein the NCO functionality of the polyisocyanate is ≥10 and the NCO content is ≥25%;

[0015] The component C1 is a diluent;

[0016] The mass ratio of the component A1, the component B1 and the component C1 is 100:(10-50):(50-70).

[0017] In some embodiments, in the component A1,

[0018] The mass percentage of the hydroxyl component is 60% to 70%; and / or,

[0019] The weight average molecular weight of the hydroxyl component is 2000Da to 8000Da; and / or,

[0020] The viscosity of the hydroxyl component is 5000cps to 20000cps; and / or,

[0021] The leveling agent is a mixture of a polyether-modified silicone leveling agent and an acrylate leveling agent in a mass ratio of (1-10):(5-15); and / or,

[0022] The mixed solvent is a mixture of a low boiling point solvent with an initial boiling point ≤120°C, a medium boiling point solvent with an initial boiling point of 120°C to 150°C and a high boiling point solvent with an initial boiling point >160°C in a mass ratio of (1-4):(1-4):(1-4).

[0023] In some embodiments, in the component A1,

[0024] The hydroxyl component is one or more of hydroxyl acrylic resin, polyester resin and alkyd resin; and / or,

[0025] The hydroxyl content of the hydroxy acrylic resin is 4.2% to 6%; and / or,

[0026] The Tg of the hydroxy acrylic resin is 70° C. to 80° C.; and / or,

[0027] The hydroxyl content of the polyester resin is 5% to 8%; and / or,

[0028] The solid content of the polyester resin is 80% to 100%; and / or,

[0029] The Tg of the polyester resin is 50°C to 60°C; and / or,

[0030] The hydroxyl content of the alkyd resin is 5% to 6%; and / or,

[0031] The solid content of the alkyd resin is 70% to 80%; and / or,

[0032] The alkyd resin has a Tg of 50°C to 60°C; and / or

[0033] The hydroxyl component is selected from one or more of the following resin products: allnex 1198SS-70, allnex SM516, allnex 2803, Zhuohe HE6790, DIC A859, DIC A862 and Mitsubishi LR7728; and / or,

[0034] The polyether-modified silicone leveling agent is selected from one or more of the following models: BYK-306, BYK-331, TEGO 450, TEGO Glide 100 and TEGO 270; and / or,

[0035] The acrylic leveling agent is selected from one or more of the following models: EFKA3777, BYK358N, BYK361 and BYK381; and / or,

[0036] The initial boiling point of the low boiling point solvent is 75°C to 120°C, the initial boiling point of the medium boiling point solvent is 120°C to 160°C, and the initial boiling point of the high boiling point solvent is 160°C to 220°C;

[0037] The low boiling point solvent is one or both of ethyl acetate and isobutyl acetate; and / or,

[0038] The medium boiling point solvent is one or both of butyl acetate and methyl isobutyl ketone; and / or,

[0039] The high boiling point solvent is one or more of trimethylbenzene, tetramethylbenzene, diisobutyl ketone and diacetone alcohol.

[0040] In some embodiments, in the component B1,

[0041] The NCO functionality of the polyisocyanate is selected from 10 to 100; and / or,

[0042] The NCO content of the polyisocyanate is 25% to 30%; and / or,

[0043] The polyisocyanate has a structural unit shown in formula (I):

[0044] Wherein, R1 is H or methyl; R3 is C 1-8 Alkylene.

[0045] In some embodiments, in the component B1,

[0046] The NCO functionality of the polyisocyanate is selected from 10 to 40; and / or,

[0047] The polyisocyanate also has a structural unit represented by formula (II):

[0048] Wherein, R2 is H or methyl; R4 is selected from one or more of methyl, ethyl, propyl, isopropyl, butyl, isobutyl, hexyl, octyl, isooctyl, decyl, lauryl and isobornyl.

[0049] In some embodiments, in the component B1, the polyisocyanate has a general structure as shown in formula (III):

[0050] wherein n is numerically equal to the NCO functionality of the polyisocyanate, n is selected from an integer ≥ 10, m is an integer selected from 0 to 5; R3 is -(CH2) a -; wherein a is 1, 2 or 3; "*" indicates the connection site.

[0051] In some embodiments, the component C1 is a mixture of ethyl acetate, butyl acetate, diisobutyl ketone and propylene glycol methyl ether acetate in a mass ratio of (1-2):(0.5-1):(2.5-5):(1-2).

[0052] In a second aspect of the present invention, a coated body is provided, comprising a topcoat film layer, and also comprising a primer film layer stacked under the topcoat film layer; wherein the topcoat film layer is prepared by applying a PU coating composition formulated with the PU coating combination system described in the first aspect of the present invention on the surface of the primer film layer.

[0053] In some embodiments of the present invention, the primer film layer is made by coating a PU primer composition;

[0054] The PU primer composition is prepared from a PU primer combination system including component A2, component B2 and component C2;

[0055] The component A2 comprises the following components, in percentage by mass: 35% to 60% of a second hydroxy acrylic resin, 20% to 50% of a second mixed solvent and 10% to 25% of a second additive; wherein the second hydroxy acrylic resin has a hydroxyl content of 0.5% to 1% and a weight average molecular weight of 1000Da to 5000Da; the second mixed solvent is a mixture of ethyl acetate and butyl acetate in a mass ratio of (1 to 4):1; the second additive is one or more of a dispersant, an anti-settling agent, a matting powder, talcum powder, a black paste and a second leveling agent;

[0056] The component B2 is a diisocyanate oligomer with a degree of polymerization of ≤3;

[0057] The composition C2 is a mixture of ethyl acetate, acetone, isobutyl acetate and diacetone alcohol, and the mass ratio of the above components is (1-3): (1-3): (1-3): 1.

[0058] In the third aspect of the present invention, there is provided an application of the PU coating combination system described in the first aspect of the present invention or the coated body described in the second aspect of the present invention on a plastic substrate, wherein the plastic substrate includes a PC substrate, an ABS substrate, a HIPS substrate, a PMMA substrate and a plastic substrate of a PC / ABS composite material.

[0059] In the fourth aspect of the present invention, a PU paint film product is provided, comprising a plastic substrate and the coated body described in the second aspect of the present invention, wherein the plastic substrate is stacked under the primer film layer, the primer film layer is prepared by applying a PU primer composition on the surface of the plastic substrate, and the topcoat film layer is prepared by applying a PU coating composition prepared by the PU coating combination system described in the first aspect of the present invention on the surface of the primer film layer.

[0060] The sunscreen resistance, film hardness and friction resistance of traditional automotive interior plastic multilayer coatings are closely related to the crosslinking density in the system. The present invention introduces a synthetic high-functionality polyisocyanate (NCO functionality ≥ 10) as a curing agent, replacing conventional diisocyanate curing agents such as HDI and IPDI and oligomers thereof (NCO functionality ≤ 3), and synergizing with components such as hydroxyl components, auxiliary agents (such as leveling agents), greatly improving the crosslinking point density, thereby significantly improving the coating density, so that the coating chemical resistance, particularly sunscreen resistance has a significant improvement. Further, with the increase of crosslinking point density, the hardness and friction resistance of the paint film are also improved to a certain extent. In addition, due to the increase of the reaction site, relative to conventional curing agents such as HDI and IPDI, the reaction speed of coating curing is further accelerated, the baking time is shortened, the film forming time is reduced, operability is stronger, energy is saved, and production efficiency is accelerated.

[0061] In the conventionally used diisocyanate curing agent, after the diisocyanate forms a polymeric structure, the higher the degree of polymerization (the more NCO groups), the lower the content of active NCO (reactive NCO), that is, the increase in the degree of polymerization will reduce the content of active NCO, and the six-membered ring in the trimer is a very stable structure, which makes it difficult to form a structure with a higher degree of polymerization. The polyisocyanate curing agent used in the present invention can achieve high NCO functionality and high NCO content at the same time through structural design, so that the coating composition can be fully cross-linked without increasing the amount of curing agent used, or even reducing the amount of curing agent used.

[0062] That is to say, the polyisocyanate of the present invention has the characteristics of high functionality (NCO functionality ≥ 10) and high isocyanate content (NCO content ≥ 25%), so that the relative content of -NCO: -OH in the system can reach a fully reacted ratio (1 to 1.5): 1 by reducing the amount of curing agent added, and at the same time, the prepared coating has particularly improved hardness, friction resistance and chemical resistance.

[0063] The PU coating combination system provided by the present invention can also form a coating body together with a PU primer, which is applied to the surface of a substrate to provide a multi-layer coating film with particularly improved chemical resistance, sunscreen resistance, hardness and friction resistance. DETAILED DESCRIPTION

[0064] The present invention will be further described in detail below in conjunction with the embodiments and examples. It should be understood that these embodiments and examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. The purpose of providing these embodiments and examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive. It should also be understood that the present invention can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various changes or modifications without violating the connotation of the present invention, and the equivalent form obtained also falls within the protection scope of the present application. In addition, in the description below, a large number of specific details are given in order to provide a more comprehensive understanding of the present invention. It should be understood that the present invention can be implemented without one or more of these details.

[0065] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing implementation modes and embodiments and are not intended to limit the present invention.

[0066] the term

[0067] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0068] The terms "and / or", "or / and", and "and / or" used in this article include any one of two or more related listed items, and also include any and all combinations of related listed items, and the arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in this application, the technical solution undoubtedly includes technical solutions that are all connected by "logical and", and undoubtedly includes technical solutions that are all connected by "logical or". For example, "A and / or B" includes three parallel solutions of A, B and A+B. For example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, the technical solution that is all connected by "logical OR"), and also includes any and all combinations of A, B, C, and D, that is, the combination of any two or any three of A, B, C, and D, and also includes the combination of four of A, B, C, and D (that is, the technical solution that is all connected by "logical AND").

[0069] In the present invention, "plurality", "multiple", "multiple times", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.

[0070] As used herein, "combination thereof", "any combination thereof", "any combination thereof" etc. include all suitable combinations of any two or more of the listed items.

[0071] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc., shall be based on the ability to implement the technical solution of the present invention, solve the technical problem of the present invention, and achieve the expected technical effect of the present invention.

[0072] Herein, "preferred", "better", "more preferred" and "suitable" are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of the present invention. If multiple "preferred" items appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "preferred" item is independent.

[0073] In the present invention, “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.

[0074] In the present invention, "optionally", "optional", and "optional" mean optional, that is, any one of the two parallel solutions of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0075] In the present invention, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0076] In the present invention, the technical features described in an open format include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features. It should be understood that when the chemical composition of a substance is described in a restrictive format, the substance may contain impurities present in a normal content, including but not limited to impurities inevitably introduced during the preparation process.

[0077] In the present invention, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.

[0078] The temperature parameters in the present invention, if not specifically limited, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0079] As used herein, the term "alkylene" refers to a hydrocarbon group having two monovalent radical centers derived from an alkyl group by removing two hydrogen atoms, which may be a saturated branched alkyl group or a saturated straight chain alkyl group. For example, "C1-C8 alkylene" or "C1-8 "Alkylene" means that the alkyl portion contains 1 to 8 carbon atoms and each occurrence can be independently C1 alkylene, C2 alkylene, C3 alkylene, C4 alkylene, C5 alkylene, C6 alkylene, C7 alkylene or C8 alkylene. Suitable examples include, but are not limited to, methylene (-CH2-), 1,1-ethyl (-CH(CH3)-), 1,2-ethyl (-CH2CH2-), 1,1-propyl (-CH(CH2CH3)-), 1,2-propyl (-CH2CH(CH3)-), 1,3-propyl (-CH2CH2CH2-) and 1,4-butyl (-CH2CH2CH2CH2-).

[0080] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as a reference separately. Unless they conflict with the invention purpose and / or technical solution of the present application, the cited documents involved in the present invention are cited with all contents and all purposes. When the present invention involves cited documents, the definitions of relevant technical features, terms, nouns, phrases, etc. in the cited documents are also cited. When the present invention involves cited documents, the examples and preferred embodiments of the cited relevant technical features may also be incorporated into this application as references, but are limited to the ability to implement the present invention. It should be understood that when the content of the citation conflicts with the description in this application, the present application shall prevail or be modified adaptively according to the description of this application.

[0081] As used herein, PU refers to polyurethane, hydroxyl is OH, VOC refers to volatile organic compound, Tg refers to glass transition temperature, NCO represents the group -N=C=O, ABS substrate refers to a substrate composed of a terpolymer of three monomers: acrylonitrile (A), butadiene (B), and styrene (S), and PC substrate refers to a substrate composed of polycarbonate.

[0082] In the present invention, viscosity, unless otherwise specified, generally refers to Bush viscosity, with the unit being cps.

[0083] In the present invention, the hydroxyl content of the resin is expressed as a percentage, which represents the mass percentage of hydroxyl groups in a certain mass of the resin, and can be converted to the hydroxyl value.

[0084] In the present invention, NCO content refers to the mass percentage of NCO groups in a certain mass of a sample.

[0085] The solid content in the present invention, unless otherwise specified, is expressed in mass percentage.

[0086] In the present invention, "molecular weight" generally refers to average molecular weight unless otherwise specified. It may be weight average molecular weight or number average molecular weight, but generally refers to weight average molecular weight unless otherwise specified.

[0087] In the present invention, "room temperature" generally refers to 15°C to 35°C, and may further be 20°C to 30°C, unless otherwise specified.

[0088] In the present invention, the approximate numbers "about", "approximately", etc., unless otherwise specified, are allowed to fluctuate within a range of ±10%, and may further be ±5%, ±2%, etc. For example, about 20°C may be 20±2°C, 20±1°C, 20±0.5°C, etc. For example, a thickness of about 5 microns may be 5±0.5 microns, 5±0.2 microns, 5±0.1 microns, etc.

[0089] The "boiling point" in the present invention refers to the initial boiling point unless otherwise specified.

[0090] In the present invention, numerical values ​​"above" or "below" include the values ​​themselves unless otherwise specified.

[0091] A first aspect of the present invention

[0092] In the first aspect of the present invention, a polyurethane coating system (PU coating system) is provided, which can be formulated into a PU coating composition for coating (including but not limited to spraying). The PU coating system uses a high-functionality and high-NCO content polyisocyanate (NCO functionality ≥ 10, NCO content ≥ 25%) as a high-functionality and high-NCO content curing agent to replace conventional diisocyanate curing agents such as HDI and IPDI (low-functionality curing agents, NCO functionality ≤ 3, and NCO content decreases with increasing functionality), and synergizes with hydroxyl components, additives (such as leveling agents) and other components to greatly increase the crosslinking point density while reducing the amount of curing agent, thereby significantly improving the density of the paint film, so that the chemical resistance of the paint film, especially the resistance to sunscreen, is significantly improved, and at the same time, it can also maintain good paint film adhesion.

[0093] In some embodiments of the present invention, the PU coating system comprises component A1, component B1 and component C1 in a mass ratio of 100: (10-50): (50-70); the hydroxyl component in component A1 provides a resin component containing hydroxyl groups, component B1 is a curing agent (referred to as the first curing agent), and provides a polyisocyanate with high functionality and high NCO content (NCO functionality ≥ 10, NCO content ≥ 25%), and component C1 is a diluent (referred to as the first diluent). The three components work together to increase the crosslinking point density of the paint film while reducing the amount of curing agent, thereby achieving the above-mentioned comprehensive beneficial effects.

[0094] In some embodiments, the PU coating system comprises component A1, component B1 and component C1;

[0095] Based on 100% by mass, the component A1 comprises:

[0096] Hydroxyl content 40% to 80%;

[0097] Leveling agent 0.6% to 2.5%; and

[0098] Mixed solvent 15% to 60%;

[0099] Wherein, the hydroxyl content of the hydroxyl component is 3% to 8%;

[0100] The component B1 comprises polyisocyanate; wherein the NCO functionality of the polyisocyanate is ≥10 and the NCO content is ≥25%;

[0101] The component C1 is a diluent;

[0102] The mass ratio of the component A1, the component B1 and the component C1 is 100:(10-50):(50-70).

[0103] Component A1

[0104] Component A1 in the PU coating system provides a resin component containing hydroxyl groups.

[0105] In some embodiments of the present invention, component A1 includes a hydroxyl component, a leveling agent (referred to as a first leveling agent) and a mixed solvent (referred to as a first mixed solvent).

[0106] In some embodiments, based on 100% by mass, the component A1 includes:

[0107] Hydroxyl content 40% to 80%;

[0108] Leveling agent 0.6% to 2.5%; and

[0109] Mixed solvent 15% to 60%;

[0110] Wherein, the hydroxyl content of the hydroxyl component is 3% to 8%;

[0111] The component B1 includes polyisocyanate, wherein the NCO functionality of the polyisocyanate is ≥10 and the NCO content is ≥25%. In some embodiments, the mixed solvent includes a low boiling point solvent with an initial boiling point ≤120°C, a medium boiling point solvent with an initial boiling point of 120°C to 150°C, and a high boiling point solvent with an initial boiling point >160°C.

[0112] In some preferred embodiments of the present invention, component A1 includes the following components, in mass percentage:

[0113]

[0114] Preferably,

[0115] The hydroxyl content of the hydroxyl component is 3% to 8%;

[0116] Leveling agent A is a polyether-modified silicone;

[0117] Leveling agent B is acrylate;

[0118] The initial boiling point of the low boiling point solvent is 75°C to 120°C; the initial boiling point of the medium boiling point solvent is 120°C to 160°C (more preferably 120°C to 150°C); the initial boiling point of the high boiling point solvent is ≥160°C.

[0119] Hydroxyl component

[0120] The hydroxyl component serves as the main supporting material for the cross-linked network of the paint film, providing fullness, hardness and increased wear resistance.

[0121] The hydroxyl component in the present invention has a high hydroxyl content, which is conducive to improving the crosslinking point density. In some embodiments of the present invention, the hydroxyl content of the hydroxyl component is 3% to 8%. If the hydroxyl content is less than 3%, the appearance fullness will be affected, and the compactness of the paint film will be reduced, and the chemical resistance, hardness and wear resistance will be reduced; if the hydroxyl content exceeds 8%, the drying is too slow, which will lead to a prolonged reaction time, affecting the production efficiency, or the paint film is still soft after a certain surface drying time, and the yield rate is reduced. It is speculated that it is due to the following reasons: as the reaction proceeds, the molecular weight increases, the rotation and movement ability of the molecular chain will decrease, causing the reaction to become more and more difficult, and then the reaction speed is slower and slower. The higher the hydroxyl content, the longer the time required for the reaction of hydroxyl and isocyanate, and the production line using the PU coating composition for coating usually has a certain surface drying stage, generally less than 15 minutes. If the surface of the paint film is not dry during this period, the dust particles of the workpiece are more likely to stick to the surface during the transfer, thereby affecting the yield rate. In addition, if the hydroxyl content in the hydroxyl component is too high, it may lead to a low resin content in the formula, which will cause the system solid content to be too low and the film thickness cannot be guaranteed. The hydroxyl content of the hydroxyl component can further be 4% to 6%. The hydroxyl content of the hydroxyl component is 3%, 3.2%, 3.5%, 3.8%, 4%, 4.2%, 4.4%, 4.5%, 4.6%, 4.8%, 5%, 5.2%, 5.4%, 5.5%, 5.8%, 6%, 6.2%, 6.4%, 6.5%, 6.6%, 6.8%, 7%, 7.2%, 7.4%, 7.5%, 7.8%, 8%, etc. In some embodiments of the present invention, the mass percentage of the hydroxyl component in component A1 is 40% to 80%, and the hydroxyl content is 3% to 8%.

[0122] The molecular weight of the hydroxyl component preferably has a weight average molecular weight of 2000Da to 8000Da, so as to provide a suitable degree of polymerization and introduce a suitable number of hydroxyl groups into the polymer side chain. If the molecular weight is too low, the paint film may have poor compactness, and the cured paint film may have gaps and be easily corroded by chemicals; if the molecular weight is too high, the system needs to add more solvent to dissolve, which may cause the solid content of the system to be too low and the film thickness cannot be guaranteed. Examples of the molecular weight of the hydroxyl component are 2000Da, 3000Da, 4000Da, 5000Da, 6000Da, 7000Da, 8000Da, etc. The molecular weight of the hydroxyl component will affect the viscosity of the resin to a certain extent, and then affect the viscosity of the coating system, the reaction rate and the film formation time. In some embodiments of the present invention, the viscosity of the hydroxyl component is 5000 cps to 20000 cps, and further examples include 5000 cps, 6000 cps, 7000 cps, 8000 cps, 9000 cps, 10000 cps, 11000 cps, 12000 cps, 15000 cps, 16000 cps, 18000 cps, 20000 cps, etc. The molecular weight of the hydroxyl component will also affect the glass transition temperature (Tg) of the resin to a certain extent, thereby affecting the temperature range during coating.

[0123] The hydroxyl component raw material preferably has a higher solid content, for example, the solid content is 70% to 100%, and further examples include 70%, 72%, 74%, 75%, 76%, 78%, 80%, 82%, 84%, 85%, 86%, 88%, 90%, 92%, 94%, 95%, 96%, 98%, 100%, etc.

[0124] The PU coating system of the present invention can be used to cooperate with the PU primer system to form a surface paint film of a plastic part. The resin component in the primer system can be selected from one or more of hydroxy acrylic resin, polyester resin and alkyd resin, which is conducive to improving the adhesion between the primer and the substrate layer. In some embodiments of the present invention, the hydroxy component is one or more of hydroxy acrylic resin, polyester resin and alkyd resin, which is conducive to promoting the compatibility between the topcoat film layer and the primer film layer, improving the bonding force between the topcoat film layer and the primer film layer, and also conducive to forming a matching shrinkage between the topcoat film layer and the primer film layer, maintaining the flatness of the paint surface, and also playing a certain role in avoiding the occurrence of orange peel phenomenon.

[0125] The hydroxyl content of the hydroxy acrylic resin used in component A1 can be 4.2% to 6%, and further examples include 4.4%, 4.5%, 4.6%, 4.8%, 5%, 5.2%, 5.4%, 5.5%, 5.8%, 6%, etc. Tg can be 70°C to 80°C, and further examples include 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, etc.

[0126] The hydroxyl content of the polyester resin used in component A1 can be 5% to 8%, and further examples include 5%, 5.2%, 5.4%, 5.5%, 5.8%, 6%, 6.2%, 6.4%, 6.5%, 6.6%, 6.8%, 7%, 7.2%, 7.4%, 7.5%, 7.8%, 8%, etc. The solid content can be 80% to 100%, and further examples include 80%, 82%, 84%, 85%, 86%, 88%, 90%, 92%, 94%, 95%, 96%, 98%, 100%, etc. Tg can be 50°C to 60°C, and further examples include 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, etc.

[0127] The hydroxyl content of the alkyd resin used in component A1 can be 5% to 6%, and further examples include 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6%, etc. The solid content can be 70% to 80%, and further examples include 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, etc. The Tg can be 50°C to 60°C, and further examples include 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, etc.

[0128] In some embodiments of the present invention, the mass percentage of hydroxyl components in component A1 is 40% to 80%. If the hydroxyl component accounts for less than 40%, the solvent content of the system will be too high, VOC will exceed the standard, and the solid content of the system will be too low, and the film thickness cannot be guaranteed; if the hydroxyl component accounts for more than 80%, the viscosity will be too large, which is not conducive to dispersion and uniform stirring, affecting the construction. The mass percentage of hydroxyl components in component A1 can further be 50% to 70%, and further can be 60% to 70%, such as 40%, 42%, 44%, 45%, 46%, 48%, 50%, 52%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 78%, 80%, etc.

[0129] In some embodiments of the present invention, the hydroxyl component is selected from one or more of the following resin products: allnex 1198SS-70, allnex SM516, allnex 2803, Zhuohe HE6790, DIC A859, DIC A862, Mitsubishi LR7728, etc.

[0130] First leveling agent

[0131] The leveling agent in component A1 is recorded as the first leveling agent. The leveling agent used in the first aspect of the present invention can be any suitable leveling agent in the art.

[0132] In some embodiments of the present invention, the first leveling agent is a mixture of a polyether-modified silicone leveling agent and an acrylate leveling agent in a mass ratio of (1-10):(5-15).

[0133] In some embodiments, the first leveling agent includes leveling agent A and leveling agent B.

[0134] In some embodiments, the first leveling agent is composed of leveling agent A and leveling agent B; wherein, leveling agent A is a polyether-modified silicone, which can improve the appearance leveling and increase the smoothness; leveling agent B is an acrylate, which can improve the leveling, reduce short waves, and reduce orange peel.

[0135] Leveling agent A is used to improve the leveling property of the appearance and increase the smoothness. Leveling agent A is preferably a polyether-modified silicone, and can be further selected from one or more of the following models: BYK-306, BYK-331, TEGO 450, TEGO Glide100, TEGO 270, etc. The mass percentage of leveling agent A in component A1 is 0.1% to 1%, and can further be 0.1% to 0.5%, for example 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, etc.

[0136] Leveling agent B is used to improve leveling, reduce short waves, and reduce orange peel. Leveling agent B is preferably acrylate, and can be further selected from one or more of the following models: EFKA3777, BYK358N, BYK361, BYK381, etc. The mass percentage of leveling agent B in component A1 is 0.5% to 1.5%, and can further be 0.5% to 1%, for example 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, etc.

[0137] In component A1, the total mass fraction of leveling agent A and leveling agent B is preferably 0.8% to 2.5%, and more preferably 1% to 2%. For example, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, etc.

[0138] In component A1, the mass ratio of leveling agent A to leveling agent B is preferably 1:(1.5-2.5), for example 1:2.

[0139] The first mixed solvent

[0140] The mixed solvent in component A1 is referred to as the first mixed solvent.

[0141] In some embodiments, the first mixed solvent in component A1 adopts a mixed solvent of low boiling point, medium boiling point and high boiling point. Low boiling point solvent provides faster volatilization rate, can make the paint film surface drying speed faster, easier to film, reduce dust adhesion, and improve product yield rate. Medium boiling point solvent plays a role in balancing the volatilization rate, and a small part of the residual paint film has a slight bite corrosion to the primer, and can provide better adhesion. High boiling point solvent volatilization rate is slow, can ensure the wet film fluidity of the paint film, so as to bring better appearance leveling, can balance the volatilization rate at the same time, reduce the paint film defects such as prickly heat and pinholes caused by volatilization too fast.

[0142] The mass percentage of the low boiling point solvent, the medium boiling point solvent and the high boiling point solvent in component A1 can be 5-20% independently, for example 5%, 6%, 7%, 8%, 9%, 10%, 12%, 15%, 16%, 18%, 20%, etc. The total mass percentage of the low boiling point solvent, the medium boiling point solvent and the high boiling point solvent can be 25%-50%, for example 25%, 26%, 27%, 28%, 28.5%, 30%, 32%, 33.5%, 35%, 38%, 38.5%, 40%, 45%, 46%, 48%, 48.5%, 50%, etc.

[0143] The initial boiling point of the low boiling point solvent in component A1 is ≤120°C, preferably 75°C to 120°C, for example 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C. In some embodiments of the present invention, the low boiling point solvent in component A1 is one or more of ethyl acetate, isobutyl acetate, etc. In some embodiments of the present invention, the mass percentage of the low boiling point solvent in component A1 is 5 to 20%, for example 5%, 6%, 7%, 8%, 9%, 10%, 12%, 15%, 16%, 18%, 20%, etc.

[0144] The initial boiling point of the medium boiling point solvent in component A1 is selected from 120°C to 160°C, preferably 120°C to 150°C, for example 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, etc. In some embodiments of the present invention, the medium boiling point solvent in component A1 is one or more of butyl acetate, isobutyl ketone, etc. In some embodiments of the present invention, the mass percentage of the medium boiling point solvent in component A1 is 7.5-15%, for example 7.5%, 8%, 8.5%, 9%, 10%, 12%, 13%, 14%, 13.5%, 15%, 16%, 18%, 20%, etc.

[0145] The initial boiling point of the high boiling point solvent in component A1 is ≥160°C, preferably 160°C to 220°C, for example 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, etc. In some embodiments of the present invention, the high boiling point solvent in component A1 is preferably one or more of trimethylbenzene, tetramethylbenzene, diisobutyl ketone, diacetone alcohol, etc. In some embodiments of the present invention, the mass percentage of the low boiling point solvent in component A1 is 10 to 20%, for example 10%, 12%, 14%, 15%, 16%, 18%, 20%, etc.

[0146] In some embodiments of the present invention, the initial boiling point of the low boiling point solvent is ≤120°C (preferably 75°C to 120°C), the initial boiling point of the medium boiling point solvent is selected from 120°C to 160°C (preferably 120°C to 150°C), and the initial boiling point of the high boiling point solvent is ≥160°C (preferably 160°C to 220°C).

[0147] In some embodiments, the first mixed solvent is a mixture of a low boiling point solvent with an initial boiling point ≤120°C, a medium boiling point solvent with an initial boiling point of 120°C to 160°C (further such as 120°C to 150°C), and a high boiling point solvent with an initial boiling point >160°C in a mass ratio of (1 to 4): (1 to 4): (1 to 4).

[0148] In some embodiments of the present invention, the first mixed solvent is a mixture of ethyl acetate, butyl acetate and diacetone alcohol, and the mass ratio of the aforementioned components is 1: (0.4-2): (1-3), and can further be 1: 0.85: 1.5, 1: 1.35: 1.5, 1: (0.4-0.5): 1, 1: 0.425: 1, 1: 1.7: 3, etc.

[0149] Component B1 (first curing agent)

[0150] Component B1 in the PU coating combination system is a curing agent, denoted as the first curing agent, mainly composed of polyisocyanate with high functionality and high NCO content (NCO functionality is preferably ≥10, further preferably 10-100, and further can be 10-40; NCO content ≥25%). It should be understood that the high functionality here refers to a higher NCO functionality, which is numerically equal to the number of active NCO groups contained in a molecule. It should also be understood that impurities or other components with normal contents are allowed to exist, including but not limited to impurities inevitably introduced due to the preparation process. The content of polyisocyanate in component B1 is preferably ≥90%, more preferably ≥95%, more preferably ≥96%, more preferably ≥97%, more preferably ≥98%, and more preferably ≥99%. In a preferred embodiment, the content of polyisocyanate in component B1 is 100%.

[0151] In the conventionally used diisocyanate curing agent, after the diisocyanate forms a polymeric structure, the higher the degree of polymerization (the more NCO groups), the lower the content of active NCO (reactive NCO), that is, the increase in the degree of polymerization will reduce the content of active NCO, and the six-membered ring in the trimer is a very stable structure, which makes it difficult to form a structure with a higher degree of polymerization. The polyisocyanate curing agent used in the present invention can achieve high NCO functionality and high NCO content at the same time through structural design, so that the coating composition can be fully cross-linked without increasing the amount of curing agent used, or even reducing the amount of curing agent used.

[0152] In some embodiments of the present invention, component B1 is a polyisocyanate, and further, the NCO functionality is ≥ 10, further can be selected from 10 to 100, further can be 10 to 40, and can also be 15 to 35; examples of NCO functionality are 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, etc. Without special limitation, the NCO functionality in the present invention refers to the average value. The present invention can achieve high NCO functionality while also achieving high NCO content. In some embodiments of the present invention, the NCO content of the polyisocyanate in component B1 is ≥25%, and can further be 25% to 30%; examples of the NCO content are 25%, 26%, 27%, 28%, 29%, 30%, etc.

[0153] In some embodiments of the present invention, the NCO functionality of the polyisocyanate in component B1 is ≥10 (preferably 10 to 100, and more preferably 10 to 40), and the NCO content is ≥25% (preferably 25% to 30%).

[0154] In some preferred embodiments of the present invention, the NCO functionality of the polyisocyanate in component B1 is ≥10, and the NCO content is 25% to 30%. At this time, the coating film can also have better compactness when the amount of curing agent added is reduced. In order to avoid the coating film being too hard and brittle, the NCO functionality of the polyisocyanate is preferably ≤100, and the NCO functionality is more preferably 10 to 40. That is, by controlling the NCO functionality of the polyisocyanate in component B1 to 10 to 100, preferably 10 to 40, the resulting coating film can better have both improved wear resistance, chemical resistance and good flexibility.

[0155] The solids content of the polyisocyanate in component B1 is preferably 100%.

[0156] The polyisocyanate in component B1 is preferably in liquid form. In this case, the preferred solid content is 100%. Here, the solid content of 100% means that the curing agent does not need to be diluted with a solvent and can be used directly as a stock solution.

[0157] The polyisocyanate in component B1 mainly consists of polyisocyanate compounds.

[0158] In some embodiments of the present invention, the polyisocyanate in component B1 has a structural unit represented by formula (I):

[0159] Wherein, R1 is H or methyl; R3 is C 1-8 Alkylene, for specific definition, please refer to the above term part. R3 can be a straight chain or branched structure, preferably a straight chain structure. In some embodiments, R1 is H. In some embodiments, R1 is methyl.

[0160] In some embodiments, the polyisocyanate in component B1 further has a structural unit represented by formula (II):

[0161] Wherein, R2 is H or methyl; R4 is selected from one or more of methyl, ethyl, propyl, isopropyl, butyl, isobutyl, hexyl, octyl, isooctyl, decyl, lauryl and isobornyl. In the molecule of the polyisocyanate curing agent, each occurrence of R4 may be the same or different.

[0162] In some embodiments, the polyisocyanate in component B1 has a general structure as shown in formula (III):

[0163] wherein n is numerically equal to the NCO functionality of the polyisocyanate, n is selected from an integer ≥ 10, m is an integer selected from 0 to 5 (which may be 0, 1, 2, 3, 4 or 5); R3 is -(CH2) a-; wherein a is 1, 2 or 3; two "*" represent connection sites, which can be connected to other structural units or end groups in the molecule. In some embodiments, both "*" are connected to end groups. The end groups in formula (III) can be selected from the end groups that may be formed at the end of the polymerization reaction of acrylic monomers. The structures such as formula (III) and their end groups in the present invention are clear to those skilled in the art.

[0164] In some embodiments, the terminal groups in formula (III) are selected from The terminal groups formed by polymerization, or and The end group formed during copolymerization. When m = 0, formula (III) is The definition of two “*” is consistent with the above, and further, both can be connected to terminal groups.

[0165] In some preferred embodiments of the present invention, the polyisocyanate in component B1 has a general structure as shown in formula (IV):

[0166]

[0167] Wherein, n is numerically equal to the NCO functionality of the polyisocyanate, and n is selected from 10 to 40; the definitions of R3 and R1 are consistent with those above. Preferably, R3 is -(CH2) p -; wherein p is 1, 2, 3, 4, 5 or 6, further, p is 2, 4 or 6, and further is 2.

[0168] In some embodiments of the present invention, the polyisocyanate in component B1 is a general structure shown in formula (V): Wherein, any "*" is independently an end group allowed to be formed by polymerization of acrylic monomers, and the two "*" may be the same or different; the definitions of n, R3, and R1 (including preferred and exemplary) are consistent with those described above.

[0169] The polyisocyanate curing agent used in component B can be prepared by the polymerization reaction of acrylic isocyanate. Acrylic isocyanate refers to a molecule having C=CC(=O)- at one end and an isocyanate group at the other end, for example The definitions of R1 and R3 (including preferred and exemplary) are the same as those described above. Specific examples of acrylic isocyanate include ethyl isocyanate acrylate and ethyl isocyanate methacrylate. When the polymerization reaction is carried out, it is also possible to contain no or a small amount of Monomers can obtain polyisocyanates of the structure shown in formula (III).

[0170] By controlling the degree of polymerization and the size of the R3 and R1 groups (especially the size of the R3 group), the NCO functionality and NCO content of the polyisocyanate curing agent can be controlled. The greater the degree of polymerization, the higher the NCO functionality; if the R3 segment is too long, the NCO content will decrease.

[0171] Component C1 (diluent)

[0172] Component C1 in the PU coating system is a diluent (referred to as the first diluent), which can adjust the viscosity of the PU coating system and regulate the film-forming process, such as the film-forming time.

[0173] In some embodiments of the present invention, component C1 is selected from one or more of ethyl acetate, butyl acetate, diisobutyl ketone, propylene glycol methyl ether acetate, and the like.

[0174] In some embodiments of the present invention, component C1 is a mixture of ethyl acetate, butyl acetate, diisobutyl ketone and propylene glycol methyl ether acetate. The mass ratio of the above four components can be (1-2): (0.5-1): (2.5-5): (1-2). The mass ratio of the above four components can also be (1.5-2.5): 1: (2.5-7.5): (1-3). This mixed form of diluent is convenient for promoting the full solvent of each component of the PU coating combination system, making the PU coating composition prepared by the PU coating combination system more uniform, which is beneficial to improving the comprehensive performance of the paint film. In some embodiments of the present invention, the mass ratio of ethyl acetate, butyl acetate, diisobutyl ketone and propylene glycol methyl ether acetate is, for example, 2: 1: 5: 2.

[0175] Component A1, Component B1 and Component C1

[0176] In some embodiments of the present invention, in the PU coating combination system, the mass ratio of component A1, component B1 and component C1 is 100:(10-50):(50-70), for example, 100:(15-30):(50-70), for example, 100:25:60, 100:25:65, 100:15:55, 100:24:70, 100:24.75:60, 100:26.14:60, 100:25.34:65, 100:15.6:55, 100:23.65:70, etc.

[0177] Based on 100 parts by weight of component A1, the amount of component B1 can be 10 to 50 parts by weight, and further can be 15 to 30 parts by weight. The amount of component B1 relative to 100 parts by weight of component A1 is, for example, 10, 12, 15, 20, 25, 30, 35, 40, 45, 50, etc. parts by weight.

[0178] Based on 100 parts by weight of component A1, the amount of component C1 can be 50 to 70 parts by weight. The amount of component C1 relative to 100 parts by weight of component A1 is, for example, 50, 55, 60, 65, 70, etc. parts by weight.

[0179] Reasonable control of the mass ratio of component A1 and component B1 can control the molar ratio of -NCO to -OH at an appropriate ratio, which is more conducive to the full reaction between the hydroxyl component and the curing agent, and is more conducive to improving the film density, chemical resistance, sunscreen resistance and hardness while maintaining good film adhesion. In some embodiments of the present invention, in the PU coating combination system, the molar ratio of -NCO to -OH is (1 to 1.5): 1, further can be (1.1 to 1.5): 1, and further can be (1.4 to 1.5): 1. Examples of the molar ratio are (1.1: 1), (1.2: 1), (1.3: 1), (1.4: 1), (1.5: 1), etc.

[0180] If the amount of diluent is too little, it will be impossible to adjust to the required viscosity. If the amount is too much, the solid content of the coating system will be low, which is not conducive to film formation.

[0181] Packaging and usage

[0182] In the PU coating combination system, component A1, component B1, and component C1 can be packaged separately or in combination. Preferably, component A1 and component B1 are packaged separately.

[0183] When using the PU coating combination system, the components are mixed according to the corresponding mass percentages, dispersed evenly, and a PU coating composition of suitable viscosity is prepared, which can be used for coating. The viscosity of the PU coating composition used for coating is 8.5-11s (Iwata-2 cup, 25°C). A known suitable coating method can be used, including but not limited to spraying. The film thickness can be about 30-35μm, for example 30μm, 31μm, 32μm, 33μm, 34μm, 35μm, etc. Before coating, sieving can also be performed to remove insoluble particles; wherein, the mesh size of the sieve is, for example, 300 mesh.

[0184] It should be understood that since component A1, component B1, and component C1 can be weighed and mixed according to the required total mass and mass ratio when used, the mass ratio of each component does not need to be strictly in accordance with the mass ratio in the aforementioned guidelines when each component is packaged independently, as long as the provided packaging can provide a PU coating combination system for preparing the aforementioned mass ratio.

[0185] Second aspect of the present invention

[0186] In a second aspect of the present invention, a coated body is provided, comprising a topcoat film layer and a primer film layer stacked under the topcoat film layer; wherein the topcoat film layer is prepared from a PU coating composition formulated from the PU coating combination system described in the first aspect of the present invention.

[0187] The PU coating composition is coated on the surface of the primer film layer to prepare the coated body.

[0188] In some embodiments of the present invention, the primer film layer is formed by coating a primer composition prepared from a PU primer combination system.

[0189] In some embodiments of the present invention, the PU primer composition is formulated from a PU primer combination system, wherein the PU primer combination system includes component A2, component B2 and component C2, wherein component A2 provides a resin component, component B2 is a curing agent (referred to as the second curing agent), and component C2 is a diluent (referred to as the second diluent).

[0190] Component A2

[0191] In some embodiments of the present invention, component A2 includes the following components, in mass percentage: 35% to 60% of a hydroxylated acrylic resin (referred to as the second hydroxylated acrylic resin), 20% to 50% of a mixed solvent (referred to as the second mixed solvent) and 10% to 25% of an additive (referred to as the second additive).

[0192] In some embodiments of the present invention, the mass percentage of the second hydroxy acrylic resin in component A2 is 35% to 60%, for example 35%, 40%, 45%, 50%, 55%, 60%, etc.

[0193] In some embodiments of the present invention, the mass percentage of the second mixed solvent in component A2 is 20% to 50%, for example 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc.

[0194] In some embodiments of the present invention, the mass percentage of the second additive in component A2 is 10% to 25%, for example 10%, 11%, 12%, 13%, 14%, 15%, 20%, 21%, 22%, 23%, 24%, 25%, etc.

[0195] In some embodiments of the present invention, the hydroxyl content of the second hydroxylated acrylic resin is 0.5% to 1% (for example, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, etc.); and / or, the weight average molecular weight of the second hydroxylated acrylic resin is 1000Da to 5000Da (for example, 1000Da, 2000Da, 3000Da, 4000Da, 5000Da, etc.).

[0196] In some embodiments of the present invention, the second mixed solvent is a mixture of ethyl acetate and butyl acetate in a mass ratio of (1-4):1, for example 1:1, 1.5:1, 2:1, 3:1, 3.5:1, 4:1, etc.

[0197] In some embodiments of the present invention, the second additive is one or more of a dispersant, an anti-settling agent, a matting powder, talcum powder, a black paste, a leveling agent (referred to as a second leveling agent), etc. In some embodiments, the second additive includes 5% to 10% of matting powder and 1% to 6% of black paste; and / or, the second additive also includes 0.5% to 1% of an anti-settling agent and 0.1% to 0.5% of a leveling agent; and / or, the second additive also includes 3% to 8% of talcum powder and 2% to 4% of a dispersant.

[0198] Component B2

[0199] In some embodiments of the present invention, component B2 (second curing agent) is a diisocyanate oligomer (polymerization degree is generally ≤3, for example, polymerization degree is 3, i.e., trimer). In some preferred embodiments of the present invention, component B2 is selected from one or more of Covestro N3580BA, Asahi Kasei TKA100, Digo T1890E, Covestro Z4470, Covestro N75, etc.

[0200] Component C2

[0201] In some embodiments of the present invention, component C2 is selected from one or more of ethyl acetate, acetone, isobutyl acetate, diacetone alcohol, and the like.

[0202] In some embodiments of the present invention, component C2 is a mixture of ethyl acetate, acetone, isobutyl acetate and diacetone alcohol, and the mass ratio of the aforementioned components is (1-3):(1-3):(1-3):1.

[0203] In some embodiments of the present invention, in component A2, the hydroxyl content of the second hydroxy acrylic resin is 0.5% to 1%, and the weight average molecular weight is 1000Da to 5000Da; the second mixed solvent is a mixture of ethyl acetate and butyl acetate in a mass ratio of (1 to 4): 1; the second additive is one or more of a dispersant, an anti-settling agent, a matting powder, talcum powder, a black paste and a second leveling agent; and / or,

[0204] Component B2 is a diisocyanate oligomer; and / or,

[0205] Component C2 is a mixture of ethyl acetate, acetone, isobutyl acetate and diacetone alcohol, and the mass ratio of the above components is (1-3): (1-3): (1-3): 1, for example 3:3:3:1.

[0206] In some embodiments of the present invention, component A2: component B2 (curing agent): component C2 (diluent) = 100: (5-10): (80-100), for example 100: 5: 80.

[0207] The third aspect of the present invention

[0208] In a third aspect of the present invention, a use of the PU coating combination system described in the first aspect of the present invention or the coated body described in the second aspect of the present invention is provided.

[0209] In some embodiments of the present invention, the application includes but is not limited to application on a plastic substrate. Further, the plastic substrate includes a PC substrate, an ABS substrate, a HIPS substrate, a PMMA substrate, and a PC / ABS composite material plastic substrate.

[0210] In some embodiments of the present invention, the application is to prepare a multilayer coating film on a plastic substrate.

[0211] In some embodiments of the present invention, the application includes but is not limited to application in automobile interior materials. Preferably, the automobile interior material has a plastic substrate.

[0212] In some embodiments of the present invention, the application is an application in the preparation of automobile interior plastic parts. Preferably, the automobile interior plastic parts include a plastic substrate and a topcoat film layer formed by the aforementioned PU coating composition, and further include a primer film layer located between the plastic substrate and the topcoat film layer. Furthermore, the primer film layer is a primer film layer formed by the PU primer composition of the present invention. The PU primer composition can be selected from any PU primer composition described in the present invention (including but not limited to a primer composition prepared by any primer combination system).

[0213] In some embodiments of the present invention, the application comprises applying the PU coating composition prepared by the PU coating combination system provided in the first aspect of the present invention on the surface of the PU primer film layer, and drying to form a PU topcoat film layer.

[0214] A fourth aspect of the present invention

[0215] In the fourth aspect of the present invention, a PU paint film product is provided, comprising a plastic substrate and a coated body according to the second aspect of the present invention, wherein the plastic substrate is laminated under a primer film layer, further, the primer film layer is prepared by coating a PU primer composition on the surface of the plastic substrate, and the topcoat film layer is prepared by coating a PU coating composition prepared by the PU coating combination system according to the first aspect of the present invention on the surface of the primer film layer.

[0216] The PU primer composition is prepared from a PU primer combination system, which can be selected from any suitable primer combination system, including but not limited to the primer combination system described in the present invention.

[0217] In some embodiments of the present invention, the primer film layer is prepared by spraying the PU primer composition on the plastic substrate, the spray film thickness is about 15 μm to 25 μm, and then baking under heating conditions (such as 80° C.) for 30 minutes to solidify the film to obtain a cured primer layer, that is, the aforementioned primer film layer, which is directly laminated on the surface of the plastic substrate. The spraying can be performed using an Iwata W-100 spray gun. The material of the plastic substrate is, for example, an ABS+PC composite material.

[0218] In some embodiments of the present invention, the PU coating composition is coated on the surface of the primer film layer in the following manner: the raw materials in the PU coating combination system are added into a mixing tank according to the preparation ratio, and the component A1 is prepared after stirring at 600-800 r / min for 5-10 min in a disperser, and the component A1, the component B1 (the first curing agent), and the component C1 (the first diluent) are mixed in a suitable mass ratio, for example, in a mass ratio of 100: (25-50): (50-70), and then put into a disperser and stirred at 200-400 r / min for 2-5 min. After being evenly dispersed, it is filtered with a 300-mesh filter to obtain a PU coating composition with a viscosity of (8.5-11s, Iwata-2 cup, 25°C). The prepared PU coating composition is sprayed onto the surface of the cured primer layer using an Iwata W-100 spray gun, with a spray film thickness of about 30 μm to 35 μm. After standing at room temperature for 5 min to 8 min in a wet film state, it is placed in a 70°C to 80°C oven and baked for 1 h to 1.5 h to obtain a PU paint film product with a matte black texture. The coating thickness after drying and film formation is substantially the same as the thickness of the spray film. In some embodiments, the coating film thickness after film formation is 30 microns, 35 microns, etc. Specific embodiments

[0220] The embodiments of the present invention will be described in detail below in conjunction with examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are preferably referred to the guidance provided in the present invention, and can also be based on the experimental manual or normal conditions in this area, can also be based on the conditions recommended by the manufacturer, or refer to experimental methods known in the art.

[0221] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed.

[0222] In the following examples, unless otherwise specified, the room temperature is 20°C to 30°C.

[0223] 1. Raw materials and reagents

[0224] 1.1. Preparation of high-functionality polyisocyanates

[0225] Some exemplary high-functionality polyisocyanates have the structure of formula (V) or formula (III):

[0226]

[0227] In formula (V), the two "*" are independently The terminal groups generated during the polymerization reaction are H or methyl, R3 is ethylene, and n is 15, 23, 25, 30, and 35. The structures of the polyisocyanates represented by formula (V) in the following examples are shown in Table 2.

[0228] by The high-functionality polyisocyanate is prepared by polymerization of a monomer (the monomer used here is ethyl isocyanate). The length of time for the polymerization reaction can be monitored by infrared detection of the residual amount of carbon-carbon double bonds. The carbon-carbon double bonds involved here are CH2=CH- or CH2-C(CH3). Detection 1640cm -1 Characteristic infrared peaks at the position.

[0229] Taking n as an example, the preparation process is as follows: 20g of ethyl acetate (the solvent needs to be dehydrated) is added to the reactor, stirring is started, and the temperature is slowly raised to 70°C. 20g of ethyl isocyanate is dissolved in ethyl acetate, 0.3g of initiator AIBN is added, and the mixture is slowly dripped into the reactor. After the dripping is completed, the infrared 1640cm -1 After confirming that all double bonds have reacted, the reaction is terminated to obtain a polyisocyanate product P0a.

[0230] The structure of product P0a was confirmed by hydrogen spectrum nuclear magnetic resonance: deuterated chloroform was used as solvent, ppm was used as the chemical shift unit of characteristic peaks, 1 In the H NMR spectrum: δ1.92-2.00, 2.28-2.45 are hydrogens on the polymer main chain, proving that a polymer has been formed; δ3.57-3.63, 4.06-4.15 are continuous CH2 characteristic peaks.

[0231] In formula (III), the two "*" are each independently and The terminal groups formed during copolymerization, m is 1, 2, 3, 4, 5; R1 is H methyl, R2 is H or methyl, R3 is ethylene, R4 is methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, hexyl, n-octyl, isooctyl, decyl, lauryl or isobornyl, and n is 12, 18, 30, respectively. The structures of the polyisocyanates represented by formula (III) in the following examples are shown in Table 2.

[0232] by The high-functionality polyisocyanate is prepared by polymerization of monomers (the monomers used here are ethyl isocyanate and acrylate monomers). The length of time for the polymerization reaction can be monitored by infrared detection of the residual amount of carbon-carbon double bonds. The carbon-carbon double bond involved here is CH2=CH- or CH2-C(CH3). When the carbon-carbon double bond is CH2=CH-, the detection of 1640cm -1 Characteristic infrared peaks at the position.

[0233] The preparation process with n being about 12 and m being 1 is as follows: 20 g of ethyl acetate (the solvents all need to be dehydrated) is added to the reactor, stirring is started, and the temperature is slowly raised to 70°C. 18 g of ethyl isocyanate acrylate and 2 g of butyl methacrylate are dissolved in ethyl acetate, 1 g of initiator AIBN is added, and the mixture is slowly dripped into the reactor. After the dripping is completed, the infrared 1640 cm -1 After confirming that all double bonds have reacted, the reaction is terminated to obtain a polyisocyanate product P0b.

[0234] The structure of the product P0b was confirmed by hydrogen spectroscopy as follows: deuterated chloroform was used as solvent, ppm was used as the chemical shift unit of the characteristic peak, 1In the H NMR spectrum: δ1.92-2.00, 2.28-2.45 are hydrogens on the polymer main chain, proving that a polymer has been formed; δ3.57-3.63, 4.06-4.15 are continuous CH2 characteristic peaks on the n unit structure; δ4.06-4.09 are CH2 characteristic peaks close to O atoms on the m unit structure; δ1.36-1.59 are continuous CH2 characteristic peaks on the m unit structure;

[0235] The δ0.95-0.99 position is the terminal CH3 characteristic peak.

[0236] 1.2. Raw materials for PU topcoat (corresponding to PU coating combination system)

[0237] 1.2.1. Raw materials of component A1

[0238] The raw materials and mass fractions of the PU topcoat main agent (component A1) used in the following examples and comparative examples are shown in Table 1. The total mass of component A1 in each example is 100 g.

[0239] The hydroxyl components used were commercially available Allnex SM516 / 70BAC, Allnex 2803 / 78BAC, Zoho HE6790, DSMCY472, and Worléepol 1181 / 03.

[0240] Allnex SM516 / 70BAC: hydroxyl acrylic resin with hydroxyl content of 5.5% and solid content of 70%;

[0241] Allnex 2803 / 78BAC: polyester resin with 6.0% hydroxyl content and 80% solid content;

[0242] Zhuohe HE6790: Hydroxyl acrylic resin with hydroxyl content of 4.5% and solid content of 70%;

[0243] DSM CY472: hydroxyl acrylic resin with hydroxyl content of 1.7% and solid content of 57%;

[0244] Worléepol 1181 / 03: A polyester resin with a hydroxyl content of 10% and a solid content of 100%.

[0245] Among them, "hydroxyl content" is the mass content of hydroxyl groups in the solid resin, and the actual hydroxyl content of each resin raw material is the hydroxyl content in the solid resin × solid content; the hydroxyl value of the resin raw material is the actual hydroxyl content × 33. Taking Allnex SM516 / 70BAC as an example, the hydroxyl value is 5.5 × 33 × 0.7 = 127.05 mgKOH / g.

[0246] Table 1. Raw materials and mass fractions of PU topcoat main agent (component A1)

[0247]

[0248] 1.2.2. Ratio of each component in PU topcoat

[0249] The matching relationship between component A1 (main agent), component B1 (curing agent), and component C1 (diluent) in the embodiments and comparative examples is shown in Table 2.

[0250] The calculation formula of curing agent dosage is as follows: NCO =(7.5×(ratio of -NCO to -OH in the system)×hydroxyl value×(resin content percentage)) / (NCO content×100).

[0251] Table 2. The matching relationship between component A1 (main agent), component B1 (curing agent), and component C1 (diluent) in PU topcoat.

[0252]

[0253] The PU topcoat thinner is a mixture of ethyl acetate, butyl acetate, diisobutyl ketone and propylene glycol methyl ether acetate in a mass ratio of 2:1:5:2.

[0254] 1.3. Raw materials for the preparation of PU primer composition

[0255] The raw materials and mass proportions used for component A2 in the PU primer composition are shown in Table 3.

[0256] Table 3.

[0257] raw material Mass percentage (%) Mitsubishi LR-7791 40 Dispersant BYK: P-104S 5 Polyamide wax paste: Desbaron 6900-HV 5 Matting powder OK520 10 talcum powder 5 Black pulp 5 Leveling agent BYK-306 0.2 Ethyl acetate 20 Butyl acetate 9.8 total 100

[0258] The diluent in the PU primer composition is a mixture of ethyl acetate, acetone, isobutyl acetate and diacetone alcohol in a mass ratio of 3:3:3:1.

[0259] 2. Preparation of coating system

[0260] The preparation process of the coating system of the embodiment and the comparative example is as follows:

[0261] After the primer component A2 (Table 3) and component B2 (N3390) were mixed at a mass ratio of 100:5, a diluent (component C2) of 80% of the mass of component A2 was added, and after stirring evenly, it was sprayed onto an ABS+PC plastic substrate with an Iwata W-100 spray gun and baked at 80°C for 30 minutes to prepare a primer film with a thickness of about 20 μm.

[0262] Then, PU topcoat was applied on the cured primer film: the topcoat raw materials in the embodiment and comparative example in Table 1 were added into the batching tank according to the preparation ratio, and component A1 was obtained after being evenly dispersed. Component A1 (Table 1), component B1 (Table 2) and diluent (component C1) in the topcoat were evenly mixed according to the mass ratio (viscosity was 9s, W-100 spray gun, 25°C) and sprayed on the surface of the primer film. The sprayed film thickness was about 32 μm. After standing at room temperature for 6 minutes in the wet film state, the system was fully leveled, and then placed in a 70°C oven for baking to fully cure the system to obtain a PU coating film (coating film to be tested), and the adhesion was tested.

[0263] 3. Test items (TL226 automotive interior test standard)

[0264] After testing the adhesion of the PU coating film, the film was baked at a temperature of 60°C to 80°C for 48 hours, and then other items were tested. The test results are shown in Table 4.

[0265] 3.1. Adhesion test: ISO 2409-2013: 1mm grid and then test with tape, which is required to reach level 0.

[0266] 3.2. Hardness test: GB T6739-2006 Chinese pencil, load 500g, requirement ≥H.

[0267] 3.3. Abrasion resistance test: The coating to be tested is subjected to a dry cloth friction resistance discoloration test, and the wear resistance of the coating is determined according to the number of frictions, the wear level, and the gray card level of the friction cloth. The more frictions, the smaller the wear level, and the larger the gray card level of the friction cloth, which means that the smaller the external friction marks, the better the friction resistance of the coating. The wear level is required to be ≤2, and there is no color change on the white cloth (according to the gray card level of the friction cloth used for the DIN EN 20105-A03 standard test, the gray card fastness level is required to be ≥4).

[0268] 3.4. Chemical resistance test: The drop test and cream resistance test were used to characterize the chemical resistance of the coating film.

[0269] 3.4.1. Spot test: Synthesize sweat A (acetic acid with a volume ratio of 0.75%, prepared by the following method: add 7.5mL of 100% acetic acid and distilled water to make up to 1L), use a pipette to drop 0.1mL of the solution (sweat A) on the surface of the coating to be tested, expose for 10 minutes, dry in a high-temperature oven at 60°C for 30 minutes, and observe the surface of the coating after 24 hours. The appearance of the coating is required to have no visible changes.

[0270] 3.4.2. Face cream resistance test (Volkswagen, Chery): Generally, the larger the SPF value of the face cream, the higher the test temperature and the longer the test time, the more difficult it is for the coating to withstand. Thierry GmbH sunscreen (Volkswagen) and NIVEA SPF50+++ sunscreen were used, respectively, and placed in a high temperature box at 100℃ for 2h (test one) and 80℃ for 24h (test two). The coating was required to have no changes in appearance and touch (such as lines, swelling, cracks, softening, and stickiness). Then the coating gray card grade was tested according to DIN EN 20105-A02 standard. A gray card grade of ≥4 means that there is no visible difference in color before and after the coating test, and there is no fading or blooming phenomenon. The substrate adhesion and hardness were further tested.

[0271] 3.5. Appearance leveling test: DOI orange grain instrument requirement ≥90.

[0272] 3.6. Surface drying speed: bake at 80℃ and record the touch drying time, which should be ≤15min.

[0273] 3.7. Drying speed: bake at 80℃ and record the drying time; the coating provided by the present invention is judged whether it is dry according to the cotton ball pressing method in GB / T 1728-1979 (1989) "Determination of drying time of paint film and putty". "hr" means "hour".

[0274] Table 4. Test results

[0275]

[0276] As shown in Table 2 and Table 4, Example 1 and Comparative Example 3 keep other conditions unchanged, change the NCO content to 25% to 30%, and change the high-functionality polyisocyanate curing agent with a functionality of 10 or more. While reducing the amount of curing agent, the density of the coating film can also be greatly improved, thereby preparing a coating film with improved hardness, actual drying speed, wear resistance and chemical resistance, especially the tolerance of the coating film to cream is greatly improved, and it can withstand the cream test with stricter conditions. At the same time, through the optimization of component A1, the combination of a polyisocyanate with a functionality of preferably 10 to 100 (more preferably 10 to 40) and a high NCO content makes the prepared coating film have good substrate adhesion, leveling effect and surface drying speed.

[0277] The technical features of the above-mentioned implementation modes and examples can be combined in any appropriate manner. To make the description concise, not all possible combinations of the technical features in the above-mentioned implementation modes and examples are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0278] The above-described embodiments only express several implementation methods of the present invention, which is convenient for understanding the technical solution of the present invention in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present invention, several variations and improvements can be made, which all belong to the protection scope of the present invention. In addition, it should be understood that after reading the above-mentioned teaching content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and the equivalent forms obtained also fall within the protection scope of this application. It should also be understood that the technical solutions obtained by those skilled in the art on the basis of the technical solution provided by the present invention through logical analysis, reasoning or limited experiments are all within the protection scope of the claims attached to the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A coated body, It is characterized in that It includes a topcoat film layer and a primer film layer stacked under the topcoat film layer; wherein the topcoat film layer is prepared from a PU coating composition prepared from a PU coating combination system; The PU coating combination system comprises component A1, component B1 and component C1; In terms of mass percentage, the component A1 comprises: Hydroxyl content 50%~70%; First leveling agent 0.6%~2.5%; and The first mixed solvent is 15% to 60%; The weight average molecular weight of the hydroxyl component is 2000 Da to 8000 Da, and the viscosity is 5000 cps to 20000 cps; the hydroxyl component is one or more of a hydroxyl acrylic resin and a polyester resin; the hydroxyl content of the hydroxyl acrylic resin is 4.2% to 6%, and the Tg is 70°C to 80°C; the hydroxyl content of the polyester resin is 5% to 8%, the solid content is 80% to 100%, and the Tg is 50°C to 60°C; The first mixed solvent is a mixture of a low boiling point solvent, a medium boiling point solvent and a high boiling point solvent in a mass ratio of (1-4):(1-4):(1-4), wherein the initial boiling point of the low boiling point solvent is 75°C-120°C, the initial boiling point of the medium boiling point solvent is 120°C-160°C, and the initial boiling point of the high boiling point solvent is 160°C-220°C; The component B1 is polyisocyanate; wherein the NCO functionality of the polyisocyanate is 10-40, and the NCO content is 25%-30%; In the component B1, the polyisocyanate has a general structure shown in formula (III): (III); wherein n is numerically equal to the NCO functionality of the polyisocyanate, n is an integer selected from 10 to 40, and m is an integer selected from 0 to 2; R 1 is H or methyl; R 2 is H or methyl; R 3 For -(CH 2 ) a -; wherein a is 2 or 3; "*" indicates the connection site; R 4 One or more selected from methyl, ethyl, propyl, butyl, hexyl, octyl, decyl, lauryl and isobornyl; The component C1 is a diluent; the component C1 is a mixture of ethyl acetate, butyl acetate, diisobutyl ketone and propylene glycol methyl ether acetate in a mass ratio of (1-2): (0.5-1): (2.5-5): (1-2); In the PU coating combination system, the molar ratio of -NCO to -OH is (1.1-1.5): 1; The mass ratio of the component A1, the component B1 and the component C1 is 100:(10-50):(50-70); The primer film layer is formed by coating a PU primer composition; the PU primer composition is prepared from a PU primer combination system including component A2, component B2 and component C2; In terms of mass percentage, the component A2 comprises: 35% to 60% of a second hydroxy acrylic resin, 20% to 50% of a second mixed solvent and 10% to 25% of a second additive; wherein the second hydroxy acrylic resin has a hydroxy content of 0.5% to 1% and a weight average molecular weight of 1000 Da to 5000 Da; the second mixed solvent is a mixture of ethyl acetate and butyl acetate in a mass ratio of (1 to 4): 1; the second additive is one or more of a dispersant, an anti-settling agent, a matting powder, talcum powder, a black paste and a second leveling agent; The component B2 is a diisocyanate oligomer, and the polymerization degree of the diisocyanate oligomer is ≤3; The component C2 is a mixture of ethyl acetate, acetone, isobutyl acetate and diacetone alcohol in a mass ratio of (1-3):(1-3):(1-3):

1.

2. The coated body according to claim 1, It is characterized in that In the component A1, The mass percentage of the hydroxyl component is 60% to 70%; and / or, The first leveling agent is a mixture of a polyether-modified silicone leveling agent and an acrylate leveling agent in a mass ratio of (1-10):(5-15).

3. The coated body according to claim 2, It is characterized in that In the component A1, The hydroxyl component is selected from one or more of the following resin products: allnex 1198SS-70, allnex SM516, allnex 2803, Zhuohe HE6790, DIC A859 and Mitsubishi LR7728; and / or, The polyether-modified silicone leveling agent is selected from one or more of the following models: BYK-306, BYK-331, TEGO 450, TEGO Glide 100 and TEGO 270; and / or, The acrylic leveling agent is selected from one or more of the following models: EFKA3777, BYK358N, BYK361 and BYK381; and / or, The low boiling point solvent is one or both of ethyl acetate and isobutyl acetate; and / or, The medium boiling point solvent is butyl acetate; and / or, The high boiling point solvent is one or more of trimethylbenzene, tetramethylbenzene, diisobutyl ketone and diacetone alcohol.

4. The coated body according to claim 1, It is characterized in that In the component B1, the NCO functionality of the polyisocyanate is 10-35.

5. The coated body according to claim 4, It is characterized in that R 4 One or more selected from methyl, ethyl, propyl and butyl.

6. The coated body according to claim 5, It is characterized in that a is 2.

7. The coated body according to any one of claims 1 to 6, It is characterized in that The component C1 is a mixture of ethyl acetate, butyl acetate, diisobutyl ketone and propylene glycol methyl ether acetate in a mass ratio of 2:1:5:

2.

8. The coated body according to claim 1, It is characterized in that The mass ratio of the component A1, the component B1 and the component C1 is 100: (15-30): (50-70); In the component A1, the first mixed solvent is a mixture of ethyl acetate, butyl acetate and diacetone alcohol in a mass fraction of 1:(0.4-2):(1-3); In the component A1, the first leveling agent consists of a leveling agent A and a leveling agent B, wherein the leveling agent A is a polyether-modified silicone leveling agent, and the leveling agent B is an acrylate leveling agent, and the mass ratio of the leveling agent A to the leveling agent B is 1:(1.5-2.5).

9. Use of the coated body according to any one of claims 1 to 8 on a plastic substrate, wherein the plastic substrate comprises a PC substrate, an ABS substrate, a HIPS substrate, a PMMA substrate and a PC / ABS composite material plastic substrate.

10. A PU paint film product, It is characterized in that The invention comprises a plastic substrate and a coating body as claimed in any one of claims 1 to 8, wherein the plastic substrate is laminated under the primer film layer, the primer film layer is prepared by coating a PU primer composition on the surface of the plastic substrate, and the topcoat film layer is prepared by coating a PU coating composition prepared by the PU coating combination system on the surface of the primer film layer.