A method for preparing a lithium supplement and a negative electrode sheet and its application.

By using lithium metal wire inside a polymer tube as a lithium replenishing agent in the negative electrode sheet, the safety hazards and dispersion difficulties of lithium powder and lithium blocks in the negative electrode lithium replenishment process are solved, achieving efficient lithium replenishment and long life of lithium batteries.

CN116417599BActive Publication Date: 2026-11-10BYD CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111637173.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-29
Publication Date
2026-11-10
Estimated Expiration
2041-12-29

AI Technical Summary

Technical Problem

In existing technologies, lithium powder and lithium blocks pose safety hazards and have difficulty in dispersion during the negative electrode lithium replenishment process, resulting in low initial coulombic efficiency of lithium batteries.

Method used

Lithium metal wires inside a polymer tube are used as lithium replenishing agents. High-speed shearing is used to uniformly disperse the lithium metal, forming a polymer fiber network matrix, which improves the bonding force between lithium metal and negative electrode active material.

Benefits of technology

This method achieves uniform dispersion of lithium metal in the negative electrode active material, improves the initial coulombic efficiency and discharge capacity of lithium batteries, and extends the battery's lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003441980920000111
    Figure BDA0003441980920000111
Patent Text Reader

Abstract

This application provides a lithium replenishing agent, a method for preparing a negative electrode sheet, and their applications. The lithium replenishing agent comprises a polymer tube and lithium metal wires contained within the polymer tube. The parameterized lithium replenishing agent provided in this application enables precise lithium replenishment to the battery negative electrode. Furthermore, after shearing, the lithium replenishing agent can be transformed into a lithium source and a polymer fiber network, which, when mixed with the negative electrode active material, can be formed into a negative electrode active material film with a certain structural strength. The negative electrode sheet prepared using the above-mentioned negative electrode active material film replenishes the irreversible capacity loss of the battery during the first charge and discharge process, thereby improving the battery's discharge capacity and initial coulombic efficiency, and extending the battery's service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of lithium-ion batteries, specifically to a method for preparing a lithium replenishing agent and a negative electrode sheet, and their applications. Background Technology

[0002] Currently, the industry often uses the method of negative electrode lithium replenishment to improve the first coulombic efficiency of lithium batteries. Generally, lithium metal materials such as lithium blocks, lithium powder, and lithium foil are directly mixed into the negative electrode or pressed onto the surface of the negative electrode active material to achieve negative electrode lithium replenishment. However, during the processing, the mixing of lithium powder involves safety issues such as dust, flammability and explosion, while lithium blocks have problems such as difficulty in dispersion during the mixing process. Summary of the Invention

[0003] In view of this, this application provides a method for preparing a lithium replenishing agent and a negative electrode sheet, and its application. By using a lithium metal wire contained in a polymer tube as a negative electrode lithium replenishing agent, it is easy to uniformly disperse lithium metal when mixed with the negative electrode active material, and there are no safety hazards in the above mixing process.

[0004] Specifically, the first aspect of this application provides a lithium replenishing agent comprising a polymer tube and a lithium metal wire contained within the polymer tube.

[0005] Containing lithium metal wire within polymer tubes protects it from damage by air and moisture, preventing the formation of lithium oxide and lithium hydroxide upon contact with air, which could affect the accurate calculation of lithium replenishment. Furthermore, the lithium metal wire is easily sheared and dispersed during high-speed shearing, ensuring uniform dispersion within the negative electrode active material. Simultaneously, the polymer tubes in the lithium replenishment agent are sheared, dispersed, and fibrillated under high shear, forming a polymer fibrillation network matrix. This matrix also acts as a binder for the lithium metal and the negative electrode active material, enhancing their bonding strength. This integrated lithium replenishment agent effectively solves the problem of difficult dispersion of lithium metal and binders within the negative electrode active material.

[0006] In some embodiments of this application, the diameter d1 of the lithium metal wire is 0.005mm-10mm. Exemplarily, it can be 0.005mm, 0.01mm, 0.05mm, 0.1mm, 0.3mm, 0.6mm, 1mm, 2mm, 5mm, 6mm, 7mm, 8mm, 9mm, 10mm, etc. The outer diameter d2 of the polymer tube is 0.1mm-25mm. Exemplarily, it can be 0.1mm, 0.2mm, 0.3mm, 0.6mm, 1mm, 5mm, 10mm, 15mm, 20mm, 25mm, etc. The wall thickness d3 of the polymer tube is 0.045mm-12.45mm. Exemplarily, it can be 0.045mm, 0.1mm, 0.3mm, 0.6mm, 1mm, 2mm, 5mm, 7.5mm, 10mm, 12.45mm, etc. By controlling the diameters of the lithium metal wire and the polymer outer tube, the mass percentage of lithium metal wire in the lithium replenishing agent can be accurately calculated, thereby achieving precise and flexible control of the lithium replenishment amount on the negative electrode. Furthermore, controlling the diameter of the lithium replenishing agent within a certain range helps improve its dispersibility and the degree of fibrillation of the polymer tube.

[0007] In some embodiments of this application, the diameters of the lithium metal wire and the polymer tube satisfy d1 ≤ d2 - 2d3. If the lithium metal wire needs to be housed within the polymer tube, its diameter must satisfy the above quantitative relationship.

[0008] In some embodiments of this application, the relationship between the length L of the lithium replenishing agent and the outer diameter of the polymer tube satisfies L≥10d². During high-speed shearing, lithium replenishing agents with a suitable aspect ratio are more easily sheared and dispersed uniformly.

[0009] In some embodiments of this application, the lithium metal wire is made of elemental lithium or a lithium alloy. The lithium alloy contains at least one alloying element selected from Mg, B, Al, Sn, Ge, Si, Pb, Ag, In, Zn, Ga, Na, and P.

[0010] In some embodiments of this application, the lithium metal accounts for 0.1-96% of the mass percentage of the lithium replenishing agent. Preferably, the lithium metal accounts for 2-95% of the mass percentage of the lithium replenishing agent. Exemplarily, the mass percentage of the lithium metal can be 2%, 3%, 5%, 6.5%, 6.9%, 7.5%, 10%, 15%, 20%, 30%, 40%, 45%, 50%, 60%, 70%, 80%, 90%, 92%, 95%, etc. An appropriate lithium metal percentage can ensure the mass percentage of the binder (i.e., polymer tube) in the lithium replenishing agent, and an appropriate amount of binder is beneficial for maintaining the structural strength of the obtained negative electrode active material film.

[0011] In some embodiments of this application, a conductive layer, comprising a carbon layer, is coated on the outer wall of the polymer tube. The thickness of the conductive layer is 0.0002 mm to 0.5 mm. Exemplarily, the thickness of the conductive layer can be 0.0002 mm, 0.002 mm, 0.01 mm, 0.05 mm, 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, or 0.5 mm. The material of the conductive layer includes, but is not limited to, at least one of acetylene black, carbon nanotubes, carbon fibers, and carbon black. The conductive layer coating the outer wall of the polymer tube acts as a conductive agent for the negative electrode, effectively solving the problem of poor dispersion of conductive agents directly added to the negative electrode active material. Furthermore, an appropriate amount of conductive agent is beneficial to the performance of the battery.

[0012] In some embodiments of this application, conductive particles are attached to the polymer tube. These conductive particles can be attached to the outer wall of the polymer tube. The conductive particles can be those commonly used in lithium-ion battery electrodes, including but not limited to at least one of acetylene black, carbon nanotube aggregates, chopped carbon fibers, and carbon black particles. In some embodiments, the conductive particles can also be carbonized particles of the polymer tube (e.g., amorphous carbon particles after carbonization of polyvinyl fluoride). In this case, the lithium replenishing agent is a partially carbonized polymer tube and lithium metal wires disposed within the carbonized or partially carbonized polymer tube. In this case, the conductive particles are dispersed on the outer wall, inner wall, or embedded within the polymer tube. In these cases, there is no need to introduce additional conductive materials, and the carbonized particles partially replace the original polymer, thereby increasing the mass percentage of lithium metal in the lithium replenishing agent.

[0013] In some embodiments of this application, the polymer tube is made of at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene oxide (PEO), and styrene-butadiene rubber (SBR). These materials exhibit good adhesion to the negative electrode active material and lithium metal wire, and their high degree of fibrillability is beneficial for maintaining the structural stability of the negative electrode active material membrane.

[0014] In this application, the lithium replenishing agent can be prepared by coaxial spinning or by injecting molten lithium metal into a commercially available polymer tube. In some embodiments, coaxial spinning is used to prepare the lithium replenishing agent: the spinning equipment includes two coaxial material chambers (inner and outer) and two coaxial nozzles (inner and outer), wherein the inner material chamber contains molten lithium metal, the outer material chamber contains molten polymer, and the inner diameter of the outer nozzle is larger than the outer diameter of the inner nozzle. When the materials in the inner and outer material chambers are ejected at the same linear velocity, and after rapid cooling, shaping, and winding, a continuous lithium replenishing agent can be obtained. In the above process, the diameter of the lithium replenishing agent can be controlled by adjusting the linear velocity of the ejected material, the linear velocity of the winding roller, and the diameter of the nozzle. The product can also be slit according to actual production needs to obtain the lithium replenishing agent provided in this application.

[0015] In other embodiments, in a glove box, a commercially available polymer tube that meets the size requirements defined in this application is immersed in molten lithium metal and kept at a high temperature in a vacuum furnace for a period of time. After being removed and cooled, and after the lithium metal has solidified and formed, the residual lithium metal on the outer wall of the polymer tube is removed to obtain the lithium replenishing agent provided in this application.

[0016] A second aspect of this application provides a method for preparing a negative electrode sheet, comprising the following steps:

[0017] (1) Under the protection of inert gas, the mixture of lithium replenishing agent and negative electrode active material provided in the first aspect of this application is subjected to high-speed shearing to make the polymer tube fibrillated and to make the lithium metal wires come out of the polymer tube and be sheared to obtain an intermediate.

[0018] (2) The intermediate is subjected to calendering to obtain a negative electrode active material film;

[0019] (3) The negative electrode active material film and the negative electrode current collector are subjected to hot pressing treatment to obtain the negative electrode sheet.

[0020] In step (1), under the protection of an inert gas, the negative electrode active material and the lithium replenishing agent are mixed in a mechanical stirring device. After being mixed evenly, the mixture is transferred to a mechanical device that can provide high-speed shearing for further processing. Under the action of high-speed shearing force, the lithium replenishing agent is sheared into smaller particles and dispersed, while the polymer tubes are elongated and fibrillated. Lithium metal can be extracted from the broken polymer tubes and fully mixed with the negative electrode active material. The fibrillated polymers intertwine and overlap until they are interwoven into a polymer fiber network matrix with a certain three-dimensional structure, and the lithium metal particles and negative electrode active material are distributed in the polymer fiber network matrix to form an intermediate.

[0021] Following the calendering process in step (2), the aforementioned intermediate is formed into a negative electrode active material film. During the calendering process, the polymer network with a certain three-dimensional structure is calendered into a polymer fiber network matrix with a certain thickness, while lithium metal particles can be loaded onto the polymer fiber network matrix together with the negative electrode active material, or fill the mesh of the polymer fiber network matrix to form a negative electrode active material film with a certain structural strength. Finally, through the hot pressing process in step (3), the negative electrode active material film is combined with the negative electrode current collector to obtain the negative electrode sheet.

[0022] In the above process, the parameterized lithium replenishing agent undergoes a series of physical changes, evolving into a polymer fiber network matrix loaded with the negative electrode active material and lithium metal particles uniformly dispersed in the negative electrode active material. Specifically, in actual production, the lithium metal content in the prepared negative electrode sheet can be precisely controlled by selecting lithium replenishing agents of different sizes and with different lithium metal mass ratios. Furthermore, the morphology of the polymer fiber network and lithium metal in the negative electrode active material film can be controlled by adjusting the shear rate in step (1), thereby achieving control over the strength of the negative electrode active material film. The above preparation process is highly controllable, simple in steps, and highly efficient, enabling large-scale industrial production.

[0023] In some embodiments of this application, the high-speed shearing employs a shearing rate of 20 m / s to 1000 m / s. This shearing rate is more precisely the shearing linear velocity. Exemplarily, the shearing rate can be 20 m / s, 50 m / s, 100 m / s, 200 m / s, 300 m / s, 400 m / s, 500 m / s, 600 m / s, 700 m / s, 800 m / s, 900 m / s, 1000 m / s, etc.

[0024] In some embodiments of this application, the high-speed shearing process can be carried out in equipment such as jet mills, hammer mills, and high-speed shear mixers. In some embodiments, a jet mill is used for high-speed shearing to disperse the lithium supplement in the negative electrode active material. This jet mill, in addition to having ordinary mechanical shear blades, also has at least one nozzle capable of ejecting a high-speed airflow. Ordinary mechanical shear blades can reduce the size of the lithium supplement to form small particles, while the high-speed airflow ejected from the nozzle of the jet mill can accelerate the collision of these small particles, causing the polymer to elongate and fibrillate. The elongated polymers intertwine and overlap until they interweave to form a thin, fibrillated network matrix, distributing the lithium metal particles and the negative electrode active material within this fibrillated network matrix.

[0025] In some embodiments of this application, when the lithium replenishing agent does not contain a conductive layer or conductive particles (i.e., the outer wall of the polymer tube is not covered by a conductive layer or has no conductive particles attached), a conductive agent needs to be added in step (1).

[0026] The third aspect of this application provides a negative electrode sheet, which is prepared by the preparation method provided in the second aspect of this application.

[0027] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material film disposed on the negative electrode current collector. The negative electrode active material film includes a polymer fiber network matrix, lithium metal particles loaded on the polymer fiber network matrix, and the negative electrode active material. The lithium metal particles and the negative electrode active material are bonded to the polymer fiber network matrix, and the polymer fiber network matrix imparts a certain structural strength to the negative electrode active material film, thereby giving the negative electrode sheet a stable structure. In addition, the lithium metal particles in the negative electrode sheet, which are non-agglomerated and uniformly dispersed in the negative electrode active material, serve as a lithium replenishment source, which can stably replenish the irreversible capacity loss during the first charge and discharge process of the battery, thereby improving the battery's discharge capacity and initial coulombic efficiency, and extending the battery's service life.

[0028] In this embodiment, the negative electrode active material is a conventional active material in the art. Exemplarily, the negative electrode active material includes at least one of graphite, hard carbon, soft carbon, silicon, silicon suboxide, and silicon-carbon composite materials.

[0029] This application provides a battery having the negative electrode provided in the third aspect of this application. The battery exhibits high discharge capacity, high initial coulombic efficiency, and long cycle life.

[0030] In this embodiment, the aforementioned negative electrode sheet, along with a conventional separator and positive electrode sheet, are stacked sequentially and wound to prepare a soft-pack battery. The positive electrode sheet includes a positive current collector and a positive active material, which is a conventional positive active material in the art. Exemplarily, the positive active material includes at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, nickel-cobalt-aluminum ternary materials (NCA) and nickel-cobalt-manganese ternary materials (NMC), lithium manganese phosphate, lithium manganese iron phosphate, lithium iron silicate, and lithium manganese silicate. Detailed Implementation

[0031] The embodiments of this application will be further described below through multiple examples.

[0032] Example 1

[0033] (1) Preparation of lithium supplement

[0034] A commercially available PTFE capillary with an outer diameter d2 of 0.6 mm, a wall thickness d3 of 0.15 mm, and a length L of 65 mm was immersed in molten lithium metal in a glove box under argon atmosphere. The capillary was then held at 190°C in a high-temperature vacuum furnace for 30 minutes until it was fully filled with lithium metal. After cooling, the capillary was removed, and any remaining lithium metal was cleaned from its surface to obtain the lithium replenishing agent provided in this application. The lithium metal content in this replenishing agent is 7.5% by mass.

[0035] (2) Preparation of negative electrode sheet

[0036] 945g of graphite, 5g of carbon fiber conductive agent HV (0.5%), and 50g of the prepared lithium supplement agent were weighed and mixed in a mechanical mixer under an inert atmosphere for 5 hours at a speed of 2000 rpm / min. The mixture was then subjected to high-speed shearing in a J-50 type jet mill, with an inlet pressure of 1.2 MPa, a feeding pressure of 0.6 MPa, and a shear rate of 100 m / s. The treated mixture was then extruded at 60°C to obtain a 250 μm thick intermediate. This anode intermediate was further calendered to obtain a 60 μm thick anode active material film. This anode active material film was then hot-pressed together with carbon-coated copper foil at 80°C to obtain the anode electrode sheet provided in this application.

[0037] (3) Preparation of positive electrode sheet

[0038] 960g of positive electrode active material - lithium iron phosphate (96%), 30g of binder PVDF (3%), 5g of acetylene black (0.5%), and 5g of conductive agent HV (0.5%) were added to 2000g of solvent N-methylpyrrolidone (NMP) and stirred in a vacuum mixer to form a stable and uniform positive electrode slurry.

[0039] A slot coating device is used to uniformly and intermittently coat the positive electrode slurry onto the surface of aluminum foil (aluminum foil dimensions: width 160mm, thickness 12μm); then it is dried at 20℃, and after being pressed by a roller press, a positive electrode sheet is obtained. The positive electrode sheet is cut into rectangular positive electrode sheets with dimensions of 48mm x 56mm, and tabs are spot-welded at the width direction.

[0040] (4) Battery manufacturing

[0041] The negative electrode obtained in step (2) and the positive electrode obtained in step (3) are alternately stacked together with a separator to prepare a battery. The positive and negative electrodes are alternately separated by the separator to obtain a dry cell. The dry cell is placed in an aluminum-plastic film outer packaging, electrolyte is injected, and then it is vacuum sealed. After being placed at 60°C for 48 hours, it is pressurized at 60°C, re-encapsulated, vented, and capacity tested to obtain the lithium battery of this embodiment. This battery is denoted as S1.

[0042] Example 2

[0043] The difference from Example 1 is that a PTFE capillary tube with an outer diameter d2 of 25 mm, a wall thickness d3 of 12.45 mm, and a length of 250 mm was used to prepare the lithium replenishing agent. The lithium metal content in the prepared lithium replenishing agent was 3% by mass. The resulting battery is designated as S2.

[0044] Example 3

[0045] The difference from Example 1 is that in step (1), the lithium replenishing agent is prepared by coaxial spinning. Specifically, the inner material chamber of the coaxial spinning equipment contains molten lithium metal, and the outer material chamber contains molten PTFE, with the inner diameter of the outer nozzle being larger than the outer diameter of the inner nozzle. The materials in both the inner and outer material chambers are ejected at the same linear velocity, and after rapid cooling, molding, winding, and slitting, a lithium replenishing agent with an outer diameter d2 of 1 mm, a wall thickness d3 of 0.045 mm, and a length L of 85 mm is obtained. The lithium metal mass percentage in the prepared lithium replenishing agent is 92%. The resulting battery is designated as S3.

[0046] Example 4

[0047] The difference from Example 1 is that in step (1), a commercially available PTFE capillary tube with an outer diameter d2 of 0.6 mm, a wall thickness d3 of 0.15 mm, and a length L of 3.6 mm is used to prepare the lithium replenishing agent. The lithium metal mass percentage in the prepared lithium replenishing agent is 6.8%. The resulting battery is designated as S4.

[0048] Example 5

[0049] The difference from Example 1 is that in step (1), a carbon layer with a thickness of 0.01 mm is also coated on the outer wall of the PTFE tube; in step (2), no conductive agent is added when preparing the negative electrode sheet. The lithium metal mass percentage in the prepared lithium replenishing agent is 6.5%. The prepared battery is designated as S5.

[0050] Example 6

[0051] The difference from Example 1 is that in step (1), the PTFE tube used is a partially carbonized PTFE tube. The lithium metal mass percentage in the prepared lithium replenishment agent is 6.9%. The prepared battery is designated as S6.

[0052] Example 7

[0053] The difference from Example 1 is that in step (2), the negative electrode active material is 950g of silicon-carbon negative electrode material. The resulting battery is designated as S7.

[0054] Example 8

[0055] The difference from Example 1 is that in step (1), lithium metal is replaced with a Li-Mg alloy, the Mg content of which is 5%, and the mixture is vacuum-held at 205°C for 30 minutes in a high-temperature vacuum furnace. The resulting battery is designated S8. Specifically, a commercially available PTFE capillary with an outer diameter d2 of 0.6 mm, a wall thickness d3 of 0.15 mm, and a length L of 65 mm is immersed in molten Li-Mg alloy in a glove box protected by an argon atmosphere. After being vacuum-held at 205°C for 30 minutes in a high-temperature vacuum furnace, the PTFE capillary is fully filled with Li-Mg alloy. It is then removed, cooled, and the residual Li-Mg alloy on the surface is cleaned to obtain the lithium replenishing agent provided in this application. The lithium metal content in this lithium replenishing agent is 7.5% by mass.

[0056] To highlight the beneficial effects of the embodiments of this application, the following comparative examples 1-2 are provided.

[0057] Comparative Example 1

[0058] (1) Preparation of negative electrode sheet

[0059] 1000g of graphite anode active material was added to 2000g of water, followed by 60g of styrene-butadiene latex solution and 20g of sodium carboxymethyl cellulose. The mixture was vigorously stirred to obtain a uniform and stable anode slurry. The anode slurry was then uniformly and intermittently coated onto the surface of a copper foil (copper foil dimensions: width 160mm, thickness 8μm) using a slot coating machine. The foil was then dried at 120℃ and pressed into a negative electrode sheet using a roller press. This negative electrode sheet was cut into rectangular sheets with dimensions of 49mm x 57mm, and tabs were spot-welded along the width direction. This yielded the negative electrode sheet of Comparative Example 1.

[0060] (2) Preparation of positive electrode sheet

[0061] 960g of positive electrode active material - lithium iron phosphate (96%), 30g of binder PVDF (3%), 5g of acetylene black (0.5%), and 5g of conductive agent HV (0.5%) were added to 2000g of solvent NMP (nitromethylpyrrolidone) and then stirred in a vacuum mixer to form a stable and uniform positive electrode slurry.

[0062] A slot coating machine is used to uniformly and intermittently coat the positive electrode slurry onto both sides of an aluminum foil (160 mm wide and 16 μm thick). The foil is then dried at 120°C and pressed into a sheet using a roller press to obtain the positive electrode sheet. The positive electrode sheet is then cut into rectangular sheets with dimensions of 48 mm x 56 mm, and tabs are spot-welded to the width direction.

[0063] (3) Battery manufacturing

[0064] The negative electrode obtained in step (1) and the positive electrode obtained in step (2) are alternately stacked with a separator to prepare a battery. The positive and negative electrodes are arranged alternately, and adjacent positive and negative electrodes are separated by a separator, resulting in a dry cell. The dry cell is placed in an aluminum-plastic film outer packaging, electrolyte is injected, and then it is vacuum-sealed. After being placed at 60°C for 48 hours, a pressure layer is applied at 60°C, followed by secondary encapsulation, venting, and capacity testing to obtain a comparative lithium battery. The resulting battery is designated DS1.

[0065] Comparative Example 2

[0066] (1) Weigh 945g of graphite, 5g of carbon fiber conductive agent HV (0.5%), 46g of PTFE powder and 4g of lithium powder with a median particle size of 12μm, and mix them in a mechanical stirrer under an inert atmosphere for 5h at a speed of 2000rpm / min; then stir the mixture evenly and extrude it at 60℃ to obtain a negative electrode material body with a thickness of 250μm. Then, further calender the negative electrode material body to obtain a negative electrode active material film with a thickness of 60μm. The negative electrode active material film is hot-pressed together with carbon-coated copper foil at 80℃ to obtain the negative electrode sheet of Comparative Example 2.

[0067] (2) Preparation of positive electrode sheet

[0068] 960g of positive electrode active material - lithium iron phosphate (96%), 30g of binder PVDF (3%), 5g of acetylene black (0.5%), and 5g of conductive agent HV (0.5%) were added to 2000g of NMP and stirred in a vacuum mixer to form a stable and uniform positive electrode slurry.

[0069] A slot coating device is used to uniformly and intermittently coat the positive electrode slurry onto the surface of aluminum foil (aluminum foil dimensions: width 160mm, thickness 12μm); then it is dried at 20℃, and after being pressed by a roller press, a positive electrode sheet is obtained. The positive electrode sheet is cut into rectangular positive electrode sheets with dimensions of 48mm x 56mm, and tabs are spot-welded at the width direction.

[0070] (3) Battery manufacturing

[0071] The negative electrode obtained in step (2) and the positive electrode obtained in step (3) are alternately stacked together with a separator to prepare a battery. The positive and negative electrodes are alternately separated by the separator to obtain a dry cell. The dry cell is placed in an aluminum-plastic film outer packaging, electrolyte is injected, and then it is vacuum sealed. After being placed at 60°C for 48 hours, a pressure layer is applied at 60°C, followed by secondary encapsulation, venting, and capacity testing to obtain the lithium battery of this embodiment. This battery is designated as DS2.

[0072] After the batteries obtained in Examples 1-8 and Comparative Examples 1-2 were formed, charge-discharge cycle tests were performed. Using a LAND CT 2001C secondary battery performance testing device at 25±1℃, the batteries were subjected to a 0.2C charge-discharge cycle test. The steps were as follows: rest for 10 minutes; constant current charging at 0.2C to 4.2V, constant voltage charging to 0.05C cutoff; rest for 10 minutes; constant current discharge to 3.0V, which constitutes one cycle. This process was repeated. During the cycle, the cycle was terminated when the battery capacity fell below 80% of the initial discharge capacity. The number of cycles is the cycle life of the battery. Five batteries were selected for testing for each example and comparative example. The average value of the five batteries was taken for each test group. The test results for each battery are summarized in Table 1.

[0073] Table 1 summarizes the performance test results of the batteries prepared in each embodiment and comparative example.

[0074]

[0075] Based on the specific lithium metal content in the lithium replenishing agents prepared in the examples and the data in Table 1, it can be seen that the lithium metal content in the negative electrode of batteries 1, 5, 6, and 8 is similar to that of battery DS2 in Comparative Example 2 (the lithium metal content in the negative electrode sheet is about 4g), and the negative electrode active materials used are the same. However, the initial discharge specific capacity, initial coulombic efficiency, and cycle number of batteries S1, S5, S6, and S8 are significantly higher than those of battery DS2. This indicates that the lithium replenishing agent (including lithium metal, conductive agent, and binder) provided in this application can be uniformly dispersed in the negative electrode sheet, giving full play to their lithium replenishment effect, thereby greatly improving battery performance. In Examples 2, 3, and 4, the outer diameter, wall thickness, and length of the polymer tube in the lithium replenishing agent were adjusted respectively, and the lithium metal content in the resulting lithium replenishing agent was significantly different from that in Comparative Example 2, but the electrochemical performance was still slightly stronger than that of battery DS2. Among them, the electrochemical performance of batteries S2 and S4 was relatively weak. This is because the lithium metal content of the negative electrode in Example 2 was only 3%, and the length L of the lithium replenishing agent prepared in Example 4 was only 6 times the outer diameter d2 of its polymer tube (not meeting the requirement of L≥10d2 as specified in this application). In addition, battery S7 used silicon-carbon negative electrode material. Due to the difference in material properties from graphite, the electrochemical performance of battery S7 was slightly different from that of the batteries in other examples. Comparative Example 1 did not perform any lithium replenishment treatment on the electrode sheets, and the discharge capacity, initial coulombic efficiency, and cycle number of the battery DS1 prepared from it were significantly weaker than those of the example batteries S1-S8.

[0076] The above results demonstrate that by using the lithium replenishing agent provided in this application to replenish the lithium on the electrode sheet, the battery with the electrode sheet exhibits higher initial coulombic efficiency and longer cycle life.

[0077] The above description is an exemplary embodiment of this application. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principles of this application, and these improvements and modifications are also considered to be within the scope of protection of this application.

Claims

1. A lithium supplement, characterized in that, The lithium replenishing agent comprises a polymer tube and a lithium metal wire contained within the polymer tube; wherein the diameter d1 of the lithium metal wire is 0.005mm-10mm; the outer diameter d2 of the polymer tube is 0.1mm-25mm; and the wall thickness d3 of the polymer tube is 0.045mm-12.45mm.

2. The lithium supplement agent according to claim 1, characterized in that, The diameters of the lithium metal wire and the polymer tube satisfy: d1≤d2-2d3.

3. The lithium supplement agent according to claim 1 or 2, characterized in that, The length L of the lithium replenishing agent and the outer diameter d2 of the polymer tube satisfy the following condition: L≥10d2.

4. The lithium supplement agent according to claim 1, characterized in that, The lithium metal wire includes at least one of elemental lithium and lithium alloy.

5. The lithium supplement agent according to claim 4, characterized in that, The alloying elements in the lithium alloy include at least one of the elements selected from Mg, B, Al, Sn, Ge, Si, Pb, Ag, In, Zn, Ga, Na, and P.

6. The lithium supplement agent according to claim 1, characterized in that, The lithium metal wire has a mass percentage of 0.1-96% in the lithium replenishing agent.

7. The lithium supplement agent according to claim 6, characterized in that, The lithium metal wire has a mass percentage of 2-95% in the lithium replenishing agent.

8. The lithium supplement agent according to claim 1, characterized in that, The outer wall of the polymer tube is coated with a conductive layer, which includes a carbon layer; the thickness of the conductive layer is 0.0002mm-0.5mm.

9. The lithium supplement agent according to claim 1, characterized in that, The polymer tube is coated with conductive particles, which include carbonized particles of the polymer tube.

10. The lithium supplement agent according to claim 1, characterized in that, The polymer tube is made of at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyethylene oxide, and styrene-butadiene rubber.

11. A method for preparing a negative electrode sheet, characterized in that, Includes the following steps: (1) Under inert gas protection, the mixture of lithium replenishing agent and negative electrode active material as described in any one of claims 1-10 is subjected to high-speed shearing to fibrillate the polymer tube and to remove the lithium metal wire from the polymer tube and cut it to obtain an intermediate; (2) The intermediate is calendered to obtain a negative electrode active material film; (3) The negative electrode active material film and the negative electrode current collector are subjected to hot pressing treatment to obtain the negative electrode sheet.

12. A negative electrode sheet, characterized in that, The negative electrode sheet is prepared according to the preparation method described in claim 11.

13. The negative electrode sheet according to claim 12, characterized in that, The negative electrode sheet includes a negative electrode current collector and a negative electrode active material film disposed on the negative electrode current collector. The negative electrode active material film includes a polymer fiber network matrix, lithium metal particles loaded on the polymer fiber network matrix, and the negative electrode active material.

14. A battery, characterized in that, The battery has a negative electrode as described in any one of claims 12-13.

Citation Information

Patent Citations

  • Lithium supplementing method for improving initial coulombic efficiency and cycle performance of lithium ion battery

    CN111509288A

  • Pole piece film and preparation method and application thereof

    CN112038574A