A method for recycling valuable metals from waste lithium-ion batteries and regenerating ternary positive electrode materials

Through sodium alginate cross-linking and sol-gel method combined with mechanical grinding technology, the complexity and high cost of recycling lithium-ion battery cathode materials have been solved, and efficient and environmentally friendly ternary cathode material regeneration and recycling have been achieved, improving the Electrochemical properties.

CN116425213BActive Publication Date: 2024-10-08JIANGSU E ONTECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310293006.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-05-08
Filing Date
2020-09-22
Publication Date
2024-10-08
Estimated Expiration
2040-09-22

AI Technical Summary

Technical Problem

Existing lithium-ion battery recycling technology is difficult to effectively classify and recycle different types of cathode materials, and the process is complex or costly, resulting in resource waste and environmental pollution.

Method used

The sodium alginate cross-linked metal ion combined sol-gel method is used to mechanically grind the nanometer ternary cathode material, assemble the precursor on its surface, and sinter it at high temperature to prepare the regenerated ternary cathode material, thereby realizing the recycling of valuable metals.

Benefits of technology

Efficient and environmentally friendly ternary cathode material recycling is achieved, reducing process complexity and cost, and improving the electrochemical cycle performance and resource utilization of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116425213B_ABST
    Figure CN116425213B_ABST
Patent Text Reader

Abstract

The present invention provides a method for recovering valuable metals of waste lithium ion batteries and regenerating ternary positive electrode materials, comprising the following steps: discharging, disassembling and removing impurities from waste lithium ion batteries to obtain positive electrode sheets, removing conductive agents and binders in positive electrode sheets at high temperature to obtain waste ternary positive electrode materials; regeneration route one can respectively leach valuable metal ions from organic acids or low eutectic solvents with added reducing agents, crosslink metal ions with sodium alginate solution to form a gel with an "egg-box structure" having a three-dimensional mesh structure, and obtain regenerated ternary positive electrode materials after calcination, and regeneration route two facilitates lithium ions to enter the interior of particles for lithium supplementation through ball milling nano-processing, gel repairs uneven surfaces, and obtains regenerated ternary positive electrode materials after calcination. The two regeneration routes are simple and easy to operate, avoid steps such as separation and purification of valuable metal ions, are novel in method, low in cost, easy to industrialize, and the prepared materials have excellent electrochemical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for recovering valuable metals of waste lithium ion batteries and regenerating ternary positive electrode materials, belonging to the technical field of recovery and regeneration of waste lithium ion batteries. Background Art

[0002] In lithium-ion batteries, especially in the cost structure of automotive power batteries, material costs account for nearly 75%. Among the material costs, positive electrode materials account for 41%. The market size of NCM ternary positive electrode materials in my country has shown rapid growth. In 2018, the market size of NCM ternary positive electrode materials in my country reached 23 billion yuan, a year-on-year increase of 33.72%. The market size of NCM ternary positive electrode materials in my country has shown rapid growth, mainly benefiting from the rapid development of domestic automotive power batteries, low cobaltization of 3C batteries, power tools, electric bicycles and other application markets, which has driven the continuous growth of market demand for NCM ternary positive electrode materials. It is estimated that the market size of NCM ternary positive electrode materials in China will exceed 60 billion yuan in 2022. However, what followed was an explosive growth in waste ternary lithium-ion batteries. Therefore, recycling ternary lithium-ion battery electrode materials has become a new focus of attention in the battery industry. When recycling waste lithium-ion batteries, it is currently difficult to classify different types of positive electrode materials. The waste positive electrodes obtained after disassembly and sorting often contain multiple positive electrode materials, and the leaching solution will contain valuable metals such as nickel, cobalt, manganese and lithium. Nickel, cobalt and manganese have accounted for 90% of the cost of positive electrode materials. These metals are difficult to mine. my country has few resource reserves. 95% of cobalt resources rely on imports, and 70% of lithium ore is imported. Green and efficient recycling of valuable metals in waste lithium-ion batteries will not only bring considerable economic and social benefits, but also effectively alleviate the shortage of resources such as cobalt and lithium in my country.

[0003] At present, the recycling of waste lithium-ion battery materials is mainly divided into two categories: pyrometallurgy and hydrometallurgy. Pyrometallurgy is a method of directly using high-temperature treatment to extract metals or metal oxides from electrodes. The process is simple, but the purity of the recycled materials is low and the high-temperature treatment time is long and the energy consumption is high. The electrolyte, adhesive and other organic matter in the waste batteries will produce harmful gases due to high-temperature reactions, and supporting facilities need to be installed for secondary waste gas treatment. Hydrometallurgy is to first disassemble the battery shell, crush and screen to obtain the electrode material, and then leaching the valuable metals in the electrode material in acid or biological solution, and then precipitate or extract to obtain the corresponding salts or oxides of each metal. Although it can effectively recover different valuable metals, the process is relatively complicated and requires the use of a large amount of chemical reagents, which is costly and easy to cause environmental pollution. Summary of the invention

[0004] The present invention proposes a method for recycling valuable metals of waste lithium-ion batteries and regenerating ternary positive electrode materials. The method can be composed of two routes: one is to organically combine the recovery of valuable metals of waste lithium-ion batteries with the preparation of ternary positive electrode materials, and use sodium alginate to crosslink metal ions directly into the production link of new electrode materials to achieve the recycling of valuable metal materials. The second is to nano-size the waste nickel-cobalt-manganese-oxide lithium ternary positive electrode materials by mechanical grinding, and then use the nano-sized waste ternary positive electrode materials as the core to assemble the ternary positive electrode material precursor on its surface by sol-gel method, and then sinter the above materials at high temperature to obtain the repaired and regenerated ternary positive electrode materials. Nano-size the waste ternary positive electrode materials by mechanical grinding so that lithium ions can easily enter the particles to replenish lithium, but mechanical grinding will cause the surface of the particles to be uneven, resulting in an increase in the specific surface area and consumption of lithium ions. Assembling the ternary positive electrode materials on the surface of nanoparticles can eliminate the above adverse effects.

[0005] The specific technical solution is:

[0006] A method for recycling waste lithium-ion batteries to regenerate ternary positive electrode materials comprises the following steps:

[0007] S11, pre-treating the waste lithium-ion battery and removing the conductive agent and binder in the positive electrode sheet under high temperature conditions;

[0008] Then proceed according to any of the following two process routes:

[0009] First route:

[0010] S12, adding the battery material obtained in step S11 to the first extracting solution or the second extracting solution to leach the transition metal ions; the first extracting solution is an organic acid with a reducing agent added, and the second extracting solution is a low eutectic solvent;

[0011] S13, adding a sodium alginate solution to the leaching solution obtained in step S12, performing a cross-linking reaction with transition metal ions to obtain a gel, and calcining the gel to obtain a regenerated ternary positive electrode material;

[0012] Second route:

[0013] S22, ball milling the positive electrode material obtained in step S11;

[0014] S23, adding a soluble lithium source, a nickel source, a cobalt source and a manganese source to the solution containing the ball-milled nanoparticles obtained in step S22, and repairing and assembling a ternary cathode material precursor on the surface of the nanoparticles by a sol-gel method using the nanoparticles as cores;

[0015] S24, calcining the above materials to obtain positive electrode materials.

[0016] In one embodiment, the transition metal ion is a nickel ion, a cobalt ion or a manganese ion.

[0017] In one embodiment, the used lithium-ion battery is a mixture of one or more of lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium nickel manganese oxide, or nickel-cobalt-manganese ternary batteries.

[0018] In one embodiment, in step S11, the pre-processing refers to one or more steps of battery discharging, disassembling or impurity removal.

[0019] In one embodiment, in step S11, the high temperature condition refers to a treatment temperature of 500-1000° C., a treatment time of 0.5-5 h, and a treatment atmosphere of air or oxygen.

[0020] In one embodiment, in the first extract, the added reducing agent is selected from a mixture of one or more of sodium thiosulfate, hydrogen peroxide, glucose, anthraquinone, hydrazine hydrate, sodium borohydride, and thiourea dioxide; the organic acid is selected from a mixture of one or more of aminosulfonic acid, ascorbic acid, maleic acid, acetic acid, oxalic acid, gluconic acid, and tartaric acid.

[0021] In one embodiment, in the second extract, the low eutectic solvent is composed of a hydrogen bond donor and a hydrogen bond acceptor, and the hydrogen bond donor is generally selected from a mixture of one or more of choline chloride, methyltriphenylphosphonium bromide, benzyltriphenylphosphonium bromide, choline bromide, and betaine; the hydrogen bond acceptor is generally selected from a mixture of one or more of urea, ethylene glycol, glycerol, amino acids, acetamide, and lactic acid.

[0022] In one embodiment, in step S12, after obtaining the leaching solution, transition metal ions and / or lithium ions are added to the leaching solution according to a set ion concentration ratio; so that the molar ratio of lithium: nickel: cobalt: manganese in the leaching solution after addition is one of 3:1:1:1, 1:0.5:0.2:0.3, 1:0.6:0.2:0.2, and 1:0.8:0.1:0.1.

[0023] In one embodiment, in step S12, in the step of adding corresponding metal ions, the lithium source is selected from one or more mixtures of lithium carbonate, lithium nitrate, lithium acetate and lithium hydroxide; the nickel source is selected from one or more mixtures of nickel carbonate, nickel nitrate, nickel acetate and nickel hydroxide; the cobalt source is selected from one or more mixtures of cobalt carbonate, cobalt nitrate, cobalt acetate and cobalt hydroxide; the manganese source is selected from one or more mixtures of manganese carbonate, manganese nitrate, cobalt acetate and manganese hydroxide.

[0024] In one embodiment, in step S13, the concentration of the sodium alginate solution is 0.1-5%, the viscosity is 5000-100000 cP at 25°C, the amount of the sodium alginate solution is 2.0-2.4 times the total molar amount of nickel, cobalt and manganese metal ions, and the crosslinking time is controlled at 0.5-6 hours.

[0025] In one embodiment, in step S13, the calcination temperature is 500-1000° C., the calcination time is 1-20 hours, and the calcination atmosphere is air or oxygen.

[0026] In one embodiment, in step S22, the ball milling process is to mix the positive electrode material, water and dispersant, the added dispersant is 1-5% of the mass of the positive electrode material, and the solid content of the positive electrode material is 10-30%; the mass ratio of the grinding balls added in the ball milling process to the ternary positive electrode material is 2-5:1, the ball milling process speed is 1500-2500r / min, and the grinding time is 2-40h.

[0027] In one embodiment, the ball milling process uses any one of a high-speed stirred mill, a ball mill, a tube mill, a cone mill, a rod mill and a sand mill.

[0028] In one embodiment, the dispersant is selected from one or more combinations of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, triethylhexyl phosphoric acid, sodium dodecyl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, polyethylene glycol fatty acid esters, hexadecyltrimethylammonium bromide, polyethylene glycol p-isooctylphenyl ether, polyacrylic acid, polyvinyl pyrrolidone, polyoxyethylene sorbitan monooleate, p-ethylbenzoic acid and polyetherimide.

[0029] In one embodiment, the ball milling process reduces the particle size of the cathode material to 50-300 nm.

[0030] In one embodiment, in step S23, the soluble lithium source, nickel source, cobalt source and manganese source, wherein the lithium source is selected from one or more mixtures of lithium carbonate, lithium nitrate, lithium acetate and lithium hydroxide; the nickel source is selected from one or more mixtures of nickel carbonate, nickel nitrate, nickel acetate and nickel hydroxide; the cobalt source is selected from one or more mixtures of cobalt carbonate, cobalt nitrate, cobalt acetate and cobalt hydroxide; the manganese source is selected from one or more mixtures of manganese carbonate, manganese nitrate, cobalt acetate and manganese hydroxide.

[0031] In one embodiment, in step S23, the ratio of the molar amount of lithium ions to the total molar amount of nickel, cobalt and manganese ions is 1.05-1.1:1, and the molar ratio of nickel, cobalt and manganese ions is one of 1:1:1, 5:2:3, 6:2:2 or 8:1:1.

[0032] In one embodiment, in step S23, the ratio of the molar amount of citric acid added to the total molar number of the three metal ions of nickel, cobalt and manganese is 1-2:1, and the pH of the solution is adjusted to 7-8 with ammonia water.

[0033] In one embodiment, in step S24, the high temperature sintering temperature is 700-1000° C., the sintering time is 5-20 hours, and the sintering atmosphere is air or oxygen.

[0034] Beneficial Effects

[0035] The above technical solution provided by the present invention has the following advantages:

[0036] (1) The present invention uses organic acid or deep eutectic solvent to leach metal ions, which is green and environmentally friendly and has a high metal ion leaching rate;

[0037] (2) A sodium alginate solution with a certain viscosity is used to crosslink transition metal ions to form a gel with a three-dimensional network structure of an "egg-box structure", and then directly calcined at high temperature to prepare a ternary cathode material. This preparation method is novel and simple in process. It does not require the addition of an alkaline solution to adjust the pH of the solution to obtain a precipitate. In addition, sodium alginate is a food additive with low cost, safety and easy availability.

[0038] (3) The ternary positive electrode material regenerated by gel has the characteristics of good crystal shape and excellent electrochemical cycle performance, which can turn waste lithium-ion batteries into "treasures" with low recycling costs, which is beneficial to the sustainable development of the environment and the development of a circular economy.

[0039] (4) The present invention uses waste nickel-cobalt-manganese-oxide lithium ternary positive electrode materials to nano-crystallize by mechanical grinding, which is conducive to the entry of lithium ions into the particles to replenish lithium.

[0040] (5) Using the sol-gel method to assemble the ternary cathode material precursor on the surface of nano waste ternary cathode material can repair the uneven particle surface formed by mechanical grinding and reduce the consumption of lithium ions during the charging and discharging process.

[0041] (6) This method is simple and easy to operate, does not require metal ion leaching and recovery, shortens the process flow, is low-cost, and is easy to industrialize. The prepared material has excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The regenerated LiNi prepared in Example 3 0.6 Co 0.2 Mn 0.2 Electron microscope image of O2 ternary cathode material;

[0043] Figure 2 The regenerated LiNi prepared in Examples 5 and 60.8 Co 0.1 Mn 0.1 XRD pattern of O2 ternary cathode material. DETAILED DESCRIPTION

[0044] The following is a further description of the two technical routes of the present invention in conjunction with specific embodiments. The described embodiments are only part of the embodiments of the present invention, but the protection scope of the present invention is not limited to the contents described.

[0045] Example 1

[0046] The waste nickel-cobalt-manganese-oxide lithium ternary battery is discharged, disassembled, and impurities are removed to obtain a positive electrode sheet, and the positive electrode sheet is placed in a muffle furnace at 700°C for 2 hours to remove the conductive agent and binder in the positive electrode sheet to obtain a waste ternary positive electrode material. Weigh 50g of the waste ternary positive electrode material and place it in a 500ml beaker, add water to adjust the mass volume ratio of the positive electrode material to water to 1:5, then add acetic acid with a molar concentration of 2mol / L and a reducing agent sodium thiosulfate with a molar concentration of 1mol / L, and the above mixed solution is reacted for 4h under magnetic stirring at 80°C, filtered, and a filtrate rich in valuable metal ions is obtained. The content of lithium ions and transition metal ions (nickel ions, cobalt ions, manganese ions) in the filtrate is determined by ICP-OES. According to the product requirement ratio, the molar ratio of lithium element, nickel element, manganese element, and cobalt element is 1:0.5:0.2:0.3, so that the chemical formula of the obtained ternary material is LiNi 0.5 Co 0.2 Mn 0.3 O2 calculates the amount of lithium salt or transition metal salt that needs to be added, and stirs magnetically for 4 hours to obtain a nickel-cobalt-manganese-lithium precursor solution. Prepare a sodium alginate solution with a mass fraction of 0.5%, stir it into a uniform transparent solution, weigh the amount of sodium alginate solution that is 2.0 times the total molar amount of nickel-cobalt-manganese metal ions, and then slowly add the nickel-cobalt-manganese-lithium precursor solution to the sodium alginate solution for a cross-linking reaction for 2 hours to obtain a gel with a three-dimensional network structure "egg-box structure", and place the above gel in a high-temperature tubular furnace and calcine it in an air atmosphere at 800°C for 6 hours to obtain a regenerated LiNi 0.5 Co 0.2 Mn 0.3 O2 ternary positive electrode material.

[0047] Example 2

[0048] The waste nickel-cobalt-manganese-oxide lithium ternary battery is discharged, disassembled, and impurities are removed to obtain a positive electrode sheet, and the positive electrode sheet is placed in a muffle furnace at 600°C for 4 hours to remove the conductive agent and binder in the positive electrode sheet to obtain a waste ternary positive electrode material. Weigh 30g of the waste ternary positive electrode material and place it in a 500ml beaker, add water to adjust the mass volume ratio of the positive electrode material to water to 1:3, then add maleic acid with a molar concentration of 2mol / L and a reducing agent hydrazine hydrate with a molar concentration of 1mol / L, and the above mixed solution is reacted for 4 hours under magnetic stirring at 80°C, filtered, and a filtrate rich in valuable metal ions is obtained. The content of lithium ions and transition metal ions (nickel ions, cobalt ions, manganese ions) in the filtrate is determined by ICP-OES. According to the product requirement ratio, the molar ratio of lithium element, nickel element, manganese element, and cobalt element is 0.5:0.2:0.3:1, so that the chemical formula of the obtained ternary material is LiNi 0.5 Co 0.2 Mn 0.3 O2 calculates the amount of lithium salt or transition metal salt that needs to be added, and stirs magnetically for 4 hours to obtain a nickel-cobalt-manganese-lithium precursor solution. Prepare a sodium alginate solution with a mass fraction of 0.5%, stir it into a uniform transparent solution, weigh the amount of sodium alginate solution that is 2.0 times the total molar amount of nickel-cobalt-manganese metal ions, and then slowly add the nickel-cobalt-manganese-lithium precursor solution to the sodium alginate solution for a cross-linking reaction for 2 hours to obtain a gel with a three-dimensional network structure "egg-box structure", and place the above gel in a high-temperature tubular furnace and calcine it in an air atmosphere at 800°C for 6 hours to obtain a regenerated LiNi 0.5 Co 0.2 Mn 0.3 O2 ternary positive electrode material.

[0049] Example 3

[0050] The waste nickel-cobalt-manganese-oxide lithium ternary battery is discharged, disassembled, and impurities are removed to obtain a positive electrode sheet, and the positive electrode sheet is placed in a muffle furnace at 600°C for 4 hours to remove the conductive agent and binder in the positive electrode sheet to obtain a waste ternary positive electrode material. Weigh 50g of the waste ternary positive electrode material and place it in a 500ml beaker, add water to adjust the mass volume ratio of the positive electrode material to water to 1:3, then add maleic acid with a molar concentration of 2mol / L and a reducing agent hydrazine hydrate with a molar concentration of 1mol / L, and the above mixed solution is reacted for 4 hours under magnetic stirring at 80°C, filtered, and a filtrate rich in valuable metal ions is obtained. The content of lithium ions and transition metal ions (nickel ions, cobalt ions, manganese ions) in the filtrate is determined by ICP-OES. According to the product requirement ratio, the molar ratio of lithium element, nickel element, manganese element, and cobalt element is 1:0.6:0.2:0.2, so that the chemical formula of the obtained ternary material is LiNi 0.6 Co 0.2 Mn 0.2O2 calculates the amount of lithium salt or transition metal salt that needs to be added, and stirs magnetically for 4 hours to obtain a nickel-cobalt-manganese-lithium precursor solution. Prepare a sodium alginate solution with a mass fraction of 1%, stir it into a uniform transparent solution, weigh the amount of sodium alginate solution that is 2.0 times the total molar amount of nickel-cobalt-manganese metal ions, and then slowly add the nickel-cobalt-manganese-lithium precursor solution to the sodium alginate solution for a cross-linking reaction for 4 hours to obtain a gel with a three-dimensional network structure "egg-box structure", and place the above gel in a high-temperature tubular furnace and calcine it in an air atmosphere at 900°C for 5 hours to obtain a regenerated LiNi 0.6 Co 0.2 Mn 0.2 O2 ternary positive electrode material.

[0051] Example 4

[0052] The waste nickel-cobalt-manganese-oxide lithium ternary battery is discharged, disassembled, and impurities are removed to obtain a positive electrode sheet. The positive electrode sheet is placed in a muffle furnace at 800°C for 2 hours to remove the conductive agent and binder in the positive electrode sheet to obtain a waste ternary positive electrode material. Choline chloride and urea are prepared into a transparent and uniform low eutectic solvent at a molar ratio of 1:2 under magnetic stirring at 80°C. Then 20g of the waste ternary positive electrode material is weighed and added to the prepared low eutectic solvent. The mass volume ratio of the positive electrode material to the low eutectic solvent is 1:3. The leaching is carried out at a temperature of 150°C and magnetic stirring for 12 hours. Filter to obtain a filtrate rich in valuable metal ions. The content of lithium ions and transition metal ions (nickel ions, cobalt ions, manganese ions) in the filtrate is determined by ICP-OES. According to the product requirement ratio, the molar ratio of lithium element, nickel element, manganese element, and cobalt element is 1:0.6:0.2:0.2, so that the chemical formula of the obtained ternary material is LiNi 0.6 Co 0.2 Mn 0.2 O2 calculates the amount of lithium salt or transition metal salt that needs to be added, and stirs magnetically for 4 hours to obtain a nickel-cobalt-manganese-lithium precursor solution. Prepare a sodium alginate solution with a mass fraction of 1%, stir it into a uniform transparent solution, weigh the amount of sodium alginate solution that is 2.0 times the total molar amount of nickel-cobalt-manganese metal ions, and then slowly add the nickel-cobalt-manganese-lithium precursor solution to the sodium alginate solution for a cross-linking reaction of 3 hours to obtain a gel with a three-dimensional network structure "egg-box structure", and place the above gel in a high-temperature tubular furnace and calcine it in an air atmosphere at 900°C for 5 hours to obtain a regenerated LiNi 0.6 Co 0.2 Mn 0.2 O2 ternary positive electrode material.

[0053] Example 5

[0054] The waste nickel-cobalt-manganese-oxide lithium ternary battery is discharged, disassembled, and impurities are removed to obtain a positive electrode sheet, and the positive electrode sheet is placed in a muffle furnace at 800°C for 2 hours to remove the conductive agent and binder in the positive electrode sheet to obtain a waste ternary positive electrode material. Choline chloride and propylene glycol are prepared into a transparent and uniform low eutectic solvent at a molar ratio of 1:2 under magnetic stirring at 180°C. Then 20g of the waste ternary positive electrode material is weighed and added to the prepared low eutectic solvent. The mass volume ratio of the positive electrode material to the low eutectic solvent is 1:5. It is leached for 8 hours under magnetic stirring at a temperature of 150°C, filtered, and a filtrate rich in valuable metal ions is obtained. The content of lithium ions and transition metal ions (nickel ions, cobalt ions, manganese ions) in the filtrate is determined by ICP-OES. According to the product requirement ratio, the molar ratio of lithium element, nickel element, manganese element, and cobalt element is 1:0.8:0.1:0.1, so that the chemical formula of the obtained ternary material is LiNi 0.8 Co 0.1 Mn 0.1 O2 calculates the amount of lithium salt or transition metal salt that needs to be added, and stirs magnetically for 4 hours to obtain a nickel-cobalt-manganese-lithium precursor solution. Prepare a sodium alginate solution with a mass fraction of 2%, stir it into a uniform transparent solution, weigh the amount of sodium alginate solution that is 2.0 times the total molar amount of nickel-cobalt-manganese metal ions, and then slowly add the nickel-cobalt-manganese-lithium precursor solution to the sodium alginate solution for a cross-linking reaction of 6 hours to obtain a gel with a three-dimensional network structure "egg-box structure", and place the above gel in a high-temperature tubular furnace and calcine it in an air atmosphere at 1000°C for 5 hours to obtain a regenerated LiNi 0.8 Co 0.1 Mn 0.1 O2 ternary positive electrode material.

[0055] Example 6

[0056] The waste nickel-cobalt-manganese-oxide lithium ternary battery is discharged, disassembled, and impurities are removed to obtain a positive electrode sheet. The positive electrode sheet is placed in a muffle furnace at 800°C for 2 hours to remove the conductive agent and binder in the positive electrode sheet to obtain a waste ternary positive electrode material. Betaine and malonic acid are prepared into a transparent and uniform low eutectic solvent at a molar ratio of 1:5 under magnetic stirring at 180°C. Then 20g of the waste ternary positive electrode material is weighed and added to the prepared low eutectic solvent. The mass volume ratio of the positive electrode material to the low eutectic solvent is 1:5. The leaching is carried out at a temperature of 150°C and magnetic stirring for 8 hours. Filter to obtain a filtrate rich in valuable metal ions. The content of lithium ions and transition metal ions (nickel ions, cobalt ions, manganese ions) in the filtrate is determined by ICP-OES. According to the product requirement ratio, the molar ratio of lithium element, nickel element, manganese element, and cobalt element is 1:0.8:0.1:0.1, so that the chemical formula of the obtained ternary material is LiNi 0.8 Co 0.1 Mn 0.1O2 calculates the amount of lithium salt or transition metal salt that needs to be added, and stirs magnetically for 4 hours to obtain a nickel-cobalt-manganese-lithium precursor solution. Prepare a sodium alginate solution with a mass fraction of 1.5%, stir it into a uniform transparent solution, weigh the amount of sodium alginate solution that is 2.0 times the total molar amount of nickel-cobalt-manganese metal ions, and then slowly add the nickel-cobalt-manganese-lithium precursor solution to the sodium alginate solution for a cross-linking reaction of 6 hours to obtain a gel with a three-dimensional network structure "egg-box structure", and place the above gel in a high-temperature tubular furnace and calcine it in an air atmosphere at 1000°C for 5 hours to obtain a regenerated LiNi 0.8 Co 0.1 Mn 0.1 O2 ternary positive electrode material.

[0057] Example 7

[0058] The waste nickel-cobalt-manganese-oxide lithium ternary battery was discharged, disassembled, and impurities were removed to obtain a positive electrode sheet, and the positive electrode sheet was placed in a muffle furnace at 700°C for 2 hours to remove the conductive agent and binder in the positive electrode sheet to obtain the waste ternary positive electrode material. 500g of ternary positive electrode material and 5g of dispersant sodium dodecyl sulfate were weighed and added to a sand mill, and an aqueous solution was added to adjust the mass solid content of the ternary positive electrode material to 10%, and then 1kg of grinding balls with a diameter of 1mm were added, and the instrument speed was adjusted to 2500r / min, and the sand milling time was 8h to obtain a ternary positive electrode material slurry with a D50 of 100nm.

[0059] Weigh 100g of nano ternary cathode material slurry into a beaker, add nickel acetate, cobalt acetate and manganese acetate in a molar ratio of 6:2:2 and lithium acetate in a molar amount of 1.1 times the total molar amount of nickel, cobalt and manganese ions under magnetic stirring, and after complete dissolution, add citric acid solution in a molar amount of 1.2 times the total molar amount of nickel, cobalt and manganese ions and adjust the pH of the solution to 7 with ammonia water until a sol is formed, and then heat in a water bath to form a gel, and place the above gel in a high-temperature tubular furnace and sinter at a high temperature of 800°C in an air atmosphere for 6h to obtain a nano waste ternary cathode material as the core and LiNi as the shell. 0.6 Co 0.2 Mn 0.2 Ternary cathode material for O2 regeneration.

[0060] Example 8

[0061] The waste nickel-cobalt-manganese-oxide lithium ternary battery was discharged, disassembled, and impurities were removed to obtain a positive electrode sheet, and the positive electrode sheet was placed in a muffle furnace at 600°C for 4 hours to remove the conductive agent and binder in the positive electrode sheet to obtain the waste ternary positive electrode material. 500g of ternary positive electrode material and 5g of dispersant sodium dodecyl sulfate were weighed and added to a sand mill, and an aqueous solution was added to adjust the mass solid content of the ternary positive electrode material to 10%, and then 1kg of grinding balls with a diameter of 2mm were added, and the instrument speed was adjusted to 2000r / min, and the sand milling time was 6h to obtain a ternary positive electrode material slurry with a D50 of 150nm.

[0062] 100g of nano ternary cathode material slurry was weighed and poured into a beaker. Nickel acetate, cobalt acetate and manganese acetate in a molar ratio of 6:2:2 and lithium acetate in a molar amount of 1.1 times the total molar amount of nickel, cobalt and manganese ions were added under magnetic stirring. After complete dissolution, a citric acid solution in a molar amount of 1.2 times the total molar amount of nickel, cobalt and manganese ions was added and the pH of the solution was adjusted to 7 with ammonia water until a sol was formed. The gel was then heated in a water bath to form a gel. The gel was placed in a high-temperature tubular furnace and sintered at 700°C in an air atmosphere for 6h to obtain a nano waste ternary cathode material as the core and LiNi as the shell. 0.6 Co 0.2 Mn 0.2 Ternary cathode material for O2 regeneration.

[0063] Example 9

[0064] The waste nickel-cobalt-manganese-oxide lithium ternary battery is discharged, disassembled, and impurities are removed to obtain a positive electrode sheet, and the positive electrode sheet is placed in a muffle furnace at 800°C for 6 hours to remove the conductive agent and binder in the positive electrode sheet to obtain the waste ternary positive electrode material. 500g of ternary positive electrode material and 5g of dispersant gul gum are weighed and added to a sand mill, and an aqueous solution is added to adjust the mass solid content of the ternary positive electrode material to 10%, and then 1kg of grinding balls with a diameter of 5mm are added, and the instrument speed is adjusted to 2200r / min, and the sand milling time is 6h to obtain a ternary positive electrode material slurry with a D50 of 200nm.

[0065] Weigh 100g of nano ternary cathode material slurry into a beaker, add nickel nitrate, cobalt nitrate and manganese nitrate in a molar ratio of 5:2:3 and lithium nitrate whose molar amount is 1.1 times the total molar amount of nickel, cobalt and manganese ions under magnetic stirring, and after complete dissolution, add citric acid solution whose molar amount is 1.2 times the total molar amount of nickel, cobalt and manganese ions and adjust the pH of the solution to 7 with ammonia water until a sol is formed, and then heat it in a water bath to form a gel, and place the above gel in a high-temperature tubular furnace and sinter it at a high temperature for 6h in an air atmosphere at 900℃ to obtain a nano waste ternary cathode material as the core and LiNi as the shell. 0.5 Co 0.2 Mn 0.3 Ternary cathode material for O2 regeneration.

[0066] Example 10

[0067] The waste nickel-cobalt-manganese-oxide lithium ternary battery was discharged, disassembled, and impurities were removed to obtain a positive electrode sheet, and the positive electrode sheet was placed in a muffle furnace at 800°C for 8 hours to remove the conductive agent and binder in the positive electrode sheet to obtain the waste ternary positive electrode material. 500g of ternary positive electrode material and 10g of dispersant gul gum were weighed and added to a sand mill, and an aqueous solution was added to adjust the mass solid content of the ternary positive electrode material to 15%, and then 2kg of grinding balls with a diameter of 5mm were added, and the instrument speed was adjusted to 2500r / min. The sand milling time was 6h, and a ternary positive electrode material slurry with a D50 of 120nm was obtained.

[0068] 100g of nano ternary cathode material slurry was weighed and poured into a beaker. Nickel acetate, cobalt acetate and manganese acetate in a molar ratio of 5:2:3 and lithium acetate in a molar amount of 1.1 times the total molar amount of nickel, cobalt and manganese ions were added under magnetic stirring. After complete dissolution, a citric acid solution in a molar amount of 1.2 times the total molar amount of nickel, cobalt and manganese ions was added and the pH of the solution was adjusted to 7 with ammonia water until a sol was formed. The gel was then heated in a water bath to form a gel. The gel was placed in a high-temperature tubular furnace and sintered at a high temperature of 1000°C in an air atmosphere for 8h to obtain a nano waste ternary cathode material as a core and a LiNi shell. 0.5 Co 0.2 Mn 0.3 Ternary cathode material for O2 regeneration.

[0069] Embodiment 11

[0070] The waste nickel-cobalt-manganese-oxide lithium ternary battery was discharged, disassembled, and impurities were removed to obtain a positive electrode sheet, and the positive electrode sheet was placed in a muffle furnace at 600°C for 4 hours to remove the conductive agent and binder in the positive electrode sheet to obtain the waste ternary positive electrode material. 500g of ternary positive electrode material and 10g of dispersant hexadecyltrimethylammonium bromide were weighed and added to a sand mill, and an aqueous solution was added to adjust the mass solid content of the ternary positive electrode material to 10%, and then 1kg of grinding balls with a diameter of 5mm were added, the instrument speed was adjusted to 2200r / min, and the sand milling time was 6h to obtain a ternary positive electrode material slurry with a D50 of 200nm.

[0071] 100g of nano ternary cathode material slurry was weighed and poured into a beaker. Nickel acetate, cobalt acetate and manganese acetate in a molar ratio of 8:1:1 and lithium acetate in a molar amount of 1.1 times the total molar amount of nickel, cobalt and manganese ions were added under magnetic stirring. After complete dissolution, a citric acid solution in a molar amount of 1.2 times the total molar amount of nickel, cobalt and manganese ions was added and the pH of the solution was adjusted to 7 with ammonia water until a sol was formed. The gel was then heated in a water bath to form a gel. The gel was placed in a high-temperature tubular furnace and sintered at a high temperature of 900°C in an air atmosphere for 6h to obtain a nano waste ternary cathode material as a core and a LiNi shell. 0.8 Co 0.1 Mn 0.1Ternary cathode material for O2 regeneration.

[0072] Comparative Example 1

[0073] The difference from Example 7 is that after the waste nickel cobalt manganese oxide batteries are ground, no surface modification treatment using the sol-gel method is performed.

[0074] The waste nickel-cobalt-manganese-oxide lithium ternary battery is discharged, disassembled, and impurities are removed to obtain a positive electrode sheet, and the positive electrode sheet is placed in a muffle furnace at 700°C for 2 hours to remove the conductive agent and binder in the positive electrode sheet to obtain a waste ternary positive electrode material. 500g of ternary positive electrode material and 5g of dispersant sodium dodecyl sulfate are weighed and added to a sand mill, and an aqueous solution is added to adjust the mass solid content of the ternary positive electrode material to 10%, and then 1kg of grinding balls with a diameter of 1mm are added, and the instrument speed is adjusted to 2500r / min, and the sand milling time is 8h to obtain a ternary positive electrode material slurry with a D50 of 100nm, centrifuged, transferred to a vacuum drying oven and dried at 80°C for 2h to obtain a nano waste ternary positive electrode material.

[0075] Comparative Example 2

[0076] The difference from Example 7 is that the ternary cathode material obtained from the waste nickel cobalt manganese oxide battery is not ground, and the ternary precursor is directly assembled on the surface of the ternary cathode material by the sol-gel method.

[0077] The waste nickel-cobalt-manganese-oxide lithium ternary battery is discharged, disassembled, and impurities are removed to obtain a positive electrode sheet, and the positive electrode sheet is placed in a muffle furnace at 700°C for 2 hours to remove the conductive agent and binder in the positive electrode sheet to obtain a waste ternary positive electrode material. Weigh 10g of the waste ternary positive electrode material and pour it into a beaker, add an aqueous solution to adjust the mass solid content of the ternary positive electrode material to 10%, add nickel acetate, cobalt acetate and manganese acetate in a molar ratio of 6:2:2 and lithium acetate in a molar amount of 1.1 times the total molar amount of nickel-cobalt-manganese ions under magnetic stirring, and after complete dissolution, add a citric acid solution in a molar amount of 1.2 times the total molar amount of nickel-cobalt-manganese ions and adjust the pH of the solution to 7 with ammonia water until a sol is formed, and then heat it in a water bath to form a gel, and place the above gel in a high-temperature tubular furnace and sinter it at high temperature for 6 hours at 800°C in an air atmosphere to obtain a waste ternary positive electrode material as the core and LiNi as the shell. 0.5 Co 0.2 Mn 0.3 Ternary cathode material for O2 regeneration.

[0078] The positive electrode materials prepared in Examples 1-11 and Comparative Examples 1-2 were subjected to cycle performance tests.

[0079] The prepared positive electrode material, acetylene black and PVDF binder were mixed evenly in NMP at a weight ratio of 8:1:1 under magnetic stirring, and the obtained slurry was coated on aluminum foil with a scraper, dried in an oven at 60°C, and the pole piece was rolled and punched into a small disc with a diameter of 13 mm. Then it was dried in a vacuum drying oven at 120°C for 16 hours and transferred to a glove box filled with an inert atmosphere. Subsequently, a metal lithium sheet was used as the negative electrode, the electrolyte was 1 mol LiPF6 / EC+DMC (volume ratio 1:1), and Celgard2400 was used as the diaphragm to assemble a button battery. The assembled button battery was subjected to constant current charge and discharge tests using the Blue Electric Battery Test System. The charge and discharge voltage range was 2.8 to 4.3 V, and the cycle performance test current was 0.2C (1C was 150 mA g -1 ). After 50 cycles, the discharge capacity and discharge capacity retention rate of the ternary cathode materials prepared by the two technical routes are shown in Table 1 and Table 2:

[0080]

[0081] Table 1

[0082]

[0083] Table 2

[0084] As can be seen from Table 1, the ternary positive electrode material prepared by regeneration route 1 has excellent cycle performance. As can be seen from Table 2, through regeneration route 2, the waste nickel-cobalt-manganese ternary positive electrode material is obtained by nano-crystallization by mechanical grinding, and then the nano-crystallized waste ternary positive electrode material is used as the core, and the ternary positive electrode material precursor is assembled on its surface by sol-gel method, and the repaired and regenerated ternary positive electrode material is obtained by high-temperature sintering, which has excellent electrochemical properties and can improve the first coulomb efficiency and cycle stability of the material. Simply grinding the waste nickel-cobalt-manganese lithium battery without surface sol-gel modification can improve the cycle performance of the material, but due to the uneven surface of the particles caused by ball milling, too many lithium ions are consumed during the charge and discharge process, resulting in a low first coulomb efficiency of the material. The obtained waste ternary positive electrode materials are not ground, and the ternary precursor is directly assembled on the surface of the ternary positive electrode material by the sol-gel method. Since the material particles are large, the ternary positive electrode material precursor is assembled on its surface, and the formed particle size is too large, which is not conducive to the internal lithium insertion and lithium replenishment of lithium, nor is it conducive to the cycle stability of the material, and the capacity retention rate is very low.

Claims

1. A method for recycling waste lithium-ion batteries to regenerate ternary positive electrode materials, It is characterized in that The following steps are involved: S11, pre-treating the waste lithium-ion batteries to remove the conductive agent and the binder in the positive electrode sheet under high temperature conditions; S22, ball milling the positive electrode material obtained in step S11; S23, adding a soluble lithium source, a nickel source, a cobalt source and a manganese source to the solution containing the ball-milled nanoparticles obtained in step S22, and after complete dissolution, adding a citric acid solution and adjusting the pH of the solution with ammonia water until a sol is formed, and then heating in a water bath to form a gel; using the nanoparticles as cores, repairing and assembling a ternary cathode material precursor on their surface by a sol-gel method; S24, calcining the gel obtained in step S23 to obtain a positive electrode material; The ball milling process reduces the particle size of the cathode material to 50-300nm; The lithium source is selected from one or more of lithium carbonate, lithium nitrate, lithium acetate and lithium hydroxide; the nickel source is selected from one or more of nickel carbonate, nickel nitrate, nickel acetate and nickel hydroxide; the cobalt source is selected from one or more of cobalt carbonate, cobalt nitrate, cobalt acetate and cobalt hydroxide; the manganese source is selected from one or more of manganese carbonate, manganese nitrate, cobalt acetate and manganese hydroxide; In step S23, the ratio of the molar amount of lithium ions to the total molar amount of nickel, cobalt and manganese ions is 1.05-1.1:1, the ratio of the molar amount of citric acid added to the total molar number of the three metal ions of nickel, cobalt and manganese is 1-2:1, and the pH of the solution is adjusted to 7-8 with ammonia water.

2. The method for recycling waste lithium-ion batteries and regenerating ternary positive electrode materials according to claim 1, It is characterized in that In step S22, the ball milling process is to mix the positive electrode material, water and dispersant, the added dispersant is 1-5% of the mass of the positive electrode material, and the solid content of the positive electrode material is 10-30%.

3. The method for recycling waste lithium-ion batteries and regenerating ternary positive electrode materials according to claim 2, It is characterized in that The mass ratio of the grinding balls added during the ball milling process to the positive electrode material is 2-5:1, the rotation speed of the ball milling process is 1500-2500r / min, and the ball milling time is 2-40h.

4. The method for recycling waste lithium-ion batteries and regenerating ternary positive electrode materials according to claim 1, It is characterized in that In step S23, the molar ratio of nickel, cobalt and manganese ions is one of 1:1:1, 5:2:3, 6:2:2 or 8:1:

1.

5. The method for recycling waste lithium-ion batteries and regenerating ternary positive electrode materials according to claim 1, It is characterized in that In step S24, the sintering temperature is 700-1000° C., the sintering time is 5-20 hours, and the sintering atmosphere is air or oxygen.

Citation Information

Patent Citations

  • Method for recovering and preparing lithium cobalt oxide by using disused lithium battery

    CN101673859A

  • Method for recovering and preparing lithium iron phosphate from waste lithium iron phosphate battery

    CN102751548A

  • Method for preparing lithium nickelate cobaltate manganate cathode material by taking waste lithium ion batteries as raw material

    CN103606651A

  • Regenerated ternary cathode material and preparation method thereof

    CN106785173A

  • Method for regenerating waste nickel-cobalt-manganese ternary lithium battery positive electrode material

    CN108767351A