A method for preparing foamed aluminum net-shaped parts based on liquid phase foaming

By pretreating the foaming agent with liquid phase method and adding bubble stabilizer, combined with extrusion casting and gas protection technology, the problems of low production efficiency and high cost of foam aluminum net forming parts in the prior art are solved, and high density and Mass production of foam aluminum net forming parts in complex configurations.

CN116516204BActive Publication Date: 2024-12-03NORTHEASTERN UNIV CHINA +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310521350.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-12-03
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

The existing technology is difficult to mass-produce aluminum foamed parts with high density and complex configurations. The liquid-phase foaming process has problems such as poor fluidity, rapid decomposition of foaming agents, and uneven pore structure, resulting in low production efficiency and high cost. .

Method used

Pretreat the foaming agent by liquid phase method, add bubble stabilizer and foaming agent, prepare dense preforms by extrusion casting, and perform slow-cooling foam under gas protection, and use vacuum and inert gas protection to form complex shape foam Aluminum net forming parts.

Benefits of technology

The density and expansion rate of the preform are improved, the decomposition of the foaming agent is reduced, the uniformity and molding accuracy of the pore structure are enhanced, the production cost is reduced, and the production is achieved at low cost mass production of foam aluminum net-formed parts of complex shapes is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116516204B_ABST
    Figure CN116516204B_ABST
Patent Text Reader

Abstract

A method for preparing a foamed aluminum net-shaped part based on liquid phase foaming belongs to the technical field of porous metal materials. The present invention relates to a method for preparing a simple configuration foamed preform by using a liquid phase method, and preparing a foamed aluminum complex net-shaped component by foaming under nitrogen or an inert atmosphere. The specific technical scheme is to melt an aluminum alloy with a specific composition, add a bubble stabilizer such as aluminum powder, add a pretreated foaming agent under stirring, and squeeze cast it into a high-density simple configuration preform. After the surface oxide film is polished to remove the surface, it is foamed in a complex configuration mold under gas protection, and a net-shaped foamed aluminum component is obtained after slow cooling. The foamed aluminum component prepared by this method has a uniform pore structure, high surface forming accuracy, fast production cycle, and is easy to mass produce.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous metal materials, and in particular relates to a method for preparing a foam aluminum net-shaped part. Background Art

[0002] Aluminum foam has low density, high specific strength, excellent properties such as energy absorption, damping and sound absorption, flame retardancy and heat insulation, and is rapidly developing in the fields of aerospace, machinery manufacturing, automobiles, trains, etc. Driven by the urgent demand for lightweight automobile bodies, the preparation and application of lightweight, high energy absorption aluminum foam net-shaped components are receiving great attention from researchers.

[0003] At present, the industrialized direct forming of foam aluminum components adopts the powder densification foaming method. Its main process is to use metal powder as raw material, prepare preforms through cold pressing, hot pressing and other processes, and then foam in the mold to obtain net-shaped parts. This method has a complex production process, low production efficiency, high costs of raw materials, molds and processes, and is difficult to apply on a large scale. In the aluminum melt of the liquid phase melt foaming method and the gas injection foaming method, thickeners or ceramic particles that significantly increase the viscosity of the melt are added. After the bubbles are formed, the fluidity is poor, and heat preservation and foaming are required, which makes it difficult to use conventional casting technology for direct injection molding. The main difficulty in using the liquid phase method to prepare foamable preforms is that the foaming agent decomposes rapidly at high temperatures, and the aluminum melt containing thickeners or particles has extremely poor fluidity, making it difficult to quickly and batch prepare dense, complex configuration preforms. In addition, uneven heating may occur during the preform heating and foaming process, resulting in incomplete foaming in some areas, or inconsistent density and pore structure due to the preform being not dense, and the foaming agent may start to decompose before the preform melts, which may lead to defects such as cracks. Currently, there is no mass-produced process for preparing preforms by liquid phase method and then heating and foaming to prepare aluminum foam net-shaped components with highly consistent pore structure and performance. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a foamed simple configuration preform based on a liquid phase method, and then preparing a complex-shaped foam aluminum net-shaped part by gas protection foaming.

[0005] In order to achieve the above purpose, the following technical solutions are adopted:

[0006] A method for preparing a foamed aluminum net-shaped part by foaming based on a liquid phase method, specifically a method for preparing a preform by a liquid phase method, and foaming the foamed aluminum net-shaped part, wherein the method has the following operating steps:

[0007] (1) Pretreatment of the foaming agent: The foaming agent titanium hydride is heated to 460-520°C in an air atmosphere, kept at this temperature and evacuated, and then cooled to room temperature while maintaining the pressure in the furnace;

[0008] (2) Adding a bubble stabilizer: Melting the aluminum alloy in a crucible, and then stirring and adding the bubble stabilizer to the molten aluminum alloy at 680-720°C;

[0009] (3) Adding foaming agent: Cool the aluminum liquid to 620-645°C, add the pretreated foaming agent while stirring, and stir to mix;

[0010] (4) Squeeze casting: After stopping stirring, the melt is quickly cast into the preform mold, and the gas in the aluminum liquid is discharged through extrusion casting and quickly solidified to prepare a dense simple configuration foam preform;

[0011] (5) Gas protection foaming: The oxide on the surface of the preform is polished off, cut into pieces, and loaded into a preheated foaming mold. The mold is then sent into a sealable heating furnace cavity. The cavity is sealed and evacuated, and then nitrogen or inert protective gas is introduced;

[0012] (6) Slow cooling with mold: The mold is transferred out of the furnace, slowly cooled under gas protection, and then opened and taken out to obtain the foam aluminum net shape part.

[0013] The above-mentioned method for preparing a foamed aluminum net-shaped part based on liquid phase foaming, wherein:

[0014] In the step (1), during the heat preservation and vacuum treatment, the gas pressure needs to be reduced to 200-480Pa.

[0015] In the step (2), the aluminum alloy is preferably an AlSi alloy with a Si mass fraction of 7-12wt%, or an AlSiCu alloy with a Cu mass fraction of 4-6wt% and a Si mass fraction of 3-7wt%. The aluminum alloy may also contain other metal elements including Mg and Zn with a mass fraction of 0-1wt%, and the rest is aluminum.

[0016] In the step (2), the components of the bubble stabilizer are metallic calcium and metallic aluminum powder, and the mass fractions of the two in the aluminum alloy are 0.2-1.0wt% of metallic Ca and 8-20wt% of metallic aluminum powder.

[0017] In the step (3), 0.8-1.2 wt % of the pretreated foaming agent is added to the molten aluminum alloy, and then stirred at a speed of 800 rpm for 120-300 s.

[0018] In the extrusion casting process of step (4), a pressure of 20-50 MPa is applied to squeeze out the gas in the aluminum liquid, and the pressure is maintained to solidify to form a dense preform.

[0019] During the foaming process of the preform in step (5), after the preform is placed in the preheating mold, it is first evacuated and then a protective gas is introduced. The foaming under the protective atmosphere can fuse the foams formed by multiple preforms to form a net-shaped part with a complex configuration in the mold; the protective gas is an inert gas such as nitrogen or argon, the mold preheating temperature is 640-700°C, the foaming temperature of the preform is between 630-680°C, and the insulation time is 14-25min;

[0020] The cooling process in the step (6) is to cool the mold slowly under the protection of nitrogen or inert atmosphere.

[0021] Beneficial effects of the present invention:

[0022] (1) Titanium hydride is converted into TiH by a two-step combined treatment of high temperature and vacuum. 1.5 The decomposition rate of the foaming agent at high temperature is significantly slowed down by using an aluminum-silicon alloy with a Si content of 7-12wt% or an AlSiCu alloy with a Cu content of 6wt% and a Si content of 3-7wt% with a lower melting point, and adding a pretreated foaming agent at 620-640°C to greatly reduce the decomposition of the foaming agent during mixing and casting, increase the density of the preform, and achieve a larger expansion rate during the foaming process of the preform; if attached Figure 1 As shown, when the foaming agent treated with high temperature and vacuum is added, the expansion rate of the liquid foam slows down significantly, while when the foaming agent treated with oxidation alone is added, the foam expands rapidly.

[0023] (2) By using alloys with good fluidity in the casting process such as AlSi and AlCuSi, controlling the amount of metal Ca added, and adding metal aluminum powder as an auxiliary bubble stabilizer, the effect of the bubble stabilizer on the fluidity of the melt is reduced to ensure the fluidity of the aluminum melt when it is injected from the stirring furnace into the extrusion casting mold, which is beneficial to improving the yield rate of preform preparation.

[0024] (3) The preform is prepared by extrusion casting process. During the molding process, the bubbles that have been formed are squeezed out and solidified under pressure, which reduces the decomposition of the foaming agent during the solidification of the aluminum liquid, improves the density of the preform, and reduces the uneven heating caused by the high porosity in the preform during the foaming process; the decomposition behavior of the foaming agent is changed by pretreatment of the foaming agent and high-temperature stirring and mixing. Figure 3 As shown, the preform expands rapidly during the continuous heating process after melting, which helps to eliminate the pore structure defects caused by the low-temperature decomposition of the foaming agent and improve the controllability of the expansion rate and pore structure uniformity of the foam.

[0025] (4) During the preform foaming process, vacuum and nitrogen or inert gas protection are used to achieve metallurgical fusion of the newly formed surfaces of the preforms after foaming. Using this method, large and complex foam aluminum net-shaped parts can be prepared using simple configuration preforms; Figure 4 It is a "U"-shaped net-shaped part prepared by fusing multiple preforms.

[0026] (5) During the cooling process, slow cooling is adopted to first form a dense layer on the outer surface of the foam component, and then slowly solidify inward, so that the outer surface molding accuracy deviation of the net-shaped part is less than 0.5mm, avoiding the shrinkage and wrinkling of bubbles on the sample surface caused by rapid cooling, which affects the surface molding accuracy. Figure 6 As shown, after measurement, the surface tolerance of the net-shaped part is less than 0.5mm.

[0027] (6) The method of the present invention is easy to achieve low-cost mass production. The preform has a simple configuration and good aluminum liquid fluidity. Multiple preforms can be prepared by a one-mold multi-cavity method, or a net-shaped part can be prepared by a one-furnace multi-mold foaming method, thereby improving the production efficiency of the preform. During the foaming process, there is no scouring effect of aluminum liquid on the surface of the foaming mold at high temperature, which reduces the erosion of the aluminum liquid on the inner surface of the mold, increases the mold life, and thus reduces the mold cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The foaming expansion rate of the preform after high temperature vacuum combined treatment;

[0029] Figure 2 The strip preform prepared in Example 1;

[0030] Figure 3 It is the expansion change curve of the preform during the heating process after melting;

[0031] Figure 4 A "U"-shaped net-shaped part prepared by fusing multiple preforms;

[0032] Figure 5 It is a block preform;

[0033] Figure 6 This is a cross section of a net-shaped aluminum foam part after the preform prepared in Example 3 is foamed and fused;

[0034] Figure 7 The difference between the three-dimensional blue-ray scanning result and the drawing of the net-shaped foam aluminum part prepared in Example 3;

[0035] Figure 8 A net-shaped rectangular cross-section part prepared in Example 4;

[0036] Fig. 9 This is the case of aluminum foam prepared in comparative example. DETAILED DESCRIPTION

[0037] Example 1

[0038] A method for preparing a foamed aluminum net-shaped part based on liquid phase foaming, the specific operation steps are as follows:

[0039] (1) Pretreatment of the foaming agent: Place the foaming agent titanium hydride in a vacuum treatment furnace, heat it to 500°C in an air atmosphere, keep it warm and evacuate it to reduce the pressure in the chamber to 280Pa, then stop heating and slowly cool it with the furnace;

[0040] (2) Adding a bubble stabilizer: 800 g of an aluminum alloy containing 10.0% silicon by mass was melted in a crucible, and then 1.0% metal calcium and 8.0% metal aluminum powder by mass were added to the molten aluminum alloy at 720° C. and stirred at 500 rpm for 180 s to mix evenly;

[0041] (3) Adding a foaming agent: The temperature of the aluminum melt is lowered to 630° C., and then 1.0% of pretreated titanium hydride is added, stirred at 800 rpm for 120 seconds, and then the melt is quickly cast into a preform mold;

[0042] (4) Extrusion casting: Extrusion mold and apply 20MPa pressure to solidify the preform to prepare a dense strip preform, such as Figure 2 As shown;

[0043] (5) Gas protection foaming: Grind off the oxide on the surface of the strip preform and cut it into small sections. Send the foaming mold to a 650℃ heating furnace for preheating. After the mold is preheated, open the foaming mold, load the preform and send it to the atmosphere heating furnace. Close the door of the atmosphere heating furnace, turn on the vacuum pump to evacuate for 1 minute, turn off the vacuum pump, and pass N2. Keep the foaming at 640℃ for 20 minutes;

[0044] (6) Slow cooling with mold: Move the foaming mold from the atmosphere heating furnace to the cooling position, slowly cool it under the protection of the atmosphere, and then open the furnace door and mold to take out the foam aluminum net shape part.

[0045] Example 2

[0046] A method for preparing a foamed aluminum net-shaped part based on liquid phase foaming, the specific operation steps are as follows:

[0047] (1) Pretreatment of the foaming agent: Place the foaming agent titanium hydride in a vacuum treatment furnace, heat it to 460°C in an air atmosphere, keep it warm and evacuate it to reduce the pressure in the chamber to 200 Pa, then stop heating and slowly cool it with the furnace;

[0048] (2) Adding a bubble stabilizer: 1200 g of an aluminum alloy containing 12.0% by mass of silicon was melted in a crucible, and then 0.5% by mass of metallic calcium and 15.0% by mass of metallic aluminum powder were added to the molten aluminum alloy at 720° C. and stirred at a speed of 500 rpm for 180 s to mix evenly;

[0049] (3) Adding a foaming agent: The temperature of the aluminum melt is lowered to 625°C, and then 1.2% of pretreated titanium hydride is added, stirred at 800 rpm for 240 seconds, and then the melt is quickly cast into a preform mold;

[0050] (4) Extrusion casting: Extrusion mold and applying 40MPa pressure to solidify the preform to prepare a dense block preform;

[0051] (5) Gas protection foaming: Grind off the oxide on the surface of the block preform and cut it into small pieces. Send the foaming mold to a 660℃ heating furnace for preheating. After the mold is preheated, open the foaming mold, load multiple foaming preforms and send them to the atmosphere heating furnace. Close the door of the atmosphere heating furnace, turn on the vacuum pump to evacuate for 2 minutes, turn off the vacuum pump, and pass Ar gas for protection. Keep warm at 650℃ for 18 minutes;

[0052] (6) Slow cooling with mold: Move the foaming mold out of the atmosphere heating furnace to the cooling position, slowly cool it under the protection of the atmosphere, and then open the furnace door and the mold to take out the foam aluminum net shape. Figure 4 shown.

[0053] Example 3

[0054] A method for preparing a foamed aluminum net-shaped part based on liquid phase foaming, the specific operation steps are as follows:

[0055] (1) Pretreatment of the foaming agent: Place the foaming agent titanium hydride in a vacuum treatment furnace, heat it to 520°C in an air atmosphere, keep it warm and evacuate it to reduce the pressure in the chamber to 480Pa, then stop heating and slowly cool it with the furnace;

[0056] (2) Adding a bubble stabilizer: 1500 g of an aluminum alloy containing 7.0% silicon and 5.0% Cu by mass was melted in a crucible, and then 0.2% metal calcium and 20.0% metal aluminum powder by mass were added to the molten aluminum alloy at 720° C. and stirred at 500 rpm for 200 s to mix evenly;

[0057] (3) Adding a foaming agent: The temperature of the aluminum melt is lowered to 640° C., and then 1.2% by mass of pretreated titanium hydride is added, stirred at a speed of 800 rpm for 240 seconds, and then the melt is quickly cast into a preform mold;

[0058] (4) Extrusion casting: Extrusion mold and apply 50MPa pressure to solidify the preform to prepare a dense block preform. Figure 5 As shown;

[0059] (5) Gas protection foaming: Place the foaming mold in a 690℃ heating furnace for preheating. After the mold is preheated, open the foaming mold, load multiple foam preforms and place them in an atmosphere heating furnace. Close the door of the atmosphere heating furnace, turn on the vacuum pump to evacuate for 1 minute, turn off the vacuum pump, and introduce N2 gas for protection. Keep the foaming at 670℃ for 23 minutes;

[0060] (6) Slow cooling with mold: Move the foaming mold out of the atmosphere heating furnace to the cooling position, slowly cool it under the protection of the atmosphere, and then open the furnace door and the mold to take out the foam aluminum net shape. Figure 6 Check its appearance, as shown in the attached Figure 7 As shown, the surface deviation is less than 0.5mm.

[0061] Example 4

[0062] A method for preparing a foamed aluminum net-shaped part based on liquid phase foaming, the specific operation steps are as follows:

[0063] (1) Pretreatment of the foaming agent: Place the foaming agent titanium hydride in a vacuum treatment furnace, heat it to 520°C in an air atmosphere, keep it warm and evacuate it to reduce the pressure in the chamber to 480Pa, then stop heating and slowly cool it with the furnace;

[0064] (2) Adding a bubble stabilizer: 1200 g of an aluminum alloy containing 7.0% by mass of silicon was melted in a crucible, and then 0.2% by mass of metal calcium and 20.0% by mass of metal aluminum powder were added to the molten aluminum alloy at 720° C. and stirred at a speed of 500 rpm for 180 seconds to mix evenly;

[0065] (3) Adding a foaming agent: The temperature of the aluminum melt is lowered to 645°C, and then 0.8% by mass of pretreated titanium hydride is added, stirred at a speed of 600 rpm for 180 seconds, and then the melt is quickly cast into a preform mold;

[0066] (4) Extrusion casting: Extrusion mold and applying 25 MPa pressure to solidify the preform to prepare a dense block preform;

[0067] (5) Gas protection foaming: Cut a 200g sample from the block preform. Place the rectangular foaming mold in a 700℃ heating furnace for preheating. After the mold is preheated, load multiple foaming preforms into the atmosphere heating furnace. Close the door of the atmosphere heating furnace, turn on the vacuum pump to evacuate for 1min30s, turn off the vacuum pump, and introduce N2 gas for protection. Keep the foaming at 680℃ for 20min;

[0068] (6) Slow cooling with mold: Move the foaming mold out of the atmosphere heating furnace to the cooling position, slowly cool it under the protection of the atmosphere, and then open the furnace door and the mold to take out the foam aluminum net shape. Figure 8 shown.

[0069] Comparative Example

[0070] A method for preparing a foamed aluminum net-shaped part based on liquid phase foaming, the specific operation steps are as follows:

[0071] (1) Pretreatment of the foaming agent: Place the foaming agent titanium hydride in a vacuum treatment furnace, heat it to 520°C in an air atmosphere, keep it warm for 20 minutes, then stop heating and slowly cool it in the furnace;

[0072] (2) Adding a bubble stabilizer: 1500 g of an AlSi alloy containing 10.0% silicon by mass was melted in a crucible, and then 3% metal calcium by mass was added to the molten aluminum alloy at 720° C. and stirred at 500 rpm for 200 s to mix evenly;

[0073] (3) Adding foaming agent: The temperature of the aluminum melt is lowered to 635°C, and then 1.2% of pretreated titanium hydride is added, stirred at 800 rpm for 240 seconds, and then the melt is quickly cast into the preform mold. Because there are a large number of bubbles in the aluminum liquid and the viscosity is high, it cannot fill the preform mold, and there are a large number of bubbles of different sizes in the preform;

[0074] (4) Heat preservation and foaming: The rectangular cross-section foaming mold is sent to a 690°C heating furnace for preheating. After the mold is preheated, the preform is loaded. Heat preservation and foaming are carried out at 670°C for 20 minutes. The foam is only partially foamed and does not fill the rectangular mold;

[0075] (5) Rapid cooling: The foaming mold is removed from the heating furnace and water is sprayed on the mold surface for rapid cooling. After cooling, the surface of the foam body in contact with the inner wall of the mold becomes obviously uneven, which is quite different from the inner wall of the mold. Fig. 9 shown.

Claims

1. A method for preparing a foamed aluminum net-shaped part based on liquid phase foaming, Features The steps are as follows: (1) Pretreatment of the foaming agent: Heat the foaming agent titanium hydride to 460-520°C in an air atmosphere, keep the temperature and evacuate, reduce the gas pressure to 200-480Pa, and then keep the pressure and cool to room temperature in the furnace; (2) Adding a bubble stabilizer: melting an aluminum alloy in a crucible, and then stirring and adding a bubble stabilizer to the molten aluminum alloy at 680-720°C; the aluminum alloy is an AlSi alloy with a Si mass fraction of 7-12wt%, or an AlSiCu alloy with a Cu mass fraction of 4-6wt% and a Si mass fraction of 3-7wt%; the bubble stabilizer comprises metallic calcium and metallic aluminum powder, and the mass fractions of the two in the aluminum alloy are 0.2-1.0wt% of metallic calcium and 8-20wt% of metallic aluminum powder; (3) Adding foaming agent: Cool the aluminum liquid to 620-645°C, add the pretreated foaming agent while stirring, and stir to mix; (4) Squeeze casting: After stopping stirring, the melt is quickly cast into the preform mold, and the gas in the aluminum liquid is expelled by applying a pressure of 20-50MPa for extrusion casting, and the pressure is maintained and solidified to form a dense preform, thereby preparing a dense simple configuration foamed preform; (5) Gas protection foaming: The oxide on the surface of the preform is polished off, cut into pieces, and loaded into a preheated foaming mold. The mold is then sent into a sealable heating furnace cavity. After the cavity is sealed, it is evacuated and then nitrogen or inert protective gas is introduced; (6) Slow cooling with mold: The mold is transferred out of the furnace, slowly cooled under gas protection, and then opened and taken out to obtain the foam aluminum net shape part.

2. A method for preparing a foamed aluminum net shape part based on liquid phase foaming according to claim 1, Features In the step (3), 0.8-1.2 wt % of the pretreated foaming agent is added to the molten aluminum alloy, and then stirred at a speed of 800 rpm for 120-300 s.

3. A method for preparing a foamed aluminum net shape part based on liquid phase foaming according to claim 1, Features During the foaming process of the preform in step (5), after the preform is placed in the preheating mold, it is first evacuated and then a protective gas is introduced. The foaming under the protective atmosphere can fuse the foams formed by multiple preforms to form a complex net-shaped part in the mold; the protective gas is nitrogen or argon inert gas, the mold preheating temperature is 640-700°C, the foaming temperature of the preform is between 630-680°C, and the insulation time is 14-25 minutes.

4. A method for preparing a foamed aluminum net shape part based on liquid phase foaming according to claim 1, Features The cooling process in step (6) is to cool the mold slowly under nitrogen or inert atmosphere protection.