A bionic heart valve for drug response release mediated by inflammatory microenvironment and its preparation method and use
By grafting chondroitin sulfate and glycyrrhizic acid on the heart valve to form anti-thrombotic and anti-inflammatory properties, it solves the problems of calcification and thrombosis of existing heart valves under inflammatory response, and achieves better blood compatibility and endothelium Chemical potential, extending valve life.
Patent Information
- Application Number
- CN202310812467.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-04
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-07-04
AI Technical Summary
After existing heart valves are implanted, inflammatory reactions lead to calcification, thrombosis, and immune rejection, impairing valve function, and there is a lack of effective long-term solutions.
The glutaraldehyde cross-linked pericardial valve is surface-grafted with chondroitin sulfate and glycyrrhizic acid. Through amination treatment and amidation reaction, a bionic heart valve material with anti-thrombotic and anti-inflammatory properties is formed, which can be released in response to the inflammatory microenvironment. Glycyrrhizic acid to inhibit inflammation and calcification.
Improves the blood compatibility and endothelialization potential of heart valves, reduces the risk of thrombosis and calcification, extends the service life of the valve, and exerts an anti-inflammatory effect in an inflammatory environment.
Smart Images

Figure CN116763993B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biomedical materials, and in particular relates to a bionic heart valve for drug response release mediated by an inflammatory microenvironment, and a preparation method and use thereof. Background Art
[0002] Valvular heart disease (VHD) is a serious cardiovascular disease that seriously threatens human life and health. 74 million people worldwide suffer from VHD. In recent years, with the aging of the population, the number of VDH patients will further increase. It is estimated that by 2030, the disease will claim the lives of more than 23 million people. However, there is no specific drug to treat VHD.
[0003] Currently, heart valve replacement has become the best option for treating VHD. About 300,000 people undergo valve replacement surgery each year, and this number is expected to reach 1 million by 2050. Bioprosthetic heart valves (BHVs) and mechanical heart valves are the only two types of artificial heart valves currently on the market. BHVs are made of heterogeneous pericardium cross-linked with glutaraldehyde (Glut). Due to their good blood compatibility, hemodynamics, and minimally invasive implantation, BHVs have been widely used. The presence of immunogenicity in heterogeneous tissues is inevitable. Cross-linking of Glut can reduce its immunogenicity to a certain extent, but it cannot be eliminated.
[0004] Clinically, a large number of immune cells, mainly macrophages, and the inflammatory factors and proteolytic enzymes they secrete are observed in the failed BHV degradation area, which means that autoimmune rejection reactions will cause greater damage to the ECM components in the BHV. Macrophages, as important participants in inflammation, can produce calcium-binding proteins and secrete extracellular vesicles that induce mineralization, increasing the risk of BHV calcification. In addition, local inflammation activates the fibrinolytic system, leading to platelet adsorption and causing thrombosis around the implant. Immune infiltration after implantation can lead to the growth of fibrous vascular tissue in the area where the recipient tissue and the prosthesis are in contact with each other. Excessive growth of the extracellular matrix may restrict the movement of the valve leaflets, damage the valve leaflets, and cause leaflet stenosis and valve dysfunction.
[0005] Controlling the immune response near the BHV leaflets helps promote leaflet endothelialization and effectively protect the integrity of the ECM. An intact endothelium can reduce the formation of valve thrombi and the exposure of heterogeneous ECM, thereby reducing the incidence of pathological intimal neoplasia, endocarditis, and early valve calcification. However, studies have shown that aldehydes exist in the form of covalent binding and physical adsorption in Glut-crosslinked BHVs, both of which can impair the activity of endothelial cells. Therefore, when designing new methods for long-lasting heart valves, it is necessary to consider not only how to regulate macrophages to reduce local inflammation and reduce side effects such as calcification and thrombosis induced by immune responses, but also how to promote the repair of the protective physiological barrier of endothelial cells and maintain the integrity of the ECM. Summary of the invention
[0006] In order to solve the problems existing in the prior art, the present invention provides a bionic heart valve for drug response release mediated by an inflammatory microenvironment, and a preparation method and use thereof.
[0007] The invention provides a bionic heart valve material, which is a pericardium with chondroitin sulfate and glycyrrhizic acid grafted on the surface.
[0008] Furthermore, the pericardium is decellularized pericardium after cross-linking with glutaraldehyde;
[0009] Preferably, the pericardium is decellularized porcine pericardium cross-linked with glutaraldehyde.
[0010] Furthermore, the method for preparing the decellularized pericardium after glutaraldehyde cross-linking comprises the following steps:
[0011] 1) Soaking the pericardium in a decellularization solution to perform decellularization to obtain a decellularized pericardium;
[0012] 2) immersing the decellularized pericardium in a glutaraldehyde solution for cross-linking to obtain a glutaraldehyde-cross-linked decellularized pericardium;
[0013] Preferably,
[0014] In step 1), the decellularization solution is a mixed aqueous solution containing 0.5% sodium deoxycholate, 0.5% sodium dodecyl sulfate and 1% penicillin-streptomycin;
[0015] And / or, in step 1), the decellularization temperature is 25 to 40° C., and the decellularization time is 10 to 20 hours;
[0016] And / or, in step 2), the glutaraldehyde solution is an aqueous glutaraldehyde solution;
[0017] And / or, in step 2), the cross-linking temperature is 25 to 40° C., and the cross-linking time is 7 to 10 days;
[0018] More preferably, the concentration of the glutaraldehyde aqueous solution is 0.5-0.7 wt %.
[0019] The present invention also provides a method for preparing the aforementioned bionic heart valve material, which comprises the following steps:
[0020] (1) performing surface amination treatment on the decellularized porcine pericardium after glutaraldehyde cross-linking to obtain surface amination-treated pericardium;
[0021] (2) immersing the aminated pericardium in a solution containing chondroitin sulfate to react, thereby obtaining the pericardium with chondroitin sulfate grafted on the surface;
[0022] (3) immersing the pericardium with chondroitin sulfate grafted on the surface in a solution containing p-aminophenylboronic acid-glycyrrhizic acid to react, thereby obtaining the pericardium with chondroitin sulfate and glycyrrhizic acid grafted on the surface; the p-aminophenylboronic acid-glycyrrhizic acid is prepared from p-aminophenylboronic acid and glycyrrhizic acid as raw materials through an amidation reaction.
[0023] Further,
[0024] In step (1), the amination treatment is performed by immersing the pericardium in a solution containing adipic acid dihydrazide and reacting at 30 to 40° C. for 20 to 30 hours.
[0025] Further,
[0026] In step (1), the solution containing adipic acid dihydrazide further comprises 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide;
[0027] And / or, in step (1), the solvent of the solution is MES buffer, and the pH value of the MES buffer is 4.0 to 7.4;
[0028] And / or, in step (1), the concentration of adipic acid dihydrazide in the solution is 0.02M to 0.15M;
[0029] And / or, in step (2), the reaction temperature is 30 to 40° C., and the reaction time is 20 to 30 hours;
[0030] and / or, in step (2), the solution containing chondroitin sulfate further comprises 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide;
[0031] And / or, in step (2), the solvent of the solution is MES buffer, and the pH value of the MES buffer is 4.0 to 7.4;
[0032] and / or, in step (2), the concentration of the chondroitin sulfate in the solution is 1 to 10 mg / mL;
[0033] Preferably,
[0034] In step (1), the concentration of adipic acid dihydrazide in the solution is 0.05 M;
[0035] And / or, in step (2), the concentration of chondroitin sulfate in the solution is 5-10 mg / mL.
[0036] Further,
[0037] In step (1), the molar ratio of adipic acid dihydrazide, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:(1-4):(1-4);
[0038] And / or, in step (2), the mass ratio of chondroitin sulfate, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:(2-5):(1-4);
[0039] Preferably,
[0040] In step (1), the molar ratio of adipic acid dihydrazide, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:2:2;
[0041] And / or, in step (2), the mass ratio of chondroitin sulfate, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:(3-4):(1-2).
[0042] Further,
[0043] In step (3), the amidation reaction further comprises 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide;
[0044] And / or, in step (3), the solvent for the amidation reaction is N,N-dimethylformamide;
[0045] And / or, in step (3), the temperature of the amidation reaction is 80 to 100° C.; the reaction time is 10 to 20 hours;
[0046] Preferably,
[0047] In step (3), the molar ratio of p-aminophenylboronic acid, glycyrrhizic acid, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:(1-2):(1-4):(1-4);
[0048] More preferably,
[0049] In step (3), the molar ratio of p-aminophenylboronic acid, glycyrrhizic acid, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:1:1.5:1.5.
[0050] Further,
[0051] In step (3), the solvent of the solution containing p-aminophenylboronic acid-glycyrrhizic acid is a mixed solution of N,N-dimethylformamide and anhydrous ethanol;
[0052] And / or, in step (3), the concentration of p-aminophenylboronic acid-glycyrrhizic acid in the solution containing p-aminophenylboronic acid-glycyrrhizic acid is 3 to 10 mg / ml;
[0053] And / or, in step (3), the temperature of the immersion in the solution containing p-aminophenylboronic acid-glycyrrhizic acid is 30 to 40° C. and the time is 1 to 5 hours;
[0054] Preferably,
[0055] In step (3), the volume ratio of N,N-dimethylformamide to anhydrous ethanol is 1:9;
[0056] And / or, in step (3), the concentration of p-aminophenylboronic acid-glycyrrhizic acid in the solution containing p-aminophenylboronic acid-glycyrrhizic acid is 5 mg / ml.
[0057] The present invention also provides the use of the aforementioned bionic heart valve material in preparing an artificial bio-valve;
[0058] Preferably, the artificial bioprosthetic valve is an artificial heart valve, an artificial pulmonary valve or an artificial venous valve.
[0059] The present invention provides a bionic heart valve material. First, amino groups are introduced into the surface of a pig pericardial valve cross-linked with glutaraldehyde using adipic acid hydrazide (ADH), and then chondroitin sulfate (CS) is introduced into the valve surface through an amidation reaction to prepare CS-PP. CS can form an ECM-like structure on the surface, thereby improving the blood compatibility and endothelialization potential of the bionic heart valve material. The present invention also synthesizes PBA-GA through an amidation reaction between p-aminophenylboronic acid (PBA) and glycyrrhizic acid (GA), and prepares CS-GA-PP through a borate bond generated between CS-PP and PBA-GA, ultimately giving the pig pericardial valve good anti-thrombotic ability and endothelialization potential, and can also respond to release GA under an inflammatory microenvironment, ultimately playing a better anti-inflammatory and anti-calcification role. In addition, the CS-GA-PP prepared by the present invention maintains the excellent structural stability and mechanical properties of the pig pericardial valve cross-linked with glutaraldehyde. The present invention provides a new idea and solution for preparing an artificial biological heart valve with better performance, and has a good application prospect.
[0060] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.
[0061] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 The relevant physical and chemical properties of the bionic heart valve GA-CS-PP of the present invention are characterized: A is the quantitative results of platelet adhesion on Glut-PP, CS-PP2.5, CS-PP5 and CS-PP10; B is the quantitative results of PBA-GA 1H-NMR spectrum; C is the infrared spectrum of Glut-PP, CS-PP and CS-GA-PP; D is the release curve of PBA-GA in different PBS solutions; E is the weight loss rate of DPP, Glut-PP, CS-PP and CS-GA-PP after collagenase degradation (n=6); F is the thermal denaturation temperature of Glut-PP, CS-PP and CS-GA-PP (n=3); G is the ultimate tensile strength of Glut-PP, CS-PP and CS-GA-PP (n=5); H is the elongation of Glut-PP, CS-PP and CS-GA-PP (n=5); I is the tangent modulus of Glut-PP, CS-PP and CS-GA-PP (n=5); ns indicates no significant difference, *p<0.05, **p<0.005, ***p<0.001.
[0063] Figure 2 The results of in vitro hematological evaluation of the bionic heart valve GA-CS-PP of the present invention are as follows: A is the fluorescence image of FITC-BSA and FITC-FBG adsorbed on Glut-PP, CS-PP and CS-GA-PP; B is the semi-quantitative fluorescence intensity of Figure A (n=12); C is the relative content of platelets adsorbed on Glut-PP, CS-PP and CS-GA-PP (n=6); D is the SEM image of platelets adsorbed on Glut-PP, CS-PP and CS-GA-PP; E is the SEM image of platelets attached to Glut-PP, CS-PP and CS-GA-PP after AV shunt. A is the visual image of red blood cells on A-PP; F is the SEM image of red blood cells attached to Glut-PP, CS-PP and CS-GA-PP after AV shunt; G is the semi-quantitative analysis of red blood cells attached to Glut-PP, CS-PP and CS-GA-PP after AV shunt (n=5); H is the visual image of hemolysis of Glut-PP, CS-PP and CS-GA-PP (PC is the positive control, NC is the negative control); I is the hemolysis rate of Glut-PP, CS-PP and CS-GA-PP (n=5); ns indicates no significant difference, ***p<0.001.
[0064] Figure 3The in vitro cell evaluation results of the bionic heart valve GA-CS-PP of the present invention: A is the viability of L929 cells after being cultured in Glut-PP, CS-PP and CS-GA-PP extracts for 1 day and 3 days (n=6); B is the relative fluorescence intensity of HUVECs after being cultured in Glut-PP, CS-PP and CS-GA-PP for 1 day and 3 days (n=8); C is the fluorescence image of HUVECs after being cultured in Glut-PP, CS-PP and CS-GA-PP for 1 day and 3 days; D is the relative proliferation rate of HUVECs after being cultured in Glut-PP, CS-PP and CS-GA-PP for 1 day and 3 days (n=8); E is the concentration of VEGF secreted by HUVECs cultured on Glut-PP, CS-PP and CS-GA-PP (n=8); ns indicates no significant difference, *p<0.05, **p<0.005, ***p<0.001.
[0065] Figure 4 The evaluation results of the anti-inflammatory property of the bionic heart valve GA-CS-PP of the present invention are as follows: A is the concentration of IL-10 secreted by RAW 264.7 cultured with Glut-PP, CS-PP and CS-GA-PP (n=6); B is the concentration of IL-6 secreted by RAW 264.7 cultured with Glut-PP, CS-PP and CS-GA-PP (n=6); C is the HE staining of Glut-PP, CS-PP and CS-GA-PP after subcutaneous implantation in rats for 7d and 14d.
[0066] Figure 5 The in vivo anti-inflammatory performance evaluation results of the bionic heart valve GA-CS-PP of the present invention: A is the iNOS immunofluorescence staining of Glut-PP, CS-PP and CS-GA-PP after subcutaneous implantation in rats for 7 days and 14 days; B is the CD206 immunofluorescence staining of Glut-PP, CS-PP and CS-GA-PP after subcutaneous implantation in rats for 7 days and 14 days; C is the relative fluorescence intensity of iNOS (n=12); D is the relative fluorescence intensity of CD206 (n=12); ns indicates no significant difference, *p<0.05, **p<0.005, ***p<0.001.
[0067] Figure 6 In vivo calcification analysis of the bionic heart valve GA-CS-PP of the present invention: A is a macroscopic image of calcification of Glut-PP, CS-PP and CS-GA-PP after subcutaneous implantation in rats for 30 days and 60 days; B is Alizarin red staining of Glut-PP, CS-PP and CS-GA-PP after subcutaneous implantation in rats for 30 days and 60 days. DETAILED DESCRIPTION
[0068] The raw materials and equipment used in the specific embodiments of the present invention are all known products and are obtained by purchasing commercially available products.
[0069] Materials: Fresh porcine pericardium (PP) was obtained from Venus Medtech Inc (Hangzhou, China); N,N-dimethylformamide (DMF) was purchased from Chengdu Best Reagent Co., Ltd. (Chengdu, China); n-hydroxysuccinimide (NHS), 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride (EDCHCl), 2-(N-morpholino)ethanesulfonic acid monohydrate (MES monohydrate), adipic acid dihydrazide (ADH), chondroitin sulfate (CS), p-aminophenylboronic acid (PBA), and glycyrrhizic acid (GA) were purchased from Macklin Biochemical Co., Ltd. (Shanghai, China); lipopolysaccharide (LPS) was purchased from Sigma Aldrich (Shanghai, China); fetal bovine serum (FBS), phosphate-buffered saline (PBS), and DMEM medium were purchased from Gibco (Thermo Fisher Scientific, USA); human VEGF ELISA kits and collagenase were purchased from Solarbio Life Sciences Co., Ltd. (Beijing, China); cell counting kit-8 (CCK-8) was purchased from Yongtai Biotechnology Co., Ltd. (Shanghai, China).
[0070] Statistical analysis in the specific embodiments of the present invention: Each data was obtained from three independent repeated experiments and calculated from at least three parallel samples. All results were calculated using mean ± standard deviation. In the experiment, t-test and univariate analysis were used to indicate significant differences between groups. p<0.05 was considered statistically significant. *p<0.05; **p<0.01; ***p<0.001.
[0071] Example 1: Preparation of the bionic heart valve of the present invention
[0072] 1. Synthesis of PBA-GA
[0073] PBA (136.94 mg, 1 mmol), GA (470.69 mg, 1 mmol), EDCHCl (287.55 mg, 1.5 mmol) and NHS (172.64 mg, 1.5 mmol) were added to 10 mL DMF, reacted at 80°C overnight, and terminated in an ice-water bath. DMF was removed by a rotary evaporator, the product was washed 3 times with ultrapure water (UW), freeze-dried, and finally PBA-GA was prepared by amidation reaction.
[0074] use 1 H-NMR was used to characterize PBA-GA. Figure 1 As shown in B: According to H 1-NMR (400MHz,CDCl3),δ=7.85(s,2H),7.64(s,2H), indicating that PBA-GA was successfully synthesized.
[0075] 2. Preparation of CS-PP
[0076] Preparation of decellularized porcine pericardium (DPP): Fresh porcine pericardium (provided by Hangzhou Venus Medical Device Co., Ltd., kept in ice bath conditions during transportation) was washed three times with saline, and the connective tissue visible to the naked eye was removed with tweezers. The fresh porcine pericardium was then soaked in a mixed aqueous solution containing 0.5% sodium deoxycholate, 0.5% sodium dodecyl sulfate, and 1% penicillin-streptomycin. After continuous shaking reaction on a shaker at room temperature overnight, impurities such as cell debris were washed away with saline to obtain decellularized porcine pericardium (DPP), which was stored in a 4C refrigerator.
[0077] Preparation of glutaraldehyde cross-linked porcine pericardium (Glut-PP): The decellularized porcine pericardium was cut into 110 mm x 110 mm size and fixed on a square iron frame to prevent shrinkage. Then, the decellularized porcine pericardium was placed in a 0.625% (wt%) glutaraldehyde aqueous solution and continuously shaken at 100 rpm at room temperature for 7 days to obtain glutaraldehyde cross-linked porcine pericardium (Glut-PP).
[0078] Amination of Glut-PP: Add ADH (0.871 g, 5 mmol), EDCHCl (1.917 g, 10 mmol), and NHS (0.5755 g, 10 mmol) to 100 mL of MES buffer (pH = 4.9), soak Glut-PP in the above solution, and react at 37°C for 24 hours to obtain surface-aminated Glut-PP (ADH-PP).
[0079] Preparation of CS-PP: The reagents and amounts used are shown in Table 1. The reagents were dissolved in 100 mL of MES buffer (pH = 4.9) according to the amounts in Table 1, and ADH-PP was immersed in the solution and reacted at 37°C for 24 hours to obtain CS-PP2.5, CS-PP5, and CS-PP10, respectively.
[0080] Table 1. Reagents and amounts used in the preparation of CS-PP
[0081]
[0082] Platelet adsorption of CS-PP: Whole blood was drawn from the ear vein of rabbits and placed in a sodium citrate blood collection tube, then centrifuged at 1500 rpm for 20 minutes, and platelet-rich plasma (PRP) was collected from the upper layer. Glut-PP, CS-PP2.5, CS-PP5, and CS-PP10 (n=6) were placed on a 96-well plate and washed three times with PBS. 100 μL of PRP was added to the wells and incubated at 37°C for 1 hour. The samples were thoroughly washed with PBS, and the relative content of platelets adsorbed on each PPs was detected using an LDH kit.
[0083] The quantitative results of platelet adhesion on Glut-PP, CS-PP2.5, CS-PP5 and CS-PP10 are shown in Figure 1 As shown in A, Figure 1 A: After CS is introduced into PP, the adsorption of platelets on PP can be effectively reduced. There is almost no difference in the number of platelets adsorbed on the surface of CS-PP5 and CS-PP10. That is, when the CS concentration reaches 5 mg / mL, the increase in CS concentration does not enhance the anti-platelet adsorption level of the material. Therefore, CS-PP5 was selected for further study.
[0084] 3. Preparation of CS-GA-PP
[0085] 0.5 g of PBA-GA was dissolved in 10 mL of DMF, and 90 mL of anhydrous ethanol was added to the solution. CS-PP (CS-PP2.5, CS-PP5 and CS-PP10) were immersed in the solution and reacted at 37°C. After reacting for 2 hours, the material was taken out and rinsed with anhydrous ethanol to remove the unbound PBA-GA, thereby obtaining the bionic heart valve CS-GA-PP (bhv) of the present invention. The CS-GA-PP prepared using CS-PP2.5, CS-PP5 and CS-PP10 were named CS-GA-PP2.5, CS-GA-PP5 and CS-GA-PP10, respectively.
[0086] Fourier transform infrared spectroscopy (FTIR) characterization: Glut-PP, CS-PP (CS-PP5) and CS-GA-PP (CS-GA-PP5) were washed with ultrapure water (UW), compressed with cover glass, freeze-dried, and the infrared spectrum was scanned with an infrared spectrometer. The scanning wavelength range was set at 500 cm -1 ~4000cm -1 between.
[0087] The infrared spectrum results are as follows Figure 1 C: CS-PP at 1750cm -1 and 3448cm -1There are vibration peaks at 2854 cm-1, which are attributed to the secondary amino group (NH) and the primary amino group (NH)2. -1 and 1737cm -1 A vibration peak appeared at , which was attributed to the carboxyl group (COOH). FTIR results showed that CS-GA-PP was successfully prepared.
[0088] The beneficial effects of the present invention are demonstrated below through specific test examples.
[0089] In the following test examples, unless otherwise specified: CS-PP is CS-PP5 prepared in Example 1, and CS-GA-PP is CS-GA-PP5 prepared in Example 1; and the samples in the same test example have the same size.
[0090] Test Example 1: Release test of PBA-GA in CS-GA-PP
[0091] 1. Experimental methods
[0092] Preparation of PBA-GA concentration standard curve: PBA-GA prepared in Example 1 was dissolved in DMF and diluted to concentrations of 1000, 500, 250, 125, 62.5, 31.25, 16.625, 8.3125, and 0 μg / mL. The absorbance values of these solutions were measured at 267 nm using a UV-3200 spectrophotometer, and the standard concentration curve of PBA-GA was obtained based on the one-to-one correspondence between the absorbance value and the concentration value.
[0093] CS-GA-PP (5cm×5cm, n=4) was immersed in 30ml of the following four solutions: (1) PBS (pH=7.0, abbreviated as pH 7.0); (2) PBS (pH=5.0, pH adjusted by adding hydrochloric acid, abbreviated as pH 5.0); (3) PBS (pH=7.0, containing 10mM H2O2, abbreviated as H2O2); (4) PBS (pH=5.0, containing 10mM H2O2, abbreviated as pH 5.0+H2O2). The above four solutions were placed on a shaker at 37°C and shaken slowly. After immersion for 0, 2, 4, 6, 8, 10, 12, and 24 hours, 3ml of solution was taken from each group and the absorbance value at 267nm was measured. The concentration of PBA-GA at different time points was obtained by the standard concentration curve, and a drug release scatter plot was made to study the release of PBA-GA.
[0094] 2. Experimental results
[0095] The release curves of PBA-GA in different PBS solutions are shown in Figure 1As shown in D: The release curve of PBA-GA shows that under acidic (PBS, pH = 5.0) or high ROS (PBS containing H2O2) conditions, the release amount of PBA-GA is higher than that of normal PBS (pH = 7.0), and the release amount is the highest in an acidic and high ROS environment (PBS pH = 5.0, containing H2O2), and the release time of PBA-GA lasts for more than 24 hours.
[0096] PBA-GA is introduced into the BHV of the present invention through a boronate bond. The experimental results show that the simulated inflammatory microenvironment can lead to the breakage of the boronate bond and the release of GA. The ROS level at the inflammatory site is much higher than the normal level, and the pH value is lower than the normal level, so GA can be released to exert its anti-inflammatory effect, thereby inhibiting the damage of inflammation to the surrounding tissues. At the same time, the release time of GA can last for more than 24 hours, achieving the purpose of sustained release.
[0097] Test Example 2: Collagenase degradation test of the bionic heart valve of the present invention
[0098] 1. Experimental methods
[0099] The decellularized PP (DPP) in Example 1 and the Glut-PP, CS-PP, and CS-GA-PP (1 cm×1 cm, n=6) prepared in Example 1 were freeze-dried and weighed, and the mass was recorded as w0. The above samples were immersed in a Tris buffer containing 125 U / mL collagenase (0.1 M, CaCl2 0.05 M, pH=7.4) and incubated at 37°C for 24 hours. These treated samples were washed three times with UW, freeze-dried, and weighed again, and the mass was recorded as w1. The weight loss rate of the sample was calculated by the following formula:
[0100]
[0101] 2. Experimental results
[0102] As the main component of the BHV material of the present invention, the stability of collagen is crucial to maintaining the durability of the BHV. Ensuring the stability of collagen in the BHV is one of the purposes of this study. Collagen is mainly decomposed by collagenase in the body, and simulating collagenase digestion is a direct method to evaluate collagen stability.
[0103] The weight loss results of DPP, Glut-PP, CS-PP and CS-GA-PP after collagenase degradation are as follows Figure 1 As shown in E, Figure 1E shows that the weight loss rate of PP (Glut-PP, CS-PP and CS-GA-PP) after glutaraldehyde cross-linking after 24 hours of degradation is significantly lower than that of DPP. The weight loss rates of Glut-PP, CS-PP and CS-GA-PP are all close to 5%, while the weight loss rate of DPP is as high as 85%. This shows that glutaraldehyde cross-linking is crucial to maintaining the stability of collagen, and CS and GA modification of PP will not destroy the stability after glutaraldehyde cross-linking, which ensures the stability of the heart valve in vivo.
[0104] Test Example 3: Thermal Denaturation Temperature Test of the Bionic Heart Valve of the Present Invention
[0105] 1. Experimental methods
[0106] Glut-PP, CS-PP and CS-GA-PP (1 cm×1 cm, n=3) prepared in Example 1 were placed in a crucible. The crucible was placed in a differential calorimeter scanner (TA Instruments, Newcastle, DE). The temperature was increased from 50°C to 100°C. The temperature corresponding to the position where the highest value appeared during the heating process was the thermal denaturation temperature of the sample.
[0107] 2. Experimental results
[0108] Thermal denaturation temperature can also reflect the stability of collagen to a certain extent. Figure 1 As shown in F: The thermal denaturation temperatures of CS-PP and CS-GA-PP are not different from those of Glut-PP, which further indicates that the introduction of CS and GA will not destroy the stability of PP after glutaraldehyde cross-linking.
[0109] Test Example 4: Uniaxial tensile test of the bionic heart valve of the present invention
[0110] 1. Experimental methods
[0111] Glut-PP, CS-PP and CS-GA-PP (1 cm × 5 cm, n = 5) prepared in Example 1 were soaked in PBS (pH = 7.4), and the thickness of the samples at three different positions was measured with a thickness gauge. These samples were fixed on a sample holder, and the initial distances at both ends of the sample holder were 2 cm. During the test, the sample was stretched at a speed of 18 mm per minute until it broke. The final tangent modulus, tensile strength and elongation were calculated according to the method described in the literature (F. Yang, H. He, L. Xu, L. Jin, G. Guo, Y. Wang, Inorganic-polymerization crosslinked tissue-siloxane hybrid as potential biomaterial for bioprosthetic heart valves, J Biomed Mater Res A 109 (5) (2021) 754-765.).
[0112] 2. Experimental results
[0113] Under physiological blood pressure conditions, the aortic valve is subjected to high pressure differentials, with a maximum pressure differential of up to 100 mm Hg. Studies have reported that the native aortic valve is highly anisotropic and much stiffer in the circumferential direction than in the radial direction. When the natural leaflet is subjected to external stress, elastin initially bears the load, while collagen remains curled. As the leaflet further expands, the load is transferred from elastin to the uncoiled collagen.
[0114] The mechanical properties of Glut-PP, CS-PP and CS-GA-PP samples were tested by uniaxial tensile test. Due to the anisotropy of porcine pericardium, the samples were fixed in the direction consistent with the collagen fibers. The tangent modulus represents the softness of the collagen fibers, the ultimate tensile strength represents the maximum load that the bionic heart valve material (BHV) can withstand, and the elongation is related to the cross-linking degree of the BHV material. The results are shown in Figure 1 As shown in Figures 1G, 1H and 1I: the tangent modulus and ultimate tensile strength of Glut-PP are 81.21MPa and 15.07MPa, respectively, the tangent modulus and ultimate tensile strength of CS-GA-PP are 79.34MPa and 15.23MPa, respectively, and the elongation of Glut-PP and CS-GA-PP are 9.25% and 10.30%, respectively. The results of the uniaxial tensile test show that there is no significant difference in mechanical properties between Glut-PP and CS-GA-PP. From the above results, it can be found that the cross-linking of Glut is crucial to maintaining the stability and mechanical properties of collagen in the bionic heart valve, while the introduction of GA and CS maintains the advantages of Glut-PP stability and mechanical properties.
[0115] Test Example 5: Protein adsorption test of the bionic heart valve of the present invention
[0116] 1. Experimental methods
[0117] Glut-PP, CS-PP, and CS-GA-PP (1 cm × 1 cm, n = 12) prepared in Example 1 were placed in a 48-well plate, washed three times with PBS, and 200 μL of fluorescein isothiocyanate-labeled bovine serum albumin (FITC-BSA) (1 mg / mL) or fluorescein isothiocyanate-labeled human fibrinogen (FITC-FBG) (0.1 mg / mL) were added respectively. The plates were incubated at 37°C. After incubation for 2 hours, the samples were thoroughly washed with PBS to remove unadsorbed proteins. The proteins adsorbed on the samples were observed and photographed using a laser confocal microscope (Zeiss LSM 800, DE).
[0118] 2. Experimental results
[0119] Good blood compatibility is a necessary condition to ensure the long-term effectiveness of BHV. After implantation in the body, plasma proteins in the blood will be adsorbed to the surface of materials with poor blood compatibility. In vitro resistance to protein adsorption is essential for BHV indicators to achieve good blood compatibility. FITC-BSA and FITC-FBG were incubated on the surface of BHV materials to evaluate the in vitro anti-protein adsorption effect of CS-GA-PP. The results are shown in Figure 2 As shown in A and 2B: The fluorescence of Glut-PP is significantly stronger than that of CS-PP and CS-GA-PP, indicating that the introduction of CS and GA improves the anti-protein adsorption performance of BHV materials in vitro.
[0120] Test Example 6: Platelet Adsorption Test of the Bionic Heart Valve of the Present Invention
[0121] 1. Experimental methods
[0122] Whole blood was drawn from the rabbit's ear vein, placed in a sodium citrate blood collection tube, and then centrifuged at 1500 rpm for 20 minutes to collect platelet-rich plasma (PRP) from the upper layer. Glut-PP, CS-PP and CS-GA-PP (1 cm × 1 cm, n = 6) prepared in Example 1 were placed on a 48-well plate and washed three times with PBS. 100 μL of PRP was added to the plate wells and incubated at 37°C for 1 hour. The samples were thoroughly washed with PBS and the relative content of platelets adsorbed on PPs was detected using an LDH kit.
[0123] In addition, the sample after platelet adsorption was treated with 2.5% (w / v) paraformaldehyde for 1 hour and then dehydrated with graded ethanol solutions. Platelet images were obtained by scanning electron microscopy (SEM).
[0124] 2. Experimental results
[0125] Leaflet thrombosis is also a common cause of BHV failure. Coagulation is closely related to platelet adsorption and aggregation. Once platelets are adsorbed to the surface of a substance, they are activated. Activated platelets increase viscosity, activate the endogenous coagulation system, and lead to thrombosis. The anti-platelet adsorption properties of BHV were studied through in vitro platelet adsorption experiments. The platelets adsorbed by BHV materials were detected using the LDH kit. The results showed that the OD value of Glut-PP was significantly higher than that of CS-PP and CS-GA-PP ( Figure 2 C). SEM images show that many platelets are adsorbed on the surface of Glut-PP, while there are fewer platelets on the surfaces of CS-PP and CS-GA-PP ( Figure 2 D). Platelet adsorption experiments showed that the combined modification strategy of CS and GA significantly improved the anti-platelet adsorption performance of BHV materials.
[0126] Test Example 7: Hemolysis Test of the Bionic Heart Valve of the Present Invention
[0127] 1. Experimental methods
[0128] Whole blood was drawn from the rabbit's ear vein, placed in a sodium citrate blood collection tube, and then centrifuged at 1500rpm for 20 minutes, and the lower layer of red blood cells was collected and diluted with PBS (the volume ratio of red blood cells to PBS was 1:9). Glut-PP, CS-PP and CS-GA-PP (1cm×1cm, h=1cm, n=5) prepared in Example 1 were washed with PBS and placed in 2ml centrifuge tubes. 200μL of diluted red blood cells and 800μL of PBS were added to the centrifuge tubes containing the samples. Deionized water and PBS were used as positive and negative controls, respectively. These centrifuge tubes were placed in a 37°C incubator. After incubation for 2 hours, the supernatant was transferred to a 0.5mL centrifuge tube and centrifuged at 3000rpm for 5 minutes. The absorbance value (OD) of hemoglobin was measured at 541nm using a microplate reader (Synergy, Bio-Tek).
[0129] 2. Experimental results
[0130] Implantable blood-contacting medical devices have very high requirements for hemolysis rate. Once a hemolysis event occurs, it will cause significant damage to organs and even endanger life. The hemolysis rates of the three samples of the present invention are all lower than the industry standard of less than 2% ( Figure 2 H and 2I). This indicates that the BHV material prepared by the present invention has good blood compatibility.
[0131] Test Example 8: Extracorporeal arteriovenous shunt test of the bionic heart valve of the present invention
[0132] 1. Experimental methods
[0133] Animal experiments have been authorized by the Medical Ethics Committee of Sichuan University (Ethics Approval No.: 20230314005). Before the experiment, samples of Glut-PP, CS-PP, and CS-GA-PP (1 cm × 1 cm, n = 5) were attached to the inner wall of the catheter and photographed. The experimental rabbits (New Zealand rabbits, 2.1 kg) were anesthetized with 1% sodium pentobarbital (30 mg / kg). Before the operation, the rabbits were intravenously injected with heparin anticoagulation (300 U / kg) under anesthesia. One end of the catheter was connected to the cervical artery of the rabbit, and the other end was connected to the contralateral external jugular vein. The arterial and venous circulation was established through the catheter, so that the blood flow was in contact with the sample in the catheter. After 1 hour of blood flow, the sample was removed from the catheter and washed with PBS to remove uncoagulated blood. The sample was fixed with 2.5% (w / v) Glut saline for 1 hour and dehydrated with gradient ethanol. The dehydrated sample was observed and photographed by scanning electron microscopy. The sample was dehydrated with gradient ethanol for 1 hour. The dehydrated sample was observed and photographed by scanning electron microscopy.
[0134] 2. Experimental results
[0135] The antithrombotic properties of CS-GA-PP under dynamic blood flow conditions were studied by AV shunt experiments. Slight thrombosis occurred on Glut-PP after 1 hour of circulation, while almost no blood components were adsorbed on CS-PP and CS-GA-PP ( Figure 2 E). SEM observation and semi-quantitative analysis showed that the surface of Glut-PP was covered with dense red blood cells, while the red blood cells on the surfaces of CS-PP and CS-GA-PP were relatively few ( Figure 2 F and 2G).
[0136] The results of Experimental Examples 5 to 8 show that the introduction of CS can effectively reduce the adsorption of proteins and platelets in blood circulation, significantly improve the anti-thrombotic properties and blood compatibility of BHV materials, and GA has no negative impact on the excellent blood compatibility of CS-PP.
[0137] Test Example 9: In vitro cytotoxicity evaluation of the bionic heart valve of the present invention
[0138] 1. Experimental methods
[0139] Glut-PP, CS-PP and CS-GA-PP (1 cm×1 cm, n=6) prepared in Example 1 were sterilized with 75% ethanol overnight and the remaining ethanol was washed off with sterile PBS. These samples were immersed in complete DMEM (5 ml, pH 5.0 and 0.2 mM H2O 2) The cells were placed in a carbon dioxide incubator (5% CO2, 37°C) for 72 hours to obtain sample extracts for cytotoxicity testing.
[0140] Mouse fibroblast (L929) cells (containing 10,000 cells) were inoculated in a 96-well plate and incubated for 12 hours. After incubation, 200 μL of the extract was used to replace the original complete culture medium and cultured for 24 and 72 hours, respectively. Cells cultured in DMEM were selected as controls. After the culture was completed, the culture medium was discarded and the viability of L929 cells was detected using CCK-8.
[0141] 2. Experimental results
[0142] The experimental results are as follows Figure 3 As shown in A: After culturing in CS-PP and CS-GA-PP extracts for 1 day and 3 days, the survival rate of L929 cells reached 90%, while the survival rate of cells cultured in Glut-PP extract was only 30%, which was significantly lower than that of CS-PP and CS-GA-PP. The results showed that CS-PP and CS-GA-PP extracts had no cytotoxicity to L929 cells, and the introduction of CS and GA reduced the cytotoxicity of Glut-PP.
[0143] Test Example 10: In vitro proliferation test of human umbilical vein endothelial cells (HUVECs) of the bionic heart valve of the present invention
[0144] 1. Experimental methods
[0145] Glut-PP, CS-PP and CS-GA-PP (φ = 1 cm, n = 8) prepared in Example 1 were sterilized in 75% ethanol for 12 hours and thoroughly washed with PBS. These samples were placed in a 48-well plate and compressed with a stainless steel ring (outer diameter = 8 mm) to prevent curling. 20,000 HUVECs were inoculated into the wells in 500 μL DMEM (5 mL, pH 5.0, 0.2 mM H2O2) and incubated in a carbon dioxide cell culture incubator for 1 and 3 days. After incubation, the culture medium was replaced with 10% CCK-8 reagent. After incubation in a carbon dioxide cell culture incubator for 1 hour, the absorbance value was detected at 450 nm, and the relative proliferation rate (RPR) of HUVECs was calculated. In addition, the living cells were stained with 0.1% diacetate fluorescein (FDA). After staining for 1 minute, live cell images were obtained by fluorescence microscopy. In addition, the concentration of VEGF secreted by HUVECs after 3 days of incubation was determined using an ELISA kit.
[0146] 2. Experimental results
[0147] Endothelialization of BHV materials is an effective method to resist nonspecific protein adsorption, improve blood compatibility, and maintain long-term therapeutic effects. The in vitro endothelialization of CS-GA-PP was evaluated by the proliferation of HUVECs on the surface. The CCK8 kit was used to quantitatively analyze the relative proliferation rate of HUVECs cultured on the surface of BHV materials for 1 day and 3 days. Fluorescence microscopy observation and semi-quantitative analysis showed that compared with Glut-PP, there were more HUVECs on the surface of CS-PP and CS-GA-PP ( Figure 3 B and 3C).
[0148] In addition, the present invention further evaluated the relative proliferation rate of HUVECs on different material surfaces. The relative proliferation rate of HUVECs on the CS-PP surface (42.59% on the first day and 52.96% on the third day) and the CS-GA-PP surface (50.35% on the first day and 53.38% on the third day) were higher than those on the Glut-PP surface (23.36% on the first day and 18.87% on the third day) ( Figure 3 D). As time goes by, the relative proliferation rate of HUVECs on the CS-GA-PP surface increases, while the relative proliferation rate on the Glut-PP surface decreases. This is due to the toxic effect of Glut on cells, leading to cell apoptosis. The results show that CS-GA-PP can promote endothelialization.
[0149] VEGF is a cytokine secreted by vascular endothelial cells, and its content can well reflect the proliferation state of endothelial cells. The culture supernatant of HUVECs cultured for 3 days was collected, and the VEGF content was detected by ELISA kit. The concentrations of VEGF secreted by HUVECs cultured on CS-PP and CS-GA-PP were 1174.26pg / mL and 1164.26pg / mL, respectively, indicating that HUVECs maintained an active proliferation state. In contrast, the concentration of VEGF secreted by HUVECs cultured on Glut-PP was 63.92pg / mL ( Figure 3 E).
[0150] It can be seen from Experimental Examples 9 to 10 that the biomimetic modification of the present invention improves the cell compatibility and in vitro endothelialization potential of the BHV material.
[0151] Test Example 11: In vitro inflammation test of the bionic heart valve of the present invention
[0152] 1. Experimental methods
[0153] Mouse mononuclear macrophages (RAW 264.7) were used for in vitro inflammation analysis. Glut-PP, CS-PP and CS-GA-PP (φ=1cm, n=6) prepared in Example 1 were disinfected with 75% ethanol overnight, and the residual ethanol was washed off with sterile PBS. The sample was placed in a 48-well plate and 500 μL of suspension (containing 20,000 cells) was added. The 48-well plate was incubated in a carbon dioxide cell culture incubator for 12 hours. After the cells were completely attached, the filtered lipopolysaccharide (LPS) solution was added to the culture medium to activate RAW 264.7, and the concentration of the LPS solution was 1 μg / mL. After incubation for 1 hour, the solution was replaced with DMEM (5 mL, pH 5.0 and 2.0 mM H2O2) and incubated in a carbon dioxide cell culture incubator for 48 hours. After incubation, the culture supernatant was collected and the concentrations of IL-6 and IL-10 were detected using an ELISA kit.
[0154] 2. Experimental results
[0155] The present invention inoculates LPS-activated macrophages on the surface of BHV materials to determine the anti-inflammatory effect of CS-GA-PP. Once activated, macrophages can differentiate into different types and secrete various inflammatory factors. In general, the inflammatory factors secreted by macrophages mainly include two types: promoting inflammation, such as IL-6, or inhibiting inflammation, such as IL-10. After 2 days of culture, RAW264.7 cell supernatants were collected and ELISA kits were used to detect IL-6 and IL-10 concentrations.
[0156] like Figure 4 As shown in A and 4B: the IL-10 concentrations secreted by macrophages cultured with Glut-PP, CS-PP and CS-GA-PP materials were 33.41pg / mL, 73.00pg / mL and 130.25pg / mL, respectively, and the IL-6 concentrations were 215.45pg / mL, 67.83pg / mL and 23.55pg / mL, respectively. The results show that the anti-inflammatory level of the bhv material of the present invention has been significantly improved. Among them, CS-GA-PP has the best anti-inflammatory level.
[0157] Test Example 12: In vivo inflammation test of the bionic heart valve of the present invention
[0158] 1. Experimental methods
[0159] The animal experiment has been approved by the Medical Ethics Committee of Sichuan University (Ethics Approval No.: 20230314005). Glut-PP, CS-PP, and CS-GA-PP (1 cm × 1 cm, n = 12) prepared in Example 1 were sterilized and stored in sterile PBS. Male SD rats (50 g ± 5 g) were selected as experimental animals. Rats were anesthetized by intraperitoneal injection of 4% sodium pentobarbital (10 mL / kg). Four 1 cm incisions were made on the back of the rat with a surgical blade, and the samples were implanted subcutaneously through the incisions. After 7 and 14 days of subcutaneous implantation, the samples were removed together with the surrounding tissues, fixed with 4% paraformaldehyde fixative, and embedded in paraffin. 5 μm sections were prepared for histological analysis. Immunofluorescence staining was performed to further evaluate the in vivo immune response. M2 macrophages and M1 macrophages were labeled with mouse anti-rat CD206 antibodies and rabbit anti-rat iNOS antibodies, respectively. Fluorescence images were obtained using a laser confocal microscope.
[0160] 2. Experimental results
[0161] To further verify the anti-inflammatory effect of CS-GA-PP in vivo, samples were collected on the 7th and 14th days after implantation. HE staining results showed that Glut-PP had a large number of inflammatory cell infiltration, while CS-GA-PP had significantly less inflammatory cell infiltration ( Figure 4 C).
[0162] In addition, anti-iNOS and anti-CD206 fluorescent staining were also performed. iNOS and CD206 are markers of M1 and M2 macrophages, respectively. In the early stages of tissue inflammation, M1 macrophages appear, recruiting inflammatory cells to fight pathogens and secreting pro-inflammatory factors to accelerate the development of inflammatory responses and cause inflammatory damage to tissues. As inflammation progresses, M1 macrophages gradually retreat and M2 macrophages increase. The latter play a key role in inhibiting inflammation in the later stages of inflammation to avoid damage to self-tissues due to excessive immune responses. The results showed that on the 7th and 14th days, CS-GA-PP had less iNOS than CS-PP and Glut-PP, proving that it caused the least inflammation, while the expression of CD206, CS-GA-PP and CS-PP compared to Glut-PP, increased, which further illustrates that CS-GA-PP can better inhibit the occurrence of inflammatory responses ( Figure 5 A-5D).
[0163] Test Example 13: In vivo calcification test of the bionic heart valve of the present invention
[0164] 1. Experimental methods
[0165] The samples were taken out 30 and 60 days after implantation according to the method described in Experimental Example 12, and some of the samples were cut into 5 μm sections for alizarin red staining.
[0166] 2. Experimental results
[0167] After subcutaneous implantation in rats, the anti-calcification properties of the samples were measured. Figure 6 As shown in A: Glut-PP has uneven calcification on the surface, while CS-GA-PP has a smooth surface without any calcification. The results of Alizarin red staining of sections at 30 days and 60 days ( Figure 6 B) It can be seen that a large red plaque appears on Glut-PP, indicating that Glut-PP calcifies after 30 days of implantation. After 60 days of implantation, Glut-PP almost completely turns red, and is accompanied by structural damage, indicating that the calcification of Glut-PP will further intensify over time. At the same time, CS-PP also appeared a little red after 60 days of implantation, indicating that CS-PP caused calcification at 60 days. Even at 60 days, CS-GA-PP can ensure the integrity of the valve structure and no obvious calcification spots appear, indicating that CS-GA-PP can significantly reduce the tendency of calcification compared with CS-PP and Glut-PP. The above results show that CS-GA-PP significantly improves the anti-calcification performance of BHV materials, and the effect is better than Glut-PP and CS-PP.
[0168] In summary, the present invention provides a bionic heart valve material, firstly using adipic acid dihydrazide (ADH) to introduce amino groups to the surface of the pig pericardial valve cross-linked by glutaraldehyde, and then introducing chondroitin sulfate (CS) to the valve surface by amidation reaction to prepare CS-PP, CS can form a structure similar to ECM on the surface, and improve the blood compatibility and endothelialization potential of the bionic heart valve material. The present invention also synthesizes PBA-GA by an amidation reaction between p-aminophenylboronic acid (PBA) and glycyrrhizic acid (GA), and prepares CS-GA-PP by the borate bond generated between CS-PP and PBA-GA, which ultimately gives the pig pericardial valve good anti-thrombotic ability and endothelialization potential, and can also respond to release GA under an inflammatory microenvironment, and finally play a better anti-inflammatory and anti-calcification effect. In addition, the CS-GA-PP prepared by the present invention maintains the excellent structural stability and mechanical properties of the pig pericardial valve cross-linked by glutaraldehyde. The present invention provides new ideas and solutions for preparing artificial biological heart valves with better performance, and has good application prospects.
Claims
1. A bionic heart valve material, characterized in that: The bionic heart valve material is a pericardium with chondroitin sulfate and glycyrrhizic acid grafted on the surface, specifically, the pericardium with chondroitin sulfate grafted on the surface is immersed in a solution containing p-aminophenylboronic acid-glycyrrhizic acid to react, thereby obtaining the pericardium with chondroitin sulfate and glycyrrhizic acid grafted on the surface; the pericardium is a decellularized pericardium cross-linked with glutaraldehyde.
2. The bionic heart valve material according to claim 1, characterized in that: The pericardium is decellularized porcine pericardium cross-linked with glutaraldehyde.
3. The bionic heart valve material according to claim 1, characterized in that: The method for preparing the decellularized pericardium after glutaraldehyde cross-linking comprises the following steps: 1) Soaking the pericardium in a decellularization solution to perform decellularization to obtain a decellularized pericardium; 2) Immersing the decellular pericardium in a glutaraldehyde solution for cross-linking to obtain a glutaraldehyde-cross-linked decellular pericardium.
4. The bionic heart valve material according to claim 3, characterized in that: In step 1), the decellularization solution is a mixed aqueous solution containing 0.5% sodium deoxycholate, 0.5% sodium dodecyl sulfate and 1% penicillin-streptomycin; And / or, in step 1), the decellularization temperature is 25-40° C., and the decellularization time is 10-20 hours; And / or, in step 2), the glutaraldehyde solution is an aqueous glutaraldehyde solution; And / or, in step 2), the cross-linking temperature is 25-40° C., and the cross-linking time is 7-10 days.
5. The bionic heart valve material according to claim 4, characterized in that: The concentration of the glutaraldehyde aqueous solution is 0.5-0.7 wt %.
6. A method for preparing the bionic heart valve material according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: (1) The surface of the decellularized porcine pericardium after glutaraldehyde cross-linking is subjected to an amination treatment to obtain a surface-amino-treated pericardium; (2) immersing the surface-amino-modified pericardium in a solution containing chondroitin sulfate to react, thereby obtaining a pericardium with chondroitin sulfate grafted on the surface; (3) immersing the pericardium with chondroitin sulfate grafted on the surface in a solution containing p-aminophenylboronic acid-glycyrrhizic acid to react, thereby obtaining the pericardium with chondroitin sulfate and glycyrrhizic acid grafted on the surface; the p-aminophenylboronic acid-glycyrrhizic acid is prepared from p-aminophenylboronic acid and glycyrrhizic acid as raw materials through an amidation reaction.
7. The method according to claim 6, characterized in that: In step (1), the amination treatment is performed by immersing the pericardium in a solution containing adipic acid dihydrazide and reacting at 30-40° C. for 20-30 hours.
8. The method according to claim 7, characterized in that: In step (1), the solution containing adipic acid dihydrazide further comprises 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide; And / or, in step (1), the solvent of the solution is MES buffer, and the pH value of the MES buffer is 4.0-7.4; And / or, in step (1), the concentration of adipic acid dihydrazide in the solution is 0.02M~0.15M; And / or, in step (2), the reaction temperature is 30-40° C., and the reaction time is 20-30 hours; and / or, in step (2), the solution containing chondroitin sulfate further comprises 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide; And / or, in step (2), the solvent of the solution is MES buffer, and the pH value of the MES buffer is 4.0-7.4; And / or, in step (2), the concentration of the chondroitin sulfate in the solution is 1-10 mg / mL.
9. The method according to claim 8, characterized in that: In step (1), the concentration of adipic acid dihydrazide in the solution is 0.05 M; And / or, in step (2), the concentration of chondroitin sulfate in the solution is 5-10 mg / mL.
10. The method according to claim 8, characterized in that: In step (1), the molar ratio of adipic acid dihydrazide, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:(1-4):(1-4); And / or, in step (2), the mass ratio of chondroitin sulfate, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:(2-5):(1-4).
11. The method according to claim 10, characterized in that: In step (1), the molar ratio of adipic acid dihydrazide, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:2:2; And / or, in step (2), the mass ratio of chondroitin sulfate, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:(3-4):(1-2).
12. The method according to claim 6, characterized in that: In step (3), the amidation reaction further comprises 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide; And / or, in step (3), the solvent for the amidation reaction is N,N-dimethylformamide; And / or, in step (3), the temperature of the amidation reaction is 80-100° C.; and the reaction time is 10-20 hours.
13. The method according to claim 12, characterized in that: In step (3), the molar ratio of p-aminophenylboronic acid, glycyrrhizic acid, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:(1-2):(1-4):(1-4).
14. The method according to claim 13, characterized in that: In step (3), the molar ratio of p-aminophenylboronic acid, glycyrrhizic acid, 1-ethyl-3-(3-trimethylaminopropyl)carbodiimide hydrochloride and n-hydroxysuccinimide is 1:1:1.5:1.
5.
15. The method according to claim 6, characterized in that: In step (3), the solvent of the solution containing p-aminophenylboronic acid-glycyrrhizic acid is a mixed solution of N,N-dimethylformamide and anhydrous ethanol; And / or, in step (3), the concentration of p-aminophenylboronic acid-glycyrrhizic acid in the solution containing p-aminophenylboronic acid-glycyrrhizic acid is 3-10 mg / ml; And / or, in step (3), the temperature of the immersion reaction in the solution containing p-aminophenylboronic acid-glycyrrhizic acid is 30-40° C. and the time is 1-5 hours.
16. The method according to claim 15, characterized in that: In step (3), the volume ratio of N,N-dimethylformamide to anhydrous ethanol is 1:9; And / or, in step (3), the concentration of p-aminophenylboronic acid-glycyrrhizic acid in the solution containing p-aminophenylboronic acid-glycyrrhizic acid is 5 mg / ml.
17. Use of the bionic heart valve material according to any one of claims 1 to 5 in the preparation of an artificial bio-valve.
18. The use according to claim 17, characterized in that The artificial bio-valve is an artificial heart valve, an artificial pulmonary valve or an artificial venous valve.