A MoS2 / PDIsm surface-modified visible light responsive forward osmosis photocatalytic film and its preparation and application
Through the surface modification technology of MoS2/PDIsm photocatalyst combined with MoS2 nanoflowers, the problem of easy pollution of TFC-FO membrane is solved, its anti-pollution performance and treatment efficiency are improved, and operating costs are reduced.
Patent Information
- Application Number
- CN202310739851.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-06-20
AI Technical Summary
Existing modification methods cannot effectively solve the low efficiency and high cost problems caused by the easy pollution characteristics of polyamide composite films (TFC-FO membranes).
By preparing a visible light-responsive MoS2/PDIsm photocatalyst and combining it with MoS2 nanoflowers, using suction filtration and interfacial polymerization technology to deposit it on one side of the TFC membrane support layer, a MoS2/PDIsm surface-modified TFC-FO membrane was synthesized to improve its resistance to pollution performance.
The modified membrane significantly alleviates the deposition of pollutants on the membrane surface in sewage treatment, maintains stable operation of high water flux, reduces maintenance and operating costs, and improves the treatment efficiency of the TFC-FO membrane.
Smart Images

Figure CN116764681B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a MoS2 / PDIsm surface-modified visible light responsive forward osmosis photocatalytic film and preparation and application thereof, belonging to the technical field of water treatment. Background Art
[0002] Polyamide composite film (TFC membrane) is mainly composed of a non-porous and highly cross-linked polyamide active layer (PA layer) and a porous support layer. Due to its stable performance, low preparation cost and large-scale production, TFC membranes dominate the production and application of nanofiltration (NF), reverse osmosis (RO) and forward osmosis (FO) membranes. However, the membrane fouling problem during long-term operation has seriously restricted the development of TFC membranes.
[0003] Organic fouling is one of the important types of TFC membrane fouling. Organic substances commonly found in water bodies, represented by sodium alginate (SA), bovine serum albumin (BSA) and humic acid (HA), contaminate TFC membranes and then deposit, adsorb or accumulate on the membrane surface or internal structure, thereby forming a filter cake / gel layer. Membrane fouling inevitably leads to adverse changes in membrane structure and significant deterioration of separation performance. In order to maintain a stable treatment effect, more frequent chemical cleaning is necessary; however, this not only increases operating costs, but also greatly shortens the service life of the membrane. Therefore, improving the anti-fouling performance of TFC membranes is the key to ensuring their long-term stable operation.
[0004] Existing modification methods can optimize the anti-fouling performance of TFC membranes to varying degrees, but there are also some problems. For example, modification methods such as surface grafting will change the main properties of the PA layer, reduce the stability of the membrane, and affect the interception performance; and the nanomaterial doping method will cause a large number of structural defects in the PA layer due to the poor compatibility between nanomaterials and organic polymers, resulting in a high reverse salt flux; the material prepared by the layer-by-layer self-assembly (LBL) method has poor stability. It is particularly important to point out that forward osmosis technology has significant advantages in the treatment of complex water bodies with high salt and high pollution due to its advantage of low membrane fouling tendency. However, as the most used FO membrane, the forward osmosis membrane of polyamide composite film (TFC-FO membrane) has low efficiency and high cost problems caused by its easy fouling characteristics, which seriously restricts the application of FO technology in the treatment of complex water bodies. Summary of the invention
[0005] [Technical issues]
[0006] The existing modification methods cannot effectively solve the problems of low efficiency and high cost caused by the easy fouling of TFC-FO membranes.
[0007] [Technical solution]
[0008] In order to solve the above problems, the present invention firstly adopts PDIsm The photocatalyst MoS2 / PDI, which is responsive to visible light and highly compatible with organic polymer films, was prepared by combining photocatalyst and MoS2 nanoflowers. sm Then, MoS2 / PDI was filtered out. sm The dispersion is deposited on one side of the TFC membrane support layer, and finally, the MoS2 / PDI sm The PA layer is synthesized on the back of the modified layer to obtain MoS2 / PDI sm Surface modified TFC-FO membrane. MoS2 / PDI prepared by the present invention sm The surface-modified TFC-FO membrane has excellent visible light anti-pollution performance, which can effectively alleviate the deposition of pollutants on the membrane surface in the sewage treatment process, thereby maintaining stable operation with high water flux, greatly improving the operating potential of the TFC-FO membrane in treating sewage and wastewater.
[0009] The first object of the present invention is to provide a method for preparing a visible light responsive photocatalyst MoS2 / PDI. sm The method comprises the following steps:
[0010] (1)PDI sm Preparation of photocatalyst:
[0011] 1-8 mmol perylene-3,4,9,10-tetracarboxylic dianhydride, 10-40 mmol 3-aminopropionic acid and 0.1-1 mol imidazole are mixed, reacted at 80-140° C. for 3-8 hours under an argon environment, and stirred throughout the process to obtain a reaction precursor; then the reaction precursor is cooled to room temperature and dispersed in ethanol, and then a hydrochloric acid solution is added and stirred thoroughly, and then allowed to stand for aging to obtain a PDI stock solution; then 0.1-2 mL triethylamine is added to the PDI stock solution, and the hydrochloric acid solution is continuously added dropwise, and stirred throughout the process; finally, by suction filtration, centrifugation, washing and drying, a PDI photocatalyst for supramolecular polymer self-assembly (PDI) is obtained. sm Photocatalysts);
[0012] (2) Preparation of MoS2 nanoflowers:
[0013] 10-60 mg of ammonium tetrathiomolybdate ((NH4)2MoS4) and 20-80 mg of urea are mixed and ultrasonicated to form a uniformly dispersed solution; then 0.05-1 mL of hydrazine hydrate is added to the solution for stirring and ultrasonic mixing to obtain a mixed solution; finally, the mixed solution is reacted at 150-250°C for 5-24 hours. After the reaction is completed, it is cooled, centrifuged, washed and dried to obtain MoS2 nanoflowers;
[0014] (3) MoS2 / PDI sm Preparation:
[0015] 2-50 mg PDI sm The photocatalyst is dispersed in a mixed solvent containing 0.1-10 mL triethylamine and 10-80 mL N, N-dimethylformamide to obtain PDI. sm Photocatalyst dispersion; 1-50 mg MoS2 nanoflowers are ultrasonically dispersed in 1-50 mL N,N-dimethylformamide solution to obtain MoS2 nanoflower dispersion; then the MoS2 nanoflower dispersion is dropped into PDI sm The mixed solution is then reacted at 40-60°C for 1-12 hours. After the reaction is completed, a hydrochloric acid solution is added and stirred thoroughly, cooled, and filtered to obtain a solid. Finally, the solid is washed and dried to obtain a visible light responsive photocatalyst MoS2 / PDI. sm .
[0016] In one embodiment of the present invention, the amount of ethanol used in step (1) is 50 to 400 mL.
[0017] In one embodiment of the present invention, when preparing the PDI stock solution in step (1), the amount of hydrochloric acid solution used is 100-500 mL, and the concentration is 1-4 mol / L.
[0018] In one embodiment of the present invention, the aging time for preparing the PDI stock solution in step (1) is 24 hours.
[0019] In one embodiment of the present invention, in step (1), PDI is prepared sm When the photocatalyst is used, the amount of hydrochloric acid solution used is 10 to 50 mL, and the concentration is 1 to 4 mol / L.
[0020] In one embodiment of the present invention, the drying in step (1) is vacuum drying at a temperature of 40 to 100°C.
[0021] In one embodiment of the present invention, the ultrasonic time for forming a uniformly dispersed solution in step (2) is 10 to 90 minutes.
[0022] In one embodiment of the present invention, when preparing the mixed solution in step (2), the stirring is magnetic stirring for 5 to 60 minutes; and the ultrasonic time is 5 to 60 minutes.
[0023] In one embodiment of the present invention, methanol and water are used for centrifugal washing in step (2).
[0024] In one embodiment of the present invention, the drying temperature in step (2) is 40-100°C.
[0025] In one embodiment of the present invention, the reaction in step (3) is an oil bath heating reaction.
[0026] In one embodiment of the present invention, the amount of hydrochloric acid solution used in step (3) is 1 to 100 mL, and the concentration is 1 to 8 mol / L.
[0027] In one embodiment of the present invention, the magnetic stirring time in step (3) is 10 to 90 minutes.
[0028] In one embodiment of the present invention, the filtration in step (3) is membrane filtration.
[0029] In one embodiment of the present invention, the washing in step (3) is performed with N,N-dimethylformamide, methanol and water respectively until neutral.
[0030] In one embodiment of the present invention, the drying in step (3) is vacuum drying, and the drying temperature is 40-100°C.
[0031] In one embodiment of the present invention, the stirring speed involved in the method is 300-600 rpm.
[0032] The second object of the present invention is to prepare the visible light responsive photocatalyst MoS2 / PDI by the method of the present invention. sm .
[0033] The third object of the present invention is a method for preparing a surface-modified MoS2 / PDIsm visible light responsive forward osmosis photocatalytic film, comprising the following steps:
[0034] (1) MoS2 / PDI sm Preparation of surface modification layer:
[0035] MoS2 / PDI sm Disperse in water to obtain a dispersion; then filter the dispersion onto the surface of the PES base membrane by vacuum filtration, dry, and wash to obtain a dispersion containing MoS2 / PDI. sm a membrane having a surface modification layer;
[0036] (2) MoS2 / PDI sm Preparation of surface-modified visible light responsive forward osmosis photocatalytic film:
[0037] With the modified layer facing downward, place the MoS2 / PDI sm The membrane with the surface modification layer is fixed, and the m-phenylenediamine solution is poured on the membrane surface (unmodified side) for infiltration, and the excess m-phenylenediamine is removed after infiltration; then the trimesoyl chloride solution is poured on the membrane surface containing m-phenylenediamine for reaction, and then a thermal cross-linking reaction is performed after draining, and MoS2 / PDI is obtained after the reaction is completed. sm Surface modified visible light responsive forward osmosis photocatalytic films.
[0038] In one embodiment of the present invention, in step (1), the surface MoS2 / PDI of the film sm The loading amount is 1.42~4.26mg / cm 2 .
[0039] In one embodiment of the present invention, the drying in step (1) is performed at 40 to 100° C. for 10 to 90 minutes.
[0040] In one embodiment of the present invention, step (1) contains MoS2 / PDI sm After the surface modification layer is prepared, the membrane needs to be stored in water at a temperature of 0 to 25°C.
[0041] In one embodiment of the present invention, the fixing in step (2) is performed using a polytetrafluoroethylene frame, a rubber ring, a glass plate and a metal clamp.
[0042] In one embodiment of the present invention, the mass fraction of the intermediate phenylenediamine solution in step (2) is 2-4%, the soaking time is 1-10 min, and the soaking temperature is 15-25°C.
[0043] In one embodiment of the present invention, the mass fraction of the trimesoyl chloride solution in step (2) is 0.1-0.2%, the reaction time is 1-10 min, and the reaction temperature is 15-25°C.
[0044] In one embodiment of the present invention, the dosage ratio of the m-phenylenediamine solution to the trimesoyl chloride solution in step (2) is 6-7 mL:7-8 mL.
[0045] In one embodiment of the present invention, the reaction in step (2) is carried out at 15-25° C. for 1-10 min.
[0046] In one embodiment of the present invention, the thermal crosslinking reaction in step (2) is carried out in a hot water bath at 80-100° C. for 2-5 minutes.
[0047] The fourth objective of the present invention is the MoS2 / PDIsm surface-modified visible light responsive forward osmosis photocatalytic film prepared by the method described in the present invention.
[0048] The fifth object of the present invention is to provide a water treatment device comprising the MoS2 / PDI of the present invention. sm Surface modified visible light responsive forward osmosis photocatalytic films.
[0049] The sixth object of the present invention is to provide a method for water treatment, which uses the MoS2 / PDI described in the present invention. sm Surface modified visible light responsive forward osmosis photocatalytic films.
[0050] [Beneficial Effects]
[0051] (1) Preparation of MoS2 / PDI by the present invention sm When the surface-modified forward osmosis photocatalytic membrane is prepared, MoS2 / PDI is firstly obtained by ultrasonic treatment. sm The dispersion was then vacuum filtered onto the surface of polyethersulfone to prepare MoS2 / PDI through interfacial polymerization. sm Surface modified TFC-FO photocatalytic film. MoS2 / PDI sm It has strong hydrophilicity, which means that the use of this material modification will give the membrane a lower water contact angle and higher anti-fouling performance, and strong hydrophilic substances can reduce the resistance of water molecules passing through the membrane, which may improve the flux performance of the membrane to a certain extent. Compared with other modification methods such as grafting protein and intermediate layer modification, MoS2 / PDI sm The surface-modified forward osmosis photocatalytic membrane can alleviate the membrane fouling during the operation of the FO membrane, which increases the operating efficiency of the TFC membrane and also reduces the maintenance and operating costs to a certain extent. Compared with ultraviolet-responsive photocatalysts such as TiO2, the visible-light-responsive MoS2 / PDI sm It can utilize sunlight more efficiently, which will have greater advantages in the further development and application of photocatalytic films in the future.
[0052] (2) MoS2 / PDI prepared by the present invention sm The surface-modified visible light-responsive forward osmosis photocatalytic membrane reveals the mechanism of photocatalytic degradation of organic matter in inhibiting membrane pollution, that is, the photocatalytic material loaded onto the surface of the forward osmosis membrane can produce strong oxidizing species under light, thereby partially or completely degrading the pollutants on the membrane surface.
[0053] (3) The present invention comprises MoS2 / PDI sm The surface-modified visible light-responsive forward osmosis photocatalytic membrane is applied to the field of sewage treatment. On the basis of exploring the influence of photocatalytic degradation of organic matter on the formation of membrane fouling, its influence mechanism on the performance of TFC-FO membrane is revealed. It is a new topic in the field of environmental engineering and materials chemistry. At the same time, it achieves the purpose of sewage treatment, high water flux under polluted conditions, and improved anti-pollution performance of TFC-FO membrane, which is of great theoretical significance and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 To prepare MoS2 / PDI sm Schematic diagram of the method for surface-modified forward osmosis photocatalytic membrane. DETAILED DESCRIPTION
[0055] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0056] Test method:
[0057] 1. Water flux:
[0058] The mass of the drawn liquid on one side is continuously recorded by an automatic counting balance. The water flux can be obtained according to the change in the mass of the drawn liquid before and after the operation according to formula (1):
[0059]
[0060] In the formula, J W Indicates the water flux of the membrane, L·m -2 ·h -1 ; ΔV represents the volume of raw liquid permeating the membrane, L; Δt represents the time of the test experiment, h; A m Represents the effective area of the membrane, m 2 .
[0061] 2. Reverse salt flux:
[0062] By testing the conductivity of the raw liquid before and after operation, its ion concentration can be calculated. According to the volume change of the raw liquid before and after operation, the reverse salt flux can be obtained using formula (2):
[0063]
[0064] In the formula, J s is the reverse salt flux of the membrane, g·m -2 ·h -1 ; C0 and C t are the initial and final salt concentrations of the raw material solution, mg·L -1 ; V0 and V t are the volumes of the raw material solution at the beginning and end, L; Δt represents the experimental time, h; A m Represents the effective area of the membrane, m 2 .
[0065] 3. Flux attenuation rate:
[0066] By calculating the initial water flux and the end water flux of the pollution experiment, the flux attenuation rate is obtained according to formula (3):
[0067]
[0068] In the formula, J wi is the initial water flux, L·m -2 ·h -1 ; J we is the end point water flux, L·m-2 ·h -1 .
[0069] 4. Cumulative water production:
[0070] The cumulative water production is the increase in the volume of the extracted liquid during the entire osmosis experiment, mL.
[0071] The raw materials used in the embodiment:
[0072] The polyethersulfone support layer was a PES base membrane with a pore size of 0.1 μm and a diameter of 47 mm, both purchased from GVS, Germany;
[0073] The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased from the market;
[0074] If no specific technology or conditions are specified, the technology or conditions described in the literature in the field or the product manual shall be followed.
[0075] Example 1
[0076] A method for preparing visible light responsive photocatalyst MoS2 / PDI sm The method comprises the following steps:
[0077] (1)PDI sm Preparation of photocatalyst:
[0078] 3.5mmol perylene-3,4,9,10-tetracarboxylic dianhydride, 28mmol 3-aminopropionic acid and 0.26mol imidazole were placed in a round-bottom flask, heated in an oil bath under an argon environment (the balloon was adjusted to ensure the argon environment), reacted at 100°C for 4h, and stirred (at a speed of 450rpm) during the whole process to obtain a reaction precursor; the reaction precursor was then cooled to room temperature and dispersed in a beaker containing 100mL of ethanol, and then 300mL of a 2mol / L hydrochloric acid solution was added and stirred (at a speed of 450rpm), and then aged for one day to obtain a PDI stock solution; then 834μL of triethylamine was added to the PDI stock solution, and 15mL of a 4mol / L hydrochloric acid solution was continuously added dropwise, and stirring was maintained (at a speed of 450rpm) during the whole process; finally, the product was washed to neutrality by suction filtration and centrifugation, and vacuum dried at 60°C to obtain a supramolecular polymer self-assembled PDI photocatalyst (PDI sm Photocatalysts);
[0079] (2) Preparation of MoS2 nanoflowers: hydrothermal / solvothermal preparation
[0080] 30 mg of ammonium tetrathiomolybdate ((NH4)2MoS4) and 30 mg of urea were placed in a beaker and ultrasonicated for 30 minutes to completely disperse them to form a uniformly dispersed solution; then 150 μL of hydrazine hydrate was added to the beaker containing the solution and magnetically stirred (at a speed of 450 rpm) for 10 minutes, and then placed in an ultrasonic cleaning machine for 30 minutes to obtain a mixed solution; finally, the mixed solution was placed in a hydrothermal reactor and reacted at 200°C for 12 hours. After the reaction was completed, the product was cooled and washed with methanol and water by centrifugation until neutral, and dried at 60°C to obtain MoS2 nanoflowers;
[0081] (3) MoS2 / PDI sm Preparation:
[0082] 20 mg PDI sm The photocatalyst was dispersed in a mixed solvent containing 105 μL triethylamine and 40 mL N, N-dimethylformamide to obtain PDI sm Photocatalyst dispersion; 10 mg of MoS2 nanoflowers were ultrasonically dispersed (ultrasonic time was 30 min) in 5 mL of N, N-dimethylformamide solution to obtain a MoS2 nanoflower dispersion; then the MoS2 nanoflower dispersion was dropped into the PDI sm The mixed solution was obtained in the photocatalyst dispersion; the mixed solution was then reacted in an oil bath at 60°C for 5h. After the reaction was completed, 15mL of 4mol / L hydrochloric acid solution was added and fully magnetically stirred for 60min (rotation speed was 450rpm). After cooling to room temperature, the solid was filtered out with a filter membrane; finally, the solid was washed with N,N-dimethylformamide, methanol and water until neutral, and vacuum dried at 60°C to obtain the visible light responsive photocatalyst MoS2 / PDI. sm .
[0083] Example 2
[0084] A method for preparing a MoS2 / PDIsm surface-modified visible light responsive forward osmosis photocatalytic film comprises the following steps:
[0085] (1) MoS2 / PDI sm Preparation of surface modification layer:
[0086] 30 mg of MoS2 / PDI from Example 1 sm The dispersion was dispersed in 2L of water to obtain a dispersion; the dispersion was then vacuum filtered onto the surface of the PES-based membrane; in order to improve the immobilization effect of the material on the membrane surface, the membrane was placed in a 60°C oven and dried for 30 minutes after filtration; finally, the membrane was taken out and the membrane surface was thoroughly rinsed with deionized water to obtain a dispersion containing MoS2 / PDI. sm The surface modified layer of the membrane is placed in 4°C deionized water for storage; wherein the surface MoS2 / PDIsm The loading capacity is 4.26 mg / cm 2 ;
[0087] (2) MoS2 / PDI sm Preparation of surface-modified visible light responsive forward osmosis photocatalytic film:
[0088] With the modified layer facing downward, place the MoS2 / PDI sm The membrane of the surface modification layer was fixed, 6.70 mL of 2% m-phenylenediamine solution was poured on the membrane surface (unmodified side), and soaked at 20°C for 1 min. After soaking, nitrogen was used to blow off the residual m-phenylenediamine solution on the membrane surface; then 7.33 mL of 0.1% trimesoyl chloride solution was poured on the membrane surface containing m-phenylenediamine, and reacted at 20°C for 2 min. After draining, it was placed in a 100°C hot water bath for thermal cross-linking reaction for 5 min. After the reaction, MoS2 / PDI was obtained. sm The surface-modified visible light responsive forward osmosis photocatalytic film was named TFC-30.
[0089] Example 3
[0090] Adjust the MoS2 / PDI in step (1) of Example 2 sm The dosage is 20 mg, and the MoS2 / PDI on the membrane surface sm The loading capacity is 2.84 mg / cm 2 ; Others are consistent with Example 2, and MoS2 / PDI is obtained sm The surface-modified visible light responsive forward osmosis photocatalytic film was named TFC-20.
[0091] Example 4
[0092] Adjust the MoS2 / PDI in step (1) of Example 2 sm The dosage is 10 mg, and the surface MoS2 / PDI sm The loading capacity is 1.42 mg / cm 2 ; Others are consistent with Example 2, and MoS2 / PDI is obtained sm The surface-modified visible light-responsive forward osmosis photocatalytic film was named TFC-10.
[0093] Comparative Example 1 Omitting MoS2 / PDI sm
[0094] A method for preparing a conventional TFC-FO membrane comprises the following steps:
[0095] The fully infiltrated polyethersulfone support layer was fixed with a plate frame, 6.70 mL of a 2% by mass m-phenylenediamine solution was poured on the membrane surface, and infiltrated at 20°C for 1 minute. After infiltration, the residual m-phenylenediamine solution on the membrane surface was blown off with nitrogen; then 7.33 mL of a 0.1% by mass trimesoyl chloride solution was poured on the membrane surface, and reacted at 20°C for 2 minutes. After draining, the membrane was placed in a 100°C hot water bath for a thermal cross-linking reaction for 5 minutes to obtain the conventional TFC-FO membrane.
[0096] Comparative Example 2
[0097] Adjust the MoS2 / PDI in step (1) of Example 2 sm For PDI sm Photocatalyst, other than that in Example 2, was consistent to obtain PDI sm Surface modified visible light responsive forward osmosis photocatalytic films.
[0098] Comparative Example 3
[0099] Adjust the MoS2 / PDI in step (1) of Example 2 sm It is MoS2 nanoflower, and the rest is consistent with Example 2 to obtain a MoS2 surface modified visible light responsive forward osmosis photocatalytic film.
[0100] The obtained forward osmosis membrane was subjected to performance testing, and the test results are as follows:
[0101] It can be seen from Table 1 that MoS2 / PDI is introduced on the back of the support layer sm The water flux of the synthesized TFC-x membrane is comparable to that of the original TFC membrane, but its reverse solute flux is greatly reduced, and the specific salt flux (i.e., the solute loss per unit water production) is greatly reduced. sm The overall performance of the modified TFC membrane is improved.
[0102] Table 1
[0103]
[0104] Example 5
[0105] A method for water treatment using MoS2 / PDI sm The surface-modified visible light responsive forward osmosis photocatalytic film specifically comprises the following steps:
[0106] The forward osmosis membranes of Examples 2-4 and Comparative Example 1 were placed in a laboratory-made forward osmosis membrane reactor (disclosed in the document Zhao, Pin et al. "Explore the forward osmosis performance using hydrolyzed polyacrylamide as draw solute for dye wastewater reclamation in the long-term process." Chemical Engineering Journal 273 (2015): 316-324.) and a pollution experiment was carried out for 16 hours;
[0107] The feed liquid was 500 mL of 200 ppm BSA solution (BSA was selected as the characteristic pollutant), the draw liquid was 1 L of 1 M NaCl solution, and the modified layer side was facing the feed liquid; the pump speed of the peristaltic pump on the feed liquid and draw liquid sides was 17.4 rpm;
[0108] During the contamination process, a 300W xenon lamp (λ>400nm) was used for irradiation, and the distance between the xenon lamp light source and the membrane surface was 10cm.
[0109] The test results are shown in Table 2 below;
[0110] It can be seen from Table 2 that the introduction of MoS2 / PDI on the back of the support layer sm It gives the TFC membrane excellent anti-fouling performance. In the pollution experiment, the flux attenuation rate of the modified TFC membrane was greatly reduced, and the water production in the same time was greatly increased. At the same time, a single MoS2 or PDI sm The effect of the modified TFC membrane is much lower than that of the composite modified TFC membrane, namely: MoS2 and PDI sm There is a synergistic effect between them.
[0111] Table 2
[0112]
[0113] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. Preparation of MoS 2 / PDI sm Method for surface modification of visible light responsive forward osmosis photocatalytic films, It is characterized in that The steps include: (1) MoS 2 / PDI sm Preparation of surface modification layer: MoS 2 / PDI sm dispersed in water to obtain a dispersion; the dispersion was then filtered onto the surface of the PES base membrane by vacuum suction, dried, and washed to obtain a dispersion containing MoS 2 / PDI sm a membrane having a surface modification layer; (2) MoS 2 / PDI sm Preparation of surface-modified visible light responsive forward osmosis photocatalytic film: With the modified layer facing downward, place the MoS 2 / PDI sm The surface modification layer of the membrane is fixed, and the m-phenylenediamine solution is poured on the membrane surface for infiltration, and the excess m-phenylenediamine is removed after infiltration; then the trimesoyl chloride solution is poured on the membrane surface containing m-phenylenediamine for reaction, and then a thermal cross-linking reaction is performed after the reaction is completed. MoS 2 / PDI sm Surface modified visible light responsive forward osmosis photocatalytic film; Wherein, in step (1), the surface MoS 2 / PDI sm The loading amount is 1.42~4.26mg / cm 2 ; In step (2), the reaction is carried out at 15 to 25°C for 1 to 10 minutes, and the thermal crosslinking reaction is carried out in a hot water bath at 80 to 100°C for 2 to 5 minutes; Visible light responsive photocatalyst MoS 2 / PDI sm The preparation method is as follows: (a) PDI sm Preparation of photocatalyst: 1-8 mmol perylene-3,4,9,10-tetracarboxylic dianhydride, 10-40 mmol 3-aminopropionic acid and 0.1-1 mol imidazole are mixed, reacted at 80-140° C. for 3-8 hours under an argon environment, and stirred throughout the process to obtain a reaction precursor; then the reaction precursor is cooled to room temperature, dispersed in 50-400 mL ethanol, and then a hydrochloric acid solution is added and stirred thoroughly, and then allowed to stand for aging to obtain a PDI stock solution; then 0.1-2 mL triethylamine is added to the PDI stock solution, and the hydrochloric acid solution is continuously added dropwise, and stirring is maintained throughout the process; finally, PDI is obtained by suction filtration, centrifugation, washing and drying. sm Photocatalysts; (b) MoS 2 Preparation of Nanoflowers: 10-60 mg of ammonium tetrathiomolybdate and 20-80 mg of urea are mixed and ultrasonicated to form a uniformly dispersed solution; then 0.05-1 mL of hydrazine hydrate is added to the solution for stirring and ultrasonic mixing to obtain a mixed solution; finally, the mixed solution is reacted at 150-250°C for 5-24 hours. After the reaction is completed, it is cooled, centrifuged, washed and dried to obtain MoS 2 Nanoflower; (c)MoS 2 / PDI sm Preparation: 2-50 mg PDI sm The photocatalyst is dispersed in a mixed solvent containing 0.1-10 mL triethylamine and 10-80 mL N, N-dimethylformamide to obtain PDI. sm Photocatalyst dispersion: 1-50 mg MoS 2 Nanoflowers were ultrasonically dispersed in 1-50 mL N,N-dimethylformamide solution to obtain MoS 2 Nanoflower dispersion; then MoS 2 Nanoflower dispersion is added to PDI sm The mixed solution is reacted at 40-60°C for 1-12 hours. After the reaction, a hydrochloric acid solution is added and stirred thoroughly, cooled, and filtered to obtain a solid. Finally, the solid is washed and dried to obtain a visible light responsive photocatalyst MoS 2 / PDI sm .
2. MoS prepared by the method according to claim 1 2 / PDIsm surface modified visible light responsive forward osmosis photocatalytic film.
3. A water treatment device, It is characterized in that It contains the MoS according to claim 2 2 / PDI sm Surface modified visible light responsive forward osmosis photocatalytic films.
4. A method for water treatment, It is characterized in that It adopts the MoS described in claim 2 2 / PDI sm Surface modified visible light responsive forward osmosis photocatalytic films.