Copolymers, molded articles, extruded articles and transfer molded articles

By adjusting the content of tetrafluoroethylene and perfluoro(propyl vinyl ether) units and the melt flow rate, a copolymer was prepared, which solved the problems of insufficient thickness uniformity and transparency in the prior art, and achieved the manufacture of molded articles with high strength and low permeability.

CN116867817BActive Publication Date: 2026-11-10DAIKIN INDUSTRIES LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280016136.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-01-31
Publication Date
2026-11-10
Estimated Expiration
2042-01-31

AI Technical Summary

Technical Problem

Existing technologies struggle to produce uniformly thick, transparent, and high-strength tetrafluoroethylene copolymer molded bodies in a molten state, and suffer from issues with transparency, wear resistance, and insufficient tensile strength at high temperatures.

Method used

A copolymer was prepared by adjusting the content of tetrafluoroethylene and perfluoro(propyl vinyl ether) units, melt flow rate and number of functional groups, so that it is not easily deformed in the molten state. The copolymer was then manufactured into a uniformly thick sheet by extrusion molding, and its transparency, compression set, tensile strength and gas permeability were optimized.

Benefits of technology

It enables the manufacture of molded bodies with excellent transparency, low compression set, high tensile strength at high temperatures, and excellent air and carbon dioxide permeability in the molten state, suitable for a wide range of applications such as large-diameter pipes and thick sheet materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004404645800000051
    Figure BDA0004404645800000051
  • Figure BDA0004404645800000181
    Figure BDA0004404645800000181
  • Figure BDA0004404645800000211
    Figure BDA0004404645800000211
Patent Text Reader

Abstract

This invention provides a copolymer containing tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, wherein the content of perfluoro(propyl vinyl ether) units is 4.9% to 7.0% by mass relative to all monomer units, the melt flow rate at 372°C is 0.5 g / 10 min to 1.5 g / 10 min, and the number of functional groups per 10 6 The main chain has fewer than 20 carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to copolymers, molded articles, extruded molded articles, and transfer molded articles. Background Technology

[0002] Patent Document 1 discloses a material for OA equipment, which is a material for OA equipment composed of a tetrafluoroethylene copolymer. The material is characterized in that the tetrafluoroethylene copolymer has tetrafluoroethylene units derived from tetrafluoroethylene and perfluoro(alkyl vinyl ether) units derived from perfluoro(alkyl vinyl ether), wherein the perfluoro(alkyl vinyl ether) units constitute 4.5% to 6.6% of all monomer units, and the unstable terminal groups are relative to each 1×10 6 The number of carbon atoms is less than 20.

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2009-042478 Summary of the Invention

[0006] The problem that the invention aims to solve

[0007] The purpose of this invention is to provide a copolymer that is not easily deformed even in the molten state. Through extrusion molding, it is possible to easily obtain thick sheets with uniform thickness. It can produce molded bodies with excellent transparency, low compression set, high tensile strength at high temperature, low air permeability, low reagent permeability, excellent rigidity at 110°C, excellent creep resistance, wear resistance, and low carbon dioxide permeability, and fluoride ions are not easily dissolved in reagents such as hydrogen peroxide.

[0008] Methods for solving problems

[0009] According to the present invention, a copolymer is provided comprising tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, wherein the content of perfluoro(propyl vinyl ether) units is 4.9% to 7.0% by mass relative to all monomer units, the melt flow rate at 372°C is 0.5 g / 10 min to 1.5 g / 10 min, and the number of functional groups per 10 6 The main chain has fewer than 20 carbon atoms.

[0010] In the copolymer of the present invention, the melt flow rate at 372°C is preferably 0.7 g / 10 min to 1.3 g / 10 min.

[0011] In addition, according to the present invention, an extruded or transfer-molded article is provided, which contains the above-mentioned copolymer.

[0012] In addition, according to the present invention, a coated wire is provided having a coating layer containing the above-mentioned copolymer.

[0013] In addition, according to the present invention, a molded body is provided, which is a molded body containing the above-mentioned copolymer, wherein the molded body is a sheet or a tube.

[0014] The effects of the invention

[0015] According to the present invention, a copolymer is provided that is not easily deformed even in the molten state, and thick sheets with uniform thickness can be easily obtained by extrusion molding. It can also produce molded articles with excellent transparency, low compression set, high tensile strength at high temperature, low air permeability, low reagent permeability, excellent rigidity at 110°C, excellent creep resistance, wear resistance and low carbon dioxide permeability, and fluoride ions that are not easily dissolved in reagents such as hydrogen peroxide. Detailed Implementation

[0016] The specific embodiments of the present invention will be described in detail below, but the present invention is not limited to the following embodiments.

[0017] The copolymer of the present invention contains tetrafluoroethylene (TFE) units and perfluoro(propyl vinyl ether) (PPVE) units.

[0018] Copolymers containing TFE and PPVE units (PFA) are used as materials for forming thick sheets. Thick sheets tend to have superior tensile strength compared to thin sheets, but the greater the thickness, the lower the transparency. Therefore, to form thick sheets with high transparency, copolymers with extremely low haze values ​​are required. Furthermore, such thick sheets are typically manufactured by extruding the copolymer using an extruder. The molten copolymer exiting the extruder is prone to deformation due to its own weight before cooling and solidifying, making it difficult to produce sheets with the desired thickness. Consequently, such thick sheets are prone to deformation or wear under long-term continuous loads.

[0019] Patent Document 1 describes that the OA equipment material possessing the above-mentioned characteristics exhibits excellent softness and release properties from colorants, an excellent balance between heat resistance and crack resistance, and excellent melt extrusion molding properties. However, if this OA equipment material is used as a material for thick sheets, it is not easy to obtain thick sheets with uniform thickness. In addition, the obtained thick sheets also have problems with insufficient transparency, abrasion resistance, resistance to compression set, and tensile strength at high temperatures.

[0020] Discovery: By appropriately adjusting the PPVE unit content, melt flow rate (MFR), and number of functional groups in copolymers containing TFE and PPVE units, copolymers with the following characteristics can be obtained: they are not easily deformed even in the molten state, thick sheets with uniform thickness can be easily obtained by extrusion molding, and molded bodies with excellent transparency, low compression set, high tensile strength at high temperature, low air permeability, low reagent permeability, excellent rigidity at 110℃, excellent creep resistance, wear resistance, and low carbon dioxide permeability, and are not prone to fluoride ion dissolution in reagents such as hydrogen peroxide.

[0021] Furthermore, by using the copolymer of the present invention, large-diameter pipes with high dimensional accuracy can be manufactured using extrusion molding. Thus, the copolymer of the present invention can be used not only as a material for sheets but also for pipes and other wide-ranging applications.

[0022] The copolymer of the present invention is a melt-processable fluoropolymer. Melt processability means that the polymer can be melted and processed using existing processing equipment such as extruders.

[0023] The content of PPVE units in the copolymer is 4.9% to 7.0% by mass relative to all monomer units. The content of PPVE units in the copolymer is preferably 5.0% by mass or more, more preferably 5.1% by mass or more, further preferably 5.2% by mass or more, even more preferably 5.3% by mass or more, particularly preferably 5.4% by mass or more, most preferably 5.5% by mass or more, preferably 6.9% by mass or less, more preferably 6.8% by mass or less, further preferably 6.7% by mass or less, even more preferably 6.6% by mass or less, particularly preferably 6.5% by mass or less, and most preferably 6.4% by mass or less. By keeping the content of PPVE units in the copolymer within the above range, a copolymer with excellent transparency, low compression set, high tensile strength at high temperature, low air permeability, low reagent permeability, and excellent rigidity, creep resistance, abrasion resistance, and low carbon dioxide permeability at 110°C can be obtained. If the content of PPVE units in the copolymer is too low, the haze value will increase, or the tensile strength at high temperature will decrease, or the abrasion resistance will be poor.

[0024] The content of TFE units in the copolymer relative to all monomer units is preferably 93.0% to 95.1% by mass, more preferably 93.1% by mass or more, even more preferably 93.2% by mass or more, even more preferably 93.3% by mass or more, even more preferably 93.4% by mass or more, particularly preferably 93.5% by mass or more, most preferably 93.6% by mass or more, more preferably 95.0% by mass or less, even more preferably 94.9% by mass or less, even more preferably 94.8% by mass or less, even more preferably 94.7% by mass or less, particularly preferably 94.6% by mass or less, and most preferably 94.5% by mass or less. By keeping the content of TFE units in the copolymer within the above range, copolymers with excellent transparency, lower compression set, higher tensile strength at high temperatures, low air permeability, low reagent permeability, and superior rigidity, creep resistance, abrasion resistance, and low carbon dioxide permeability at 110°C can be obtained. If the copolymer contains too much TFE unit, the haze value may increase, the tensile strength at high temperatures may decrease, or the wear resistance may deteriorate.

[0025] In this invention, the content of each monomer unit in the copolymer is determined by... 19 Determined by F-NMR method.

[0026] The copolymer may also contain monomer units from monomers capable of copolymerizing with TFE and FAVE. In this case, the content of monomer units capable of copolymerizing with TFE and PPVE is preferably 0 to 2.1% by mass, more preferably 0.05% to 1.5% by mass, and even more preferably 0.1% to 0.9% by mass, relative to all monomer units of the copolymer.

[0027] Monomers capable of copolymerizing with TFE and PPVE include hexafluoropropylene (HFP) and CZ. 1 Z 2 =CZ 3 (CF2) n Z 4 (where Z) 1 Z 2 and Z 3 Same or different, represented by H or F, Z 4 Vinyl monomers (represented by H, F, or Cl, where n represents an integer from 2 to 10), CF2 = CF-ORf 1 (where Rf) 1 Perfluoro(alkyl vinyl ether) [PAVE] (except for PPVE) represented by perfluoroalkyl groups having 1 to 8 carbon atoms, and CF2=CF-OCH2-Rf 1 (where Rf is in the formula) 1This refers to perfluoroalkyl groups having 1 to 5 carbon atoms. Alkyl perfluorovinyl ether derivatives, etc., are also included. HFP is preferred.

[0028] The copolymer is preferably selected from at least one of the groups consisting of copolymers composed only of TFE units and PPVE units, and TFE / HFP / PPVE copolymers, and more preferably copolymers composed only of TFE units and PPVE units.

[0029] The melt flow rate (MFR) of the copolymer is 0.5 g / 10 min to 1.5 g / 10 min. The MFR of the copolymer is preferably 0.6 g / 10 min or more, more preferably 0.7 g / 10 min or more, even more preferably 0.8 g / 10 min or more, particularly preferably 0.9 g / 10 min or more, preferably 1.4 g / 10 min or less, more preferably 1.3 g / 10 min or less, and even more preferably 1.1 g / 10 min or less. By keeping the MFR of the copolymer within the above range, it is not easily deformed even in the molten state, and thick materials with uniform thickness can be easily obtained by extrusion molding. Furthermore, by using such a copolymer, molded articles with excellent transparency, low compression set, high tensile strength at high temperatures, high-temperature rigidity, abrasion resistance, and low carbon dioxide permeability can be obtained. If the MFR of the copolymer is too high, it is difficult to manufacture thick sheets with uniform thickness, and the resulting molded articles have poor transparency, abrasion resistance, compression set resistance, and high-temperature tensile strength. If the MFR of the copolymer is too low, the extrusion pressure during molding will be high, the moldability will be poor, or the resulting molded body will have poor air permeability, rigidity at 110°C, and low carbon dioxide permeability.

[0030] In this invention, MFR is a value obtained according to ASTM D1238 using a melt index meter in the form of the mass (g / 10 min) of polymer flowing out of a nozzle with an inner diameter of 2.1 mm and a length of 8 mm every 10 minutes at 372°C and a load of 5 kg.

[0031] MFR can be adjusted by modifying the type and amount of polymerization initiator and chain transfer agent used during monomer polymerization.

[0032] In this invention, every 10 of the copolymer 6 The number of functional groups per main chain carbon atom is less than 20. For every 10... 6 The number of functional groups per carbon atom in the main chain is preferably 15 or less, more preferably 10 or less, and even more preferably less than 6. By keeping the number of functional groups in the copolymer within the above range, it is possible to obtain a molded article with excellent carbon dioxide permeability, air permeability, reagent permeability, and creep resistance, and which does not easily allow fluoride ions to dissolve into reagents such as hydrogen peroxide.

[0033] The identification of the types of functional groups and the determination of the number of functional groups mentioned above can be achieved using infrared spectroscopy.

[0034] Regarding the number of functional groups, specifically, it was determined using the following method. First, the above copolymer was cold-pressed to produce a film with a thickness of 0.25 mm to 0.3 mm. The film was analyzed by Fourier transform infrared spectroscopy to obtain the infrared absorption spectrum of the above copolymer, and a differential spectrum was obtained compared with the background spectrum of a fully fluorinated copolymer without functional groups. The number of functional groups in the above copolymer was calculated from the absorption peaks of specific functional groups shown in the differential spectrum according to the following formula (A). 6 The number of functional groups N per carbon atom.

[0035] N = I × K / t (A)

[0036] I: Absorbance

[0037] K: Correction coefficient

[0038] t: Membrane thickness (mm)

[0039] For reference, the absorption frequencies, molar absorptivity, and correction factors for some functional groups are shown in Table 1. Furthermore, the molar absorptivity was determined using FT-IR measurements of low-molecular-weight model compounds.

[0040] [Table 1]

[0041] Table 1

[0042]

[0043] The absorption frequencies of -CH2CF2H, -CH2COF, -CH2COOH, -CH2COOCH3, and -CH2CONH2 are tens of Kaiser (cm) lower than those of -CF2H, -COF, free -COOH, and bonded -COOH, -COOCH3, and -CONH2, respectively, as shown in the table. -1 ).

[0044] For example, the number of functional groups in -COF refers to the number of functional groups originating from the absorption frequency of -CF2COF, which is 1883 cm⁻¹. -1 The number of functional groups derived from the absorption peak at 1840 cm⁻¹ and the absorption frequency originating from -CH₂COF were also analyzed. -1 The total number of functional groups obtained from the absorption peak at the given location.

[0045] Functional groups are those present at the ends of the main chain or side chains of the copolymer, and those present in the main chain or side chains. The number of functional groups can be the total number of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2, and -CH2OH.

[0046] The aforementioned functional groups are introduced into the copolymer, for example, through chain transfer agents or polymerization initiators used in the manufacturing of the copolymer. For instance, when an alcohol is used as a chain transfer agent, or when a peroxide having a -CH2OH structure is used as a polymerization initiator, -CH2OH is introduced to the ends of the copolymer's main chain. Alternatively, the aforementioned functional groups are introduced to the ends of the copolymer's side chains by polymerizing monomers containing functional groups.

[0047] By fluorinating the copolymer having such functional groups, copolymers having the number of functional groups within the aforementioned range can be obtained. That is, the copolymer of the present invention is preferably a fluorinated copolymer. The copolymer of the present invention also preferably has a -CF3 terminal group.

[0048] The melting point of the copolymer is preferably 290°C to 310°C, more preferably 296°C to 304°C. By keeping the melting point within this range, the copolymer is less prone to deformation even in the molten state. Furthermore, copolymers that provide molded articles with lower compression set and higher tensile strength at high temperatures can be obtained.

[0049] In this invention, the melting point can be determined using a differential scanning calorimeter (DSC).

[0050] The haze value of the copolymer of the present invention is preferably 4.5% or less, more preferably 4.0% or less. By keeping the haze value within the above range, when using the fluorinated copolymer of the present invention to obtain molded bodies such as sheets, tubes, pipes, connectors, flow meter housings, bottles, and nuts, it becomes easier to observe the interior of the molded body visually or with a camera, and it becomes easier to confirm the flow rate and balance of the contents. The haze value can be reduced by adjusting the content of PPVE units and the melt flow rate (MFR) of the copolymer. In the present invention, the haze value can be measured according to JIS K 7136.

[0051] The copolymer of the present invention preferably has a compression set of 45% to 77% when placed at 65°C for 72 hours under a compression ratio of 50%. By keeping the compression set at 65°C within the above range, it is possible to obtain a molded article that is not easily deformed under long-term continuous load.

[0052] In this invention, the compressive permanent deformation rate can be determined according to the methods described in ASTM D395 or JIS K 6262:2013.

[0053] The tensile strength of the copolymer of the present invention at 150°C is preferably 20.5 MPa or higher. By maintaining the tensile strength at 150°C within the above range, the resulting molded article exhibits high durability even under high temperature and high pressure. The tensile strength at 150°C can be increased by adjusting the PPVE unit content and melt flow rate (MFR) of the copolymer. In the present invention, the tensile strength at 150°C can be measured according to ASTM D638.

[0054] The preferred carbon dioxide permeability of the copolymer is 2300 cm⁻¹. 3 ·mm / (m 2 (24h·atm) or less, more preferably 2250cm 3 ·mm / (m 2 The temperature range is below 24 h atm. The copolymers of the present invention exhibit excellent low carbon dioxide permeability due to the appropriate adjustment of the PPVE unit content, melt flow rate (MFR), and number of functional groups in copolymers containing TFE and PPVE units. Therefore, for example, molded articles obtained using the copolymers of the present invention can be suitably used as sealing components to prevent leakage of carbon dioxide refrigerant.

[0055] In this invention, the carbon dioxide transmission coefficient can be determined under test conditions of 70°C and 0% RH. The specific determination of the carbon dioxide transmission coefficient can be performed using the methods described in the examples.

[0056] The air permeability coefficient of the copolymer is preferably 620 cm⁻¹. 3 ·mm / (m 2 (24h·atm) or less, preferably 600cm 3 ·mm / (m 2 The copolymers of the present invention exhibit excellent low air permeability due to the appropriate adjustment of the PPVE unit content, melt flow rate (MFR), and number of functional groups in copolymers containing TFE and PPVE units.

[0057] In this invention, the air permeability coefficient can be measured under test conditions of 70°C and 0% RH. The specific measurement of the air permeability coefficient can be performed using the methods described in the examples.

[0058] The preferred ethyl acetate permeability of the copolymer is 7.8 g·cm / m. 2 The following is more preferred: 7.2 g·cm / m 2The copolymers of the present invention exhibit excellent low permeability to ethyl acetate due to appropriate adjustments to the PPVE unit content, melt flow rate (MFR), and number of functional groups in copolymers containing TFE and PPVE units. In other words, by using the copolymers of the present invention, molded articles that are difficult for reagents such as ethyl acetate to permeate can be obtained.

[0059] In this invention, the ethyl acetate transmittance can be measured at 60°C for 45 days. The specific measurement of ethyl acetate transmittance can be performed using the methods described in the examples.

[0060] The copolymers of the present invention can be manufactured by polymerization methods such as suspension polymerization, solution polymerization, emulsion polymerization, and bulk polymerization. Emulsion polymerization or suspension polymerization is preferred as the polymerization method. In these polymerizations, conditions such as temperature and pressure, polymerization initiators, and other additives can be appropriately set according to the composition and amount of the copolymer.

[0061] Oil-soluble or water-soluble free radical polymerization initiators can be used as polymerization initiators.

[0062] Oil-soluble free radical polymerization initiators can be well-known oil-soluble peroxides, and the following substances can be cited as representative examples:

[0063] Dialkyl percarbonate esters, such as di-n-propyl percarbonate, diisopropyl percarbonate, disec-butyl percarbonate, and di-2-ethoxyethyl percarbonate;

[0064] Peroxide esters such as tert-butyl peroxide isobutyrate and tert-butyl perpentyl peroxide;

[0065] Dialkyl peroxides such as di-tert-butyl peroxide;

[0066] Di[fluoro(or fluorochloro)acyl] peroxides; etc.

[0067] Examples of diacyl peroxides include those represented by [(RfCOO)-]2 (where Rf is a perfluoroalkyl, ω-hydroperfluoroalkyl, or fluorochloroalkyl).

[0068] Examples of di[fluoro(or fluorochloro)acyl]peroxides include, for example, di(ω-hydro-dodecanoyl)peroxide, di(ω-hydro-tetradecanoyl)fluoroheptanoyl)peroxide, di(ω-hydro-hexadecanoyl)fluorononanoyl)peroxide, di(perfluoropropionyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluoropentanoyl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, di(ω-chloro-hexafluorobutyryl)peroxide, and di... (ω-chloro-decafluorohexanoyl) peroxide, di(ω-chloro-tetrafluorooctanoyl) peroxide, ω-hydro-dodecanoheptafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydro-dodecanoheptafluorobutyryl-perfluorobutyryl-peroxide, di(dichloropentafluorobutyryl) peroxide, di(trichlorooctafluorohexanoyl) peroxide, di(tetrachloroundecanoyl) peroxide, di(pentachlorotetrafluorodecanoyl) peroxide, di(undecachlorotetrafluorotetradecanoyl) peroxide, di(undecachlorotetrafluorotetradecanoyl) peroxide, etc.

[0069] Water-soluble free radical polymerization initiators can be well-known water-soluble peroxides, such as ammonium, potassium, and sodium salts of persulfate, perboric acid, perchloric acid, superphosphoric acid, and percarbonate; organic peroxides such as disuccinate peroxide and diglutaric acid peroxide; tert-butyl maleate peroxide; and tert-butyl hydroperoxide. Reducing agents such as sulfites can also be used in combination with peroxides, with the amount used relative to the peroxide ranging from 0.1 to 20 times.

[0070] In polymerization, surfactants, chain transfer agents, and solvents can be used, each of which can be existing and well-known substances.

[0071] As the surfactant, known surfactants can be used, such as nonionic surfactants, anionic surfactants, and cationic surfactants. Among these, fluorinated anionic surfactants are preferred, and more preferably, fluorinated anionic surfactants with straight or branched chains having 4 to 20 carbon atoms, with or without ether-bonded oxygen (i.e., oxygen atoms can be inserted between carbon atoms). The amount of surfactant added (relative to the polymerization water) is preferably 50 ppm to 5000 ppm.

[0072] Examples of chain transfer agents include: hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetates such as ethyl acetate and butyl acetate; alcohols such as methanol and ethanol; thiols such as methyl mercaptan; and halogenated hydrocarbons such as carbon tetrachloride, chloroform, dichloromethane, and chloromethane. The amount of chain transfer agent added varies depending on the chain transfer constant of the compound used, and is typically used in the range of 0.01% to 20% by mass relative to the polymerization solvent.

[0073] Examples of solvents include water and mixed solvents of water and alcohol.

[0074] In suspension polymerization, fluorinated solvents can be used in addition to water. Examples of fluorinated solvents include hydrochlorofluorocarbons such as CH3CClF2, CH3CCl2F, CF3CF2CCl2H, and CF2ClCF2CFHCl; chlorofluorocarbons such as CF2ClCFClCF2CF3 and CF3CFClCFClCF3; hydrofluorocarbons such as CF3CFHCFHCF2CF2CF3, CF2HCF2CF2CF2CF2H, and CF3CF2CF2CF2CF2CF2CF2H; and CH3OC2F5. Hydrofluoroethers such as CH3OC3F5CF3CF2CH2OCHF2, CF3CHFCF2OCH3, CHF2CF2OCH2F, (CF3)2CHCF2OCH3, CF3CF2CH2OCH2CHF2, and CF3CHFCF2OCH2CF3; perfluorocyclobutanes such as CF3CF2CF2CF3, CF3CF2CF2CF2CF3, and CF3CF2CF2CF2CF2CF3, with perfluoroalkanes being preferred. From the perspectives of suspension and economy, the amount of fluorinated solvent relative to the aqueous medium is preferably 10% to 100% by mass.

[0075] There is no particular limitation on the polymerization temperature, which can be 0 to 100°C. The polymerization pressure is appropriately determined according to the type, amount, vapor pressure, polymerization temperature, and other polymerization conditions used, and is usually 0 to 9.8 MPaG.

[0076] When an aqueous dispersion containing a copolymer is obtained through polymerization, the copolymer can be recovered by precipitating it, washing, and drying. Alternatively, when a copolymer is obtained as a slurry through polymerization, the copolymer can be recovered by removing the slurry from the reaction vessel, washing, and drying. The copolymer can also be recovered as a powder by drying.

[0077] The copolymer obtained through polymerization can also be granulated. There are no particular limitations on the granulation method; existing known methods can be used. For example, methods such as using a single-screw extruder, twin-screw extruder, or tandem extruder to melt-extrude the copolymer and cut it to a specified length to form granules can be employed. The extrusion temperature during melt extrusion needs to be varied depending on the melt viscosity of the copolymer and the manufacturing method; preferably, it is between the copolymer's melting point +20°C and the copolymer's melting point +140°C. There are no particular limitations on the copolymer cutting method; existing known methods such as wire cutting, thermal cutting, underwater cutting, and sheet cutting can be used. The volatile components in the granules can also be removed by heating (degassing treatment). Alternatively, the granules can be treated by contacting them with warm water at 30°C to 200°C, steam at 100°C to 200°C, or hot air at 40°C to 200°C.

[0078] The copolymer obtained by polymerization can also be fluorinated. Fluorination can be carried out by contacting the unfluorinated copolymer with a fluorinated compound. Through fluorination, thermally unstable functional groups such as -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, and -CONH2, as well as relatively thermally stable functional groups such as -CF2H, can be converted into extremely thermally stable -CF3. As a result, the total number of functional groups (-COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2, and -CF2H) of the copolymer can be easily adjusted to the above-mentioned range.

[0079] There are no particular limitations on fluorine-containing compounds; examples of fluorine radical sources that generate fluorine radicals under fluorination conditions can be cited. Examples of such fluorine radical sources include F2 gas, CoF3, AgF2, UF6, OF2, N2F2, CF3OF, and fluorinated halogens (e.g., IF5, ClF3).

[0080] Fluorine radical sources such as F2 gas can be 100% concentrated, but from a safety perspective, it is preferable to mix them with an inert gas and dilute them to 5% to 50% by mass before use, and more preferably to 15% to 30% by mass. Examples of such inert gases include nitrogen, helium, and argon; from an economic perspective, nitrogen is preferred.

[0081] The conditions for fluorination are not particularly limited; the molten copolymer can be brought into contact with a fluorinated compound. However, it is generally carried out at a temperature below the melting point of the copolymer, preferably between 20°C and 240°C, and more preferably between 100°C and 220°C. The fluorination treatment is typically carried out for 1 hour to 30 hours, preferably 5 hours to 25 hours. Fluorination is preferably carried out by bringing the unfluorinated copolymer into contact with fluorine gas (F2 gas).

[0082] The copolymers of the present invention can also be mixed with other components as needed to obtain compositions. Examples of other components include fillers, plasticizers, processing aids, mold release agents, pigments, flame retardants, lubricants, light stabilizers, weather stabilizers, conductive agents, antistatic agents, ultraviolet absorbers, antioxidants, foaming agents, fragrances, oils, softeners, defluorinated hydrogen agents, etc.

[0083] Examples of fillers include silica, kaolin, clay, organoclay, talc, mica, alumina, calcium carbonate, calcium terephthalate, titanium dioxide, calcium phosphate, calcium fluoride, lithium fluoride, cross-linked polystyrene, potassium titanate, carbon, boron nitride, carbon nanotubes, and glass fiber. Examples of conductive agents include carbon black. Examples of plasticizers include dioctyl phthalate and pentaerythritol. Examples of processing aids include carnauba wax, sulfone compounds, low molecular weight polyethylene, and fluorinated additives. Examples of defluorinating agents include organonium and amidines.

[0084] Other polymers besides the copolymers described above can also be used as other components. Examples of other polymers include fluoropolymers, fluororubbers, and non-fluorinated polymers, in addition to the copolymers described above.

[0085] Examples of methods for manufacturing the above composition include: dry mixing of the copolymer with other components; pre-mixing of the copolymer with other components using a mixer, followed by melt mixing using a kneader, melt extruder, etc.; etc.

[0086] The copolymers of the present invention or the above-described compositions can be used as processing aids, molding materials, etc., and are preferably used as molding materials. Aqueous dispersions, solutions, suspensions, and copolymer / solvent systems of the copolymers of the present invention can also be used as coatings, or for encapsulation, impregnation, and film casting. However, due to the aforementioned properties, the copolymers of the present invention are preferably used as the above-described molding materials.

[0087] The copolymer of the present invention or the above composition can also be molded to obtain a molded body.

[0088] The method for molding the above-described copolymer or composition is not particularly limited, and examples include injection molding, extrusion molding, compression molding, blow molding, transfer molding, rotational molding, and roll forming. Among these molding methods, extrusion molding, compression molding, or transfer molding are preferred, and are even more preferred because they enable high-productivity production of the molded body. That is, as the molded body, an extruded molded body, a compression molded body, an injection molded body, or a transfer molded body is preferred, and is even more preferred because it enables high-productivity production. By molding the copolymer of the present invention using extrusion molding or transfer molding, a beautiful molded body can be obtained.

[0089] The molded body containing the copolymer of the present invention can be, for example, a nut, bolt, joint, membrane, bottle, gasket, wire sheath, tube, hose, pipe, valve, sheet, seal, gasket, can, roller, container, stopcock, connector, filter housing, filter cover, flow meter, pump, wafer carrier, wafer box, etc.

[0090] The copolymers, compositions, or molded articles of the present invention can be used for, for example, the following purposes.

[0091] Food packaging films, lining materials for fluid transport pipelines used in food manufacturing processes, gaskets, sealing materials, thin sheets, and other fluid transport components for food manufacturing equipment;

[0092] Chemical stoppers, packaging films, lining materials for fluid delivery pipelines used in chemical manufacturing processes, gaskets, sealing materials, thin plates, and other reagent delivery components;

[0093] Inner lining components for reagent containers and piping in chemical equipment and semiconductor plants;

[0094] O-rings / pipes / gaskets, valve core materials, hoses, sealing materials, etc. used in the fuel system and peripheral devices of automobiles; hoses, sealing materials, and other fuel delivery components used in the AT system of automobiles.

[0095] The carburetor flange gaskets, shaft seals, valve stem seals, sealing materials, hoses, etc. used in the engine and peripheral devices of automobiles; brake hoses, air conditioning hoses, radiator hoses, wire sheathing materials, and other automobile components.

[0096] O-rings, tubes, gaskets, valve core materials, hoses, sealing materials, rollers, washers, diaphragms, connectors and other reagent delivery components for semiconductor manufacturing equipment;

[0097] Coating and ink components for coating equipment, such as coating rollers, hoses, tubes, and ink containers;

[0098] Food and beverage conduits, hoses, belts, gaskets, connectors and other food and beverage conveying components, food packaging materials, and glass cooking equipment;

[0099] Pipes, hoses, and other components used for waste liquid transportation;

[0100] Pipes, hoses, and other components used for high-temperature liquid transfer;

[0101] Pipes, hoses and other components used in steam piping;

[0102] Corrosion-resistant tape for piping, such as tape wrapped around the deck of a ship;

[0103] Various coating materials, such as wire coating materials, optical fiber coating materials, transparent surface coating materials and backing agents applied to the light incident side of photovoltaic elements in solar cells;

[0104] The diaphragm and various sliding components such as gaskets in a diaphragm pump;

[0105] Weather-resistant covers for agricultural films, various roofing materials, and sidewalls;

[0106] Interior materials used in the construction industry, and glass-like covering materials such as non-combustible fire-resistant safety glass;

[0107] Lining materials such as laminated steel sheets used in the home appliance industry.

[0108] Further examples of fuel delivery components used in the fuel systems of the aforementioned automobiles include fuel hoses, filler hoses, and evaporator hoses. These fuel delivery components can also be used for fuels resistant to acidic gasoline, alcohol-based fuels, and fuels containing gasoline additives such as those resistant to methyl tert-butyl ether and amines.

[0109] The stoppers and packaging films used for the aforementioned chemicals exhibit excellent resistance to acids and other chemicals. Additionally, anti-corrosion tape wrapped around the piping of chemical equipment can also be cited as a component for transporting the aforementioned reagents.

[0110] Examples of such molded bodies include radiator water chambers for automobiles, reagent tanks, bellows, partitions, rollers, gasoline tanks, waste liquid conveying containers, high-temperature liquid conveying containers, and fish farming and aquaculture tanks.

[0111] Further examples of the molded bodies mentioned above include components used in automobile bumpers, door panels, dashboards, food processing devices, cooking machines, waterproof and oil-proof glass, lighting-related instruments, indicator panels and housings of OA instruments, electrically illuminated signboards, displays, LCD screens, mobile phones, printer chassis, electrical and electronic components, groceries, trash cans, bathtubs, prefabricated bathrooms, exhaust fans, lighting frames, etc.

[0112] The molded articles containing the copolymers of this invention exhibit exceptional transparency, low compression set, high tensile strength at high temperatures, and excellent air and reagent permeability. They also demonstrate superior rigidity at 110°C, creep resistance, abrasion resistance, and low carbon dioxide permeability. Furthermore, they do not readily leach fluoride ions into reagents such as hydrogen peroxide. Therefore, they are suitable for use in nuts, bolts, joints, gaskets, valves, stopcocks, connectors, filter housings, filter covers, flow meters, pumps, etc. They are particularly suitable for use as piping components (especially valves and joints) in reagent delivery and as flow meter housings that provide a flow path for the reagent. The piping components and flow meter housings of this invention exhibit exceptional transparency, low compression set, and high tensile strength at high temperatures. Consequently, the internal visibility of the piping components and flow meter housings of this invention is excellent. In particular, the internal float of the flow meter housing can be easily observed visually or with a camera. Even under repeated stress due to changes in reagent flow start, stop, and flow rate, they are not easily damaged.

[0113] The molded articles containing the copolymers of this invention exhibit extremely excellent transparency, low compression set, high tensile strength at high temperatures, and excellent low air permeability, low reagent permeability, rigidity at 110°C, creep resistance, abrasion resistance, and low carbon dioxide permeability. They also do not readily leach fluoride ions into reagents such as hydrogen peroxide, making them suitable for use as gaskets, sealing gaskets, and other compressible components. The compressible components of this invention can be gaskets or sealing gaskets. The gaskets or sealing gaskets of this invention exhibit extremely excellent transparency, low compression set, high tensile strength at high temperatures, and excellent low air permeability, low reagent permeability, rigidity at 110°C, creep resistance, abrasion resistance, and low carbon dioxide permeability, making them unlikely to leach fluoride ions into reagents such as hydrogen peroxide. Furthermore, the excellent low carbon dioxide permeability of the compressible components of this invention also makes them suitable for use as sealing components to prevent leakage of carbon dioxide refrigerant.

[0114] The compressed component of the present invention exhibits excellent resistance to permanent compression deformation even when deformed at a high compression rate. The compressed component of the present invention can be used under compression deformation at a rate of 10% or more, and can be used under compression deformation at a rate of 20% or more, or 25% or more. By using the compressed component of the present invention under such a high compression rate, a certain degree of resilience can be maintained over a long period, and sealing and insulation properties can be maintained for a long time.

[0115] Regarding the aforementioned compressive deformation rate, when the compressed member is used in a compressed state, it is the compressive deformation rate of the part with the largest compressive deformation rate. For example, when a flat compressed member is used in a state where it is compressed along its thickness direction, it is the compressive deformation rate in the thickness direction. Furthermore, for example, when the compressed member is used in a state where only a portion of it is compressed, it is the compressive deformation rate of the part with the largest compressive deformation rate among the compressed portions.

[0116] The size and shape of the compressed member of the present invention can be appropriately set according to the application and are not particularly limited. The shape of the compressed member of the present invention can be, for example, ring-shaped. In addition, the compressed member of the present invention can have a circular, elliptical, or quadrilateral shape with rounded corners when viewed from above, and has a through hole in its central part.

[0117] The compressed member of the present invention is preferably used as a component for constructing a non-aqueous electrolyte battery. The compressed member of the present invention is particularly suitable as a component used in a state of contact with the non-aqueous electrolyte in a non-aqueous electrolyte battery. That is, the compressed member of the present invention can have a liquid-contacting surface for contact with the non-aqueous electrolyte in a non-aqueous electrolyte battery.

[0118] As for non-aqueous electrolyte batteries, there are no particular limitations as long as the battery contains a non-aqueous electrolyte; examples include lithium-ion secondary batteries and lithium-ion capacitors. Furthermore, components constituting non-aqueous electrolyte batteries include sealing components and insulating components.

[0119] The non-aqueous electrolyte is not particularly limited and can be one or more of the following known solvents: propylene carbonate, ethylene carbonate, butyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate. The non-aqueous electrolyte battery may further include an electrolyte. The electrolyte is not particularly limited and can be LiClO4, LiAsF6, LiPF6, LiBF4, LiCl, LiBr, CH3SO3Li, CF3SO3Li, cesium carbonate, etc.

[0120] The compressed component of the present invention can preferably be used as a sealing component such as a sealing gasket or sealing pad, or as an insulating component such as an insulating gasket or insulating sealing pad. A sealing component is used to prevent leakage of liquid or gas or intrusion of liquid or gas from the outside. An insulating component is used for electrical insulation. The compressed component of the present invention can also be used for both sealing and insulation purposes.

[0121] The compressible member of the present invention is suitable for use as a sealing member or insulating member for non-aqueous electrolyte batteries due to its low compression set and high tensile strength at high temperatures. For example, during charging of batteries such as non-aqueous electrolyte secondary batteries, the battery temperature may temporarily exceed 40°C, and particularly exceed 150°C. The compressible member of the present invention, even when deformed at high temperatures with a high compression set in batteries such as non-aqueous electrolyte secondary batteries, does not compromise its high resilience even when in contact with non-aqueous electrolytes at high temperatures. Therefore, when used as a sealing member, it exhibits excellent sealing properties, which are maintained for extended periods even at high temperatures. Furthermore, the compressible member of the present invention, containing the aforementioned copolymer, possesses excellent insulating properties. Therefore, when used as an insulating member, it provides a strong seal with two or more conductive members, preventing short circuits for extended periods.

[0122] The copolymers of the present invention can be suitable for use as materials for forming wire sheaths.

[0123] The coated wire has a core wire and a coating layer disposed around the core wire containing the copolymer of the present invention. For example, an extruded body formed by melt-extruding the copolymer of the present invention onto the core wire can be used as the coating layer. The coated wire is suitable for LAN cables (Eathernet cables), high-frequency transmission cables, flat cables, heat-resistant cables, etc., and is particularly suitable for transmission cables such as LAN cables (Eathernet cables) and high-frequency transmission cables.

[0124] For example, copper, aluminum, or other metallic conductors can be used as the core wire material. The core wire diameter is preferably 0.02 mm to 3 mm. More preferably, the core wire diameter is 0.04 mm or more, even more preferably 0.05 mm or more, and particularly preferably 0.1 mm or more. Even more preferably, the core wire diameter is 2 mm or less.

[0125] Specific examples of core wires include AWG (American wire gauge)-46 (solid copper wire with a diameter of 40μm), AWG-26 (solid copper wire with a diameter of 404μm), AWG-24 (solid copper wire with a diameter of 510μm), and AWG-22 (solid copper wire with a diameter of 635μm).

[0126] The thickness of the coating layer is preferably 0.1 mm to 3.0 mm. The thickness of the coating layer is also preferably less than 2.0 mm.

[0127] Coaxial cables are an example of high-frequency transmission cables. Coaxial cables typically have a structure consisting of an inner conductor, an insulating sheath, an outer conductor layer, and a protective sheath layer layered sequentially from the core to the outer periphery. Molded bodies containing the copolymer of the present invention can be suitable as the insulating sheath layer containing the copolymer. The thickness of each layer in the above structure is not particularly limited; typically, the diameter of the inner conductor is about 0.1 mm to 3 mm, the thickness of the insulating sheath is about 0.3 mm to 3 mm, the thickness of the outer conductor layer is about 0.5 mm to 10 mm, and the thickness of the protective sheath is about 0.5 mm to 2 mm.

[0128] The coating may contain air bubbles, which are preferably evenly distributed in the coating.

[0129] The average bubble diameter is not limited, but is preferably 60 μm or less, more preferably 45 μm or less, further preferably 35 μm or less, even more preferably 30 μm or less, particularly preferably 25 μm or less, and especially preferably 23 μm or less. Furthermore, the average bubble diameter is preferably 0.1 μm or more, more preferably 1 μm or more. The average bubble diameter can be obtained by acquiring an electron microscope image of the wire cross-section, calculating the diameter of each bubble using image processing, and then averaging the results.

[0130] The foaming rate of the coating layer can be 20% or more. More preferably, it is 30% or more, further preferably 33% or more, and even more preferably 35% or more. There is no particular upper limit, for example, 80%. The upper limit of the foaming rate can also be 60%. The foaming rate is calculated as ((specific gravity of wire coating material - specific gravity of coating layer) / specific gravity of wire coating material) × 100. The foaming rate can be adjusted appropriately according to the application, for example, by adjusting the gas insertion amount in the extruder described later, or by selecting the type of dissolved gas.

[0131] The coated wire may also have other layers between the core wire and the coating layer, and may further have other layers (outer layers) around the coating layer. If the coating layer contains air bubbles, the wire of the present invention may also be a two-layer structure (skin-foam body) with a non-foamed layer inserted between the core wire and the coating layer; a two-layer structure (foam body-skin body) with a non-foamed layer coated on the outer layer; and a three-layer structure (skin-foam body-skin body) with a non-foamed layer coated on the outer layer of the skin-foam body. The non-foamed layer is not particularly limited and may be a resin layer composed of TFE / HFP copolymers, TFE / PAVE copolymers, TFE / ethylene copolymers, vinylidene fluoride polymers, polyolefin resins such as polyethylene [PE], and resins such as polyvinyl chloride [PVC].

[0132] Coated wires can be manufactured, for example, by heating a copolymer using an extruder and extruding it onto the core wire while the copolymer is in a molten state to form a coating.

[0133] During the formation of the coating layer, the copolymer can also be heated, and gas can be introduced into the copolymer while it is in a molten state to form the aforementioned coating layer containing bubbles. The gas can be, for example, dichlorofluoromethane, nitrogen, carbon dioxide, or a mixture of these gases. The gas can be introduced into the heated copolymer in the form of pressurized gas, or it can be generated by mixing a chemical foaming agent into the copolymer. The gas dissolves in the molten copolymer.

[0134] In addition, the copolymers of the present invention are suitable for use as materials in products for high-frequency signal transmission.

[0135] As for the aforementioned high-frequency signal transmission products, there are no particular limitations as long as the product is used for high-frequency signal transmission. Examples include (1) insulating boards for high-frequency circuits, insulating materials for connecting components, printed wiring boards, and other molded boards; (2) bases for high-frequency vacuum tubes, radomes, and other molded bodies; and (3) sheathed wires such as coaxial cables and LAN cables. The aforementioned high-frequency signal transmission products are suitable for use in satellite communication equipment, mobile phone base stations, and other equipment that utilizes microwaves, especially microwaves from 3 GHz to 30 GHz.

[0136] In the aforementioned high-frequency signal transmission products, the copolymer of the present invention, from the perspective of low dielectric loss tangent, is suitable for use as an insulator.

[0137] As for the molded plate described in (1) above, a printed wiring substrate is preferred from the perspective of obtaining good electrical characteristics. There are no particular limitations on the printed wiring substrate described above; examples include printed wiring substrates for electronic circuits in mobile phones, various computers, and communication devices. As for the molded body described in (2) above, an antenna radome is preferred from the perspective of low dielectric loss.

[0138] The copolymer of the present invention is not easily deformed even in the molten state, and can easily produce thick sheets with uniform thickness. Furthermore, the resulting molded body has excellent transparency, is not easily deformed even at high temperatures, has excellent tensile strength at high temperatures, and exhibits excellent air permeability, reagent permeability, rigidity at 110°C, creep resistance, abrasion resistance, and carbon dioxide permeability. It also does not easily cause fluoride ions to dissolve into reagents such as hydrogen peroxide, thus making it suitable for use as a film or sheet.

[0139] The film of the present invention is useful as a release film. The release film can be manufactured by molding the copolymer of the present invention through melt extrusion molding, calendering, compression molding, casting, etc. From the perspective of obtaining a uniform film, the release film can be manufactured by melt extrusion molding.

[0140] The membrane of this invention can be applied to the surface of rollers used in OA equipment. Furthermore, the copolymer of this invention can be molded into necessary shapes, such as sheets, films, or tubes, through extrusion molding, compression molding, or pressing, for use as a surface material for OA equipment rollers or belts. In particular, thick sheets and large tubes can be manufactured using melt extrusion molding.

[0141] The copolymer of the present invention is not easily deformed even in the molten state, thus large-diameter tubes with high dimensional accuracy can be easily obtained by extrusion molding. Furthermore, the resulting molded body exhibits excellent transparency, low compression set, high tensile strength at high temperatures, and excellent air and reagent permeability, rigidity at 110°C, creep resistance, abrasion resistance, and low carbon dioxide permeability, making it difficult for fluoride ions to leach into reagents such as hydrogen peroxide. Therefore, the fluorinated copolymer of the present invention is suitable for use in tubes or pipes. Tubes containing the fluorinated copolymer of the present invention can be manufactured with high productivity even when they have large diameters and large thicknesses, and possess beautiful shapes, excellent transparency, low compression set, high tensile strength at high temperatures, low air and reagent permeability, excellent rigidity at 110°C, creep resistance, abrasion resistance, and low carbon dioxide permeability, making it difficult for fluoride ions to leach into reagents such as hydrogen peroxide.

[0142] The molded articles containing the copolymers of this invention exhibit extremely excellent transparency, low compression set, high tensile strength at high temperatures, and excellent low air permeability, low reagent permeability, rigidity at 110°C, creep resistance, abrasion resistance, and low carbon dioxide permeability. They also do not readily leach fluoride ions into reagents such as hydrogen peroxide, making them suitable for use as bottles. The bottles of this invention allow for easy visual inspection of the contents and are less prone to damage during use.

[0143] The embodiments have been described above, but it is understood that various changes can be made to the methods and details without departing from the spirit and scope of the claims.

[0144] Example

[0145] Next, embodiments will be given to illustrate the implementation of the present invention, but the present invention is not limited to the embodiments described.

[0146] The values ​​in the examples were measured using the following methods.

[0147] (Monomer content)

[0148] The content of each monomer unit was determined by an NMR analyzer (e.g., an AVANCE300 high-temperature probe manufactured by Bruker BioSpin).

[0149] (Mel flow rate (MFR))

[0150] According to ASTM D1238, the mass (g / 10 min) of polymer flowing out of a nozzle with an inner diameter of 2.1 mm and a length of 8 mm per 10 minutes was determined using a melt indexer G-01 (manufactured by Toyo Seiki Co., Ltd.) at 372°C and a load of 5 kg.

[0151] (Number of functional groups)

[0152] The copolymer granules were cold-pressed to produce films with a thickness of 0.25 mm to 0.3 mm. The films were then scanned 40 times using a Fourier transform infrared spectroscopy (FT-IR) device (Spectrum One, PerkinElmer) to obtain infrared absorption spectra. A differential spectrum was then obtained between this spectrum and the background spectrum of a fully fluorinated film devoid of functional groups. The number of functional groups N relative to each 1 × 10⁶ carbon atom in the sample was calculated from the absorption peaks of specific functional groups observed in the differential spectrum using the following formula (A).

[0153] N = I × K / t(A)

[0154] I: Absorbance

[0155] K: Correction coefficient

[0156] t: Membrane thickness (mm)

[0157] For reference, the absorption frequencies, molar absorptivity, and correction factors for the functional groups in this invention are shown in Table 2. The molar absorptivity was determined by FT-IR measurements of the low-molecular-weight model compounds.

[0158] [Table 2]

[0159] Table 2

[0160]

[0161] (Melting point)

[0162] The first heating was performed using a differential scanning calorimeter (trade name: X-DSC7000, manufactured by Hitachi High-Tech Science) at a heating rate of 10°C / min, from 200°C to 350°C. Then, the temperature was cooled from 350°C to 200°C at a cooling rate of 10°C / min. The second heating was performed again at a heating rate of 10°C / min, from 200°C to 350°C. The melting point was determined from the peak value of the melting curve generated during the second heating process.

[0163] Example 1

[0164] 26.6 L of pure water was added to a 174 L autoclave, and after thorough nitrogen purging, 30.4 kg of perfluorocyclobutane and 1.76 kg of perfluoropropyl vinyl ether (PPVE) were added. The system temperature was maintained at 35 °C and the stirring speed at 200 rpm. Next, tetrafluoroethylene (TFE) was injected to 0.58 MPa, followed by 0.010 kg of a 50% methanol solution of di-n-propyl peroxide dicarbonate, to initiate polymerization. Since the pressure within the system decreased as polymerization progressed, TFE was continuously supplied to maintain a constant pressure. For every 1 kg of TFE supplied, 0.058 kg of PPVE was added, and polymerization continued for 6 hours. After releasing the TFE and restoring atmospheric pressure to the autoclave, the resulting reaction product was washed with water and dried to obtain 15 kg of powder.

[0165] The obtained powder was melt-extruded at 360°C using a screw extruder (trade name: PCM46, manufactured by Ikebe Co., Ltd.) to obtain TFE / PPVE copolymer granules. The PPVE content of the obtained granules was determined using the method described above. The results are shown in Table 3.

[0166] The obtained granules were placed in a VVD-30 vacuum vibratory reactor (manufactured by Okawahara Seisakusho Co., Ltd.) and heated to 210°C. After evacuation, F2 gas diluted to 20% by volume with N2 gas was introduced to atmospheric pressure. 0.5 hours after the introduction of F2 gas, a temporary vacuum was applied, and F2 gas was introduced again. Then, after another 0.5 hours, a vacuum was applied again, and F2 gas was introduced again. This process of introducing F2 gas and evacuating the vacuum was repeated once every hour, and the reaction was carried out at 210°C for 10 hours. After the reaction was completed, the reactor was completely replaced with N2 gas to end the fluorination reaction. Various physical properties of the fluorinated granules were measured using the above method. The results are shown in Table 3.

[0167] Example 2

[0168] The PPVE was changed to 2.12 kg, and the PPVE was changed to an additional 0.068 kg for every 1 kg of TFE supplied. The polymerization time was changed to 7 hours. Otherwise, fluorinated pellets were obtained in the same manner as in Example 1. The results are shown in Table 3.

[0169] Example 3

[0170] 51.8 L of pure water was added to a 174 L autoclave, and after thorough nitrogen purging, 40.9 kg of perfluorocyclobutane, 3.01 kg of perfluoropropyl vinyl ether (PPVE), and 0.92 kg of methanol were added. The system temperature was maintained at 35 °C, and the stirring speed was maintained at 200 rpm. Next, tetrafluoroethylene (TFE) was injected to 0.64 MPa, followed by 0.013 kg of a 50% methanol solution of di-n-propyl peroxide dicarbonate, to initiate polymerization. Since the pressure in the system decreased as polymerization progressed, TFE was continuously supplied to maintain a constant pressure, with an additional 0.063 kg of PPVE added for every 1 kg of TFE supplied. Polymerization was terminated when the additional TFE amount reached 40.9 kg. Unreacted TFE was released, and the autoclave pressure was restored to atmospheric pressure. The resulting reaction product was washed with water and dried to obtain 43.5 kg of powder.

[0171] The obtained powder was subjected to a fluorination reaction in the same manner as in Example 1 to obtain fluorinated granules. The results are shown in Table 3.

[0172] Comparative Example 1

[0173] 26.6 L of pure water was added to a 174 L autoclave, and after thorough nitrogen purging, 30.4 kg of perfluorocyclobutane, 1.32 kg of perfluoropropyl vinyl ether (PPVE), and 0.06 kg of methanol were added. The system temperature was maintained at 35 °C, and the stirring speed was maintained at 200 rpm. Next, tetrafluoroethylene (TFE) was injected to 0.58 MPa, followed by 0.010 kg of a 50% methanol solution of di-n-propyl peroxide dicarbonate, to initiate polymerization. Since the pressure in the system decreased as polymerization progressed, TFE was continuously supplied to maintain a constant pressure. For every 1 kg of TFE supplied, 0.046 kg of PPVE was added, and polymerization continued for 5.5 hours. After releasing the TFE and restoring atmospheric pressure to the autoclave, the resulting reaction product was washed with water and dried to obtain 15 kg of powder.

[0174] The obtained powder was melt-extruded at 360°C using a screw extruder (trade name: PCM46, manufactured by Ikebe Co., Ltd.) to obtain TFE / PPVE copolymer granules. The PPVE content of the obtained granules was determined using the method described above. The results are shown in Table 3.

[0175] The obtained granules were placed in a VVD-30 vacuum vibratory reactor (manufactured by Okawahara Seisakusho Co., Ltd.) and heated to 210°C. After evacuation, F2 gas diluted to 20% by volume with N2 gas was introduced to atmospheric pressure. 0.5 hours after the introduction of F2 gas, a temporary vacuum was applied, and F2 gas was introduced again. Then, after another 0.5 hours, a vacuum was applied again, and F2 gas was introduced again. This process of introducing F2 gas and evacuating the vacuum was repeated once every hour, and the reaction was carried out at 210°C for 10 hours. After the reaction was completed, the reactor was completely replaced with N2 gas to end the fluorination reaction. Various physical properties of the fluorinated granules were measured using the above method. The results are shown in Table 3.

[0176] Comparative Example 2

[0177] The PPVE was changed to 1.72 kg, the methanol to 0.08 kg, and the PPVE was changed to an additional 0.057 kg for every 1 kg of TFE supplied. The polymerization time was changed to 6.5 hours. Otherwise, fluorinated pellets were obtained in the same manner as in Comparative Example 1. The results are shown in Table 3.

[0178] Comparative Example 3

[0179] The PPVE was changed to 2.12 kg, the methanol to 0.03 kg, and the PPVE was changed to an additional 0.068 kg for every 1 kg of TFE supplied. The polymerization time was changed to 7 hours. Otherwise, fluorinated pellets were obtained in the same manner as in Comparative Example 1. The results are shown in Table 3.

[0180] Comparative Example 4

[0181] The PPVE was changed to 2.08 kg, and the PPVE was changed to an additional 0.067 kg for every 1 kg of TFE supplied. The polymerization time was changed to 7 hours. Otherwise, unfluorinated pellets were obtained in the same manner as in Example 1. The results are shown in Table 3.

[0182] Comparative Example 5

[0183] 51.8 L of pure water was added to a 174 L autoclave, and after thorough nitrogen purging, 40.9 kg of perfluorocyclobutane and 3.33 kg of perfluoropropyl vinyl ether (PPVE) were added. The system temperature was maintained at 35 °C, and the stirring speed was maintained at 200 rpm. Next, tetrafluoroethylene (TFE) was injected to 0.64 MPa, followed by 0.004 kg of a 50% methanol solution of di-n-propyl peroxide dicarbonate, initiating polymerization. Since the pressure within the system decreased as polymerization progressed, TFE was continuously supplied to maintain a constant pressure, with an additional 0.068 kg of PPVE added for every 1 kg of TFE supplied. Polymerization was terminated when the additional TFE supply reached 40.9 kg. Unreacted TFE was released, and the autoclave pressure was restored to atmospheric pressure. The resulting reaction product was then washed with water and dried to obtain 41.0 kg of powder.

[0184] The obtained powder was subjected to a fluorination reaction in the same manner as in Example 1 to obtain fluorinated granules. The results are shown in Table 3.

[0185] [Table 3]

[0186] Table 3

[0187]

[0188] The “<6” in Table 3 refers to the number of functional groups being less than 6.

[0189] Next, the obtained granules were used to evaluate the following properties. The results are shown in Table 4.

[0190] (Haze value)

[0191] Using the above-mentioned granules and a hot press molding machine, sheets with a thickness of approximately 1.0 mm were produced. Using a haze meter (trade name: NDH7000SP, manufactured by Nippon Denshoku Kogyo Co., Ltd.), the sheets were immersed in a quartz dish containing pure water according to JIS K 7136, and the haze value was measured.

[0192] (Compression permanent deformation (CS))

[0193] The determination of compressive permanent deformation rate shall be made in accordance with the methods described in ASTM D395 or JIS K6262:2013.

[0194] With approximately 2g of the aforementioned granules placed in a mold (inner diameter 13mm, height 38mm), the mixture was melted at 370°C for 30 minutes using a hot plate press. Then, while being water-cooled under pressure of 0.2MPa (resin pressure), a molded body with a height of approximately 8mm was produced. Subsequently, the molded body was cut to produce a test piece with an outer diameter of 13mm and a height of 6mm. Using a compression device, the test piece was compressed at room temperature to a compression set of 50% (i.e., compressing the 6mm high test piece to a height of 3mm).

[0195] Next, the compressed test piece was placed in an electric furnace while fixed in the compression device and kept at 65°C for 72 hours. The compression device was then removed from the furnace and allowed to cool to room temperature before the test piece was taken off. The recovered test piece was left at room temperature for 30 minutes, and its height was measured. The compression set was then calculated using the following formula.

[0196] Compression set (%) = (t0 - t2) / (t0 - t1) × 100

[0197] t0: Original height of the test piece (mm)

[0198] t1: Height of the spacer (mm)

[0199] t2: Height of the test piece removed from the compression device (mm)

[0200] In the above experiment, t0 = 6 mm and t1 = 3 mm.

[0201] (Tensile strength at 150℃ (TS))

[0202] Determine the tensile strength at 150°C according to ASTM D638.

[0203] The molded parts with high tensile strength at 150℃ have excellent pressure resistance.

[0204] (Sheet formability)

[0205] use An extruder (manufactured by Imoto Manufacturing Co., Ltd.) and a T-die are used to form granules into sheets. The extrusion molding conditions are as follows.

[0206] a) Winding speed: 0.1 m / min

[0207] b) Roller temperature: 120℃

[0208] c) Membrane width: 70mm

[0209] d) Thickness: 1.00mm

[0210] e) Extrusion conditions:

[0211] • Single-screw extruder with a barrel diameter of 14mm and an L / D ratio of 20

[0212] Extruder set temperatures: Barrel section C-1 (330℃), Barrel section C-2 (350℃), Barrel section C-3 (370℃), T-die head (380℃)

[0213] Continue extruding the copolymer until it is stably extruded from the molding machine. Next, extrude the copolymer to produce sheets with a length of 3m or more (70mm wide) with a thickness of 1.00mm. Cut a 2-3m section from the end of the obtained sheet to prepare test pieces (1m long, 70mm wide) for measuring thickness variation. Measure the thickness at a total of three locations: the center point in the width direction at the end of the prepared sheet and two locations 25mm away from that center point in the width direction. Furthermore, measure the thickness at a total of nine locations: three center points spaced at 25cm intervals from the center point at one end of the sheet towards the other end, and two locations 25mm away from each center point in the width direction. Of the total 12 measurements, those with 1 or fewer measurements outside the ±10% range of 1.00mm are marked as ○, and those with 2 or more measurements outside the ±10% range of 1.00mm are marked as ×.

[0214] (Tube Formability)

[0215] use The extruder (manufactured by Tanabe Plastic Machinery) extrudes granules to form tubes with an outer diameter of 10.0 mm and a wall thickness of 1.0 mm. The extrusion molding conditions are as follows.

[0216] a) Die head inner diameter: 25mm

[0217] b) Outer diameter of the spindle: 13mm

[0218] c) Inner diameter of the shaping mold: 10.5mm

[0219] d) Traction speed: 0.4 m / min

[0220] e) Outer diameter: 10.0mm

[0221] f) Wall thickness: 1.0mm

[0222] g) Extrusion conditions:

[0223] • Single-screw extrusion molding machine with a barrel shaft diameter of 30mm and an L / D ratio of 22

[0224] Extruder set temperatures: Barrel section C-1 (350℃), Barrel section C-2 (370℃), Barrel section C-3 (380℃), Head section H-1 (390℃), Die section D-1 (390℃), Die section D-2 (390℃)

[0225] The obtained tubes are observed and evaluated according to the following criteria. The appearance of the tubes is confirmed visually.

[0226] ○: Good appearance

[0227] ×: The cross-section is not circular, and flatness or uneven thickness is observed, resulting in a poor appearance.

[0228] (Deformation test due to self-weight during melting)

[0229] Using granulation and a thermoforming machine, molded bodies with a diameter of 13 mm and a height of approximately 6.5 mm were produced. The resulting molded bodies were then cut to create test pieces with a height of 6.3 mm. The test pieces were placed in SUS (Sulfated Ultrasonic Flask) dishes and heated in an electric furnace at 330°C for 30 minutes. The dishes containing the test pieces were then water-cooled. The diameter of the bottom surface of the removed test piece was measured using vernier calipers, and the increase in bottom area was calculated using the following formula.

[0230] Bottom area increase rate (%) = {bottom area of ​​the test piece after heating (mm²)} 2 - Bottom area of ​​the test piece before heating (mm²) 2 )} / Bottom area of ​​the test piece before heating (mm²) 2 )×100

[0231] A lower base area increase rate means that the molded body is less likely to deform under its own weight when melted. Copolymers that provide molded bodies with a low base area increase rate are superior in that even when the copolymer is molded into thick sheets or large tubes by extrusion molding, the molded body in the molten state is not easily deformed, and the molded body obtains the desired shape after cooling and solidification.

[0232] (Abrasion test)

[0233] Using a granulation and hot-press molding machine, sheet-like test pieces with a thickness of approximately 0.2 mm were prepared, from which 10 cm × 10 cm test pieces were cut. The prepared test pieces were fixed on the test bench of a Tiber abrasion testing machine (No. 101 Special Type Tiber Abrasion Testing Machine, manufactured by Yasuda Seiki Co., Ltd.). Abrasion tests were conducted using the Tiber abrasion testing machine under the conditions of a load of 500 g, an abrasion wheel CS-10 (grinding with #240 abrasive paper for 20 revolutions), and a rotation speed of 60 rpm. The weight of the test piece was measured after 1000 revolutions, and the same test piece was further tested after 10000 revolutions, and the weight of the test piece was measured again. The amount of abrasion was calculated using the following formula.

[0234] Wear amount (mg) = M1 - M2

[0235] M1: Weight of the test piece after 1000 revolutions (mg)

[0236] M2: Weight of the test piece (mg) after 10,000 revolutions.

[0237] (Carbon dioxide permeability coefficient)

[0238] A sheet-like test piece with a thickness of approximately 0.1 mm was prepared using granulation and a hot press molding machine. Using the obtained test piece, the carbon dioxide transmittance was measured using a differential pressure gas transmittance meter (L100-5000 type gas transmittance meter, manufactured by Systech Illinois) according to the method described in JIS K7126-1:2006. The transmittance area was found to be 50.24 cm². 2 The carbon dioxide transmittance was measured at a test temperature of 70℃ and a test humidity of 0%RH. Using the obtained carbon dioxide transmittance and the thickness of the test piece, the carbon dioxide transmittance coefficient was calculated using the following formula.

[0239] Carbon dioxide permeability (cm) 3 ·mm / (m 2 ·24h·atm))=GTR×d

[0240] GTR: Carbon dioxide transmittance (cm) 3 / (m 2 ·24h·atm))

[0241] d: Thickness of the test piece (mm)

[0242] (Air permeability coefficient)

[0243] A sheet-like test piece with a thickness of approximately 0.1 mm was prepared using granulation material and a hot press molding machine. Using the obtained test piece, the air permeability was measured using a differential pressure gas permeability meter (L100-5000 type gas permeability meter, manufactured by Systech Illinois) according to the method described in JIS K7126-1:2006. The permeability area was found to be 50.24 cm². 2 The air transmittance value is obtained at a test temperature of 70℃ and a test humidity of 0%RH. Using the obtained air transmittance and the thickness of the test piece, the air transmittance coefficient is calculated using the following formula.

[0244] Air transmittance coefficient (cm) 3 ·mm / (m 2 ·24h·atm))=GTR×d

[0245] GTR: Air Transmittance (cm) 3 / (m2 ·24h·atm))

[0246] d: Thickness of the test piece (mm)

[0247] (Ethyl acetate permeability)

[0248] Using granulation and a thermoforming machine, sheet-like test pieces with a thickness of approximately 0.1 mm were produced. These were then placed in a test cup (with a transparency area of ​​12.56 cm²). 2 Add 10g of ethyl acetate to the solution, cover with a test sheet, and secure with a PTFE gasket. Ensure the test sheet is in contact with the ethyl acetate. After maintaining the solution at 60℃ for 45 days, remove the test sheet and allow it to stand at room temperature for 1 hour to measure the mass loss. Calculate the ethyl acetate transmittance (g·cm / m) using the following formula. 2 ).

[0249] Ethyl acetate (g·cm / m 2 = Mass reduction (g) × Thickness of sheet test piece (cm) / Transmitting area (m²) 2 )

[0250] (Deflection under load at 110℃)

[0251] Using granulation and a hot press molding machine, sheet-like test pieces with a thickness of approximately 4.2 mm were prepared. 80 × 10 mm test pieces were cut from these pieces and heated in an electric furnace at 100°C for 20 hours. In addition to using the obtained test pieces, tests were conducted according to the method described in JIS K-K7191-1 using a heat distortion tester (manufactured by Yasuda Seiki Co., Ltd.) under the conditions of a test temperature of 30°C to 150°C, a heating rate of 120°C / hour, a bending stress of 1.8 MPa, and the flatwise method. The load deflection was calculated using the following formula. Sheets with low load deflection at 110°C exhibit excellent rigidity at this high temperature.

[0252] Load-induced deflection (%) = a2 / a1 × 100

[0253] a1: Thickness of the test piece before the test (mm)

[0254] a2: Deflection at 110℃ (mm)

[0255] (Creep Resistance Evaluation)

[0256] Creep resistance was determined according to the methods described in ASTM D395 or JIS K6262:2013. A 13mm outer diameter and 8mm height molded body was prepared using granulation and a hot press. Test pieces with an outer diameter of 13mm and a height of 6mm were fabricated by cutting the molded body. The test pieces were compressed at room temperature to a compression set of 25% using a compression device. The compressed test pieces were then placed in an electric furnace at 80°C for 72 hours while still attached to the compression device. After removing the compression device from the furnace and cooling to room temperature, the test pieces were removed. The recovered test pieces were left at room temperature for 30 minutes, and their height was measured. The recovery ratio was calculated using the following formula.

[0257] Recovery rate (%) = (t2 - t1) / t3 × 100

[0258] t1: Height of the spacer (mm)

[0259] t2: Height of the test piece removed from the compression device (mm)

[0260] t3: Height after compression deformation (mm)

[0261] In the above experiment, t1 = 4.5 mm and t3 = 1.5 mm.

[0262] (Hydrogen peroxide immersion test)

[0263] 25g of granules were immersed in 50g of a 3% (w / w) hydrogen peroxide solution, heated in an electric furnace at 90°C for 20 hours, then sterilized in a sterilizer at 121°C for 1 hour, and cooled to room temperature. The granules were removed from the aqueous solution, and TISAB solution (10) (manufactured by Kanto Chemical Co., Ltd.) was added to the remaining aqueous solution. The concentration of fluoride ions in the resulting aqueous solution was measured using a fluoride ion meter. The concentration of fluoride ions per unit weight of granules (amount of fluoride ions dissolved) was calculated from the measured values ​​according to the following formula.

[0264] Dissolved fluoride ion content (ppm by mass) = Measured value (ppm by mass) × Aqueous solution volume (g) / Granule weight (g)

[0265] (Extrusion pressure)

[0266] Extrusion pressure was measured using a RHEOGRAPH 25 dual capillary rheometer (manufactured by Goettfert). A main die inner diameter of 1 mm, L / D = 16, and a secondary die inner diameter of 1 mm, L / D < 1 were used. The test conditions were: a measurement temperature of 390°C, a residual heat time of 10 minutes after pellet feeding, and a shear rate of 20 sec. -1 The barrel pressure value after 10 minutes of extrusion is Bagley corrected and used as the extrusion pressure. Copolymers with low extrusion pressure exhibit excellent extrusion molding properties, injection molding properties, and other molding properties.

[0267] (Dielectric loss tangent)

[0268] The granules were melt-molded to produce cylindrical test pieces with a diameter of 2 mm. These test pieces were then placed on a 6 GHz cavity resonator manufactured by Kanto Electronics Application Development Co., Ltd., and measurements were taken using a network analyzer manufactured by Agilent Technologies. The measurement results were analyzed using the analysis software "CPMA" manufactured by Kanto Electronics Application Development Co., Ltd. on a personal computer connected to the network analyzer, thereby determining the dielectric loss tangent (tanδ) at 20°C and 6 GHz.

[0269]

Claims

1. A copolymer comprising tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, The content of perfluoro(propyl vinyl ether) units is 4.9% to 7.0% by mass relative to all monomer units. The content of tetrafluoroethylene units relative to all monomer units is 93.0%–95.1% by mass. The melt flow rate at 372℃ is 0.5 g / 10 min to 1.5 g / 10 min. The number of functional groups -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2, and -CH2OH relative to 10 6 The main chain has fewer than 20 carbon atoms.

2. The copolymer of claim 1, wherein, The melt flow rate at 372℃ is 0.7 g / 10 min to 1.3 g / 10 min.

3. An extruded article comprising the copolymer of claim 1 or 2.

4. A transfer molded article comprising the copolymer of claim 1 or 2.

5. A coated wire having a coating layer comprising the copolymer of claim 1 or 2.

6. A molded article comprising the copolymer of claim 1 or 2, wherein, The molded body is a sheet or a tube.

Citation Information

Patent Citations

  • Office automation equipment material and image fixing member therefor

    JP2009042478A

  • Modified fluorine-containing copolymer and fluorine resin molded article

    CN105849163A

  • Tetrafluoroethylene and perfluorinated allyl ether copolymers

    CN107207671A