Protective film, frame and electronic equipment
By using a protective film with a film thickness of 3 μm or more on the electronic component frame, the dynamic index is 9 to 13, and the 60° glossiness is 10 to 50. Combined with a specific resin and hardener, the gloss and durability of the existing technology are solved. It solves the difficult problem of balancing performance and performance, and achieves a protective film with high gloss, abrasion resistance, and solvent resistance.
Patent Information
- Application Number
- CN202310332229.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-03-31
AI Technical Summary
It is difficult for existing pre-coated alloy plates to achieve the best gloss and brightness while meeting durability requirements such as wear resistance and solvent resistance.
Use a protective film with a film thickness of 3 μm or more, a dynamic index (FI) of 9 to 13, and a 60° gloss of 10 to 50. Adjust the FI and 60° gloss by adjusting the amount of wax or inorganic filler added and the average particle size. , and the protective film forming coating contains main agents such as acrylic resin, epoxy resin, etc., combined with hardeners and inorganic fillers to improve wear resistance and solvent resistance.
It achieves the best gloss and brightness on the electronic parts frame, while improving the wear resistance and solvent resistance, making it suitable for use as a protective film for modern electronic equipment.
Smart Images

Figure CN116891658B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a protective film for a frame body for accommodating electronic components, a frame body, and an electronic device. Background Art
[0002] Conventionally, as an outer casing for housing electronic components such as semiconductor devices, an outer casing manufactured by injection molding a thermoplastic resin has been often used.
[0003] In recent years, the market for electronic devices such as smartphones, tablets, and portable notebook personal computers has expanded, but in such applications, miniaturization, lightness, and thinness have developed rapidly, and the previous molded resin frames can no longer cope with them. This is because if the wall thickness is thinned in the previous resin frame, the strength is weak. Therefore, the number of metal frames such as magnesium or aluminum that can ensure strength and meet requirements such as electromagnetic wave shielding and heat dissipation has increased. In addition, metal frames are easy to reuse.
[0004] Recently, in addition to durability such as abrasion resistance and solvent resistance, there are many cases where a high level of design such as glossiness and matteness is required to achieve a better appearance, and this is often addressed by using a coating agent to protect the frame.
[0005] Japanese Patent Application Laid-Open No. 2004-98624 discloses a pre-coated aluminum alloy plate for a frame body, which uses resin beads containing any of polyester resin, acrylic resin, epoxy resin, and polyurethane resin and contains acrylic resin or fluororesin and has excellent scratch resistance.
[0006] Japanese Patent Application Laid-Open No. 2010-228279 discloses a pre-coated aluminum alloy sheet having excellent wear resistance and scratch resistance by adding a hard inorganic aggregate such as silica to a resin film, and is used for housings of electrical and electronic equipment such as notebook personal computers. Summary of the invention
[0007] However, in conventional pre-coated alloy sheets, it is difficult to achieve both optimum gloss and brilliance and satisfactory performance of a protective film, that is, durability such as abrasion resistance and solvent resistance.
[0008] In the past, glossiness was measured using a gloss meter to determine the quality of glossiness, but the glossiness had to be determined visually. However, in recent years, glossiness has been quantitatively quantified using products manufactured by X-Rite and BYK-mac i manufactured by BYK.
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a protective film having an optimal gloss and brightness and also having durability such as abrasion resistance and solvent resistance, and being suitable for use in a housing for housing electronic components.
[0010] The present invention is a protective film for a frame containing electronic components, the film thickness of which is above 3 μm, the Flop Index (FI) is 9 to 13, and the 60° glossiness is 10 to 50.
[0011] According to the present invention, a protective film having optimal gloss and brilliance and durability such as abrasion resistance and solvent resistance can be provided, which is suitable for use in a housing for housing electronic components.
[0012] The above and other objects, features and advantages of the present disclosure will be more fully understood in conjunction with the detailed description given below and the accompanying drawings which are given by way of illustration only, and therefore the detailed description and the accompanying drawings should not be construed as limiting the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a schematic cross-sectional view of the electronic device according to this embodiment.
[0014] Figure 2 This is a diagram for explaining the Flop Index (FI) according to this embodiment.
[0015] [Explanation of Symbols]
[0016] 1: Electronic equipment
[0017] 2: Protective film
[0018] 3: Frame base material
[0019] 4: Electronic parts
[0020] 10: Frame DETAILED DESCRIPTION
[0021] Hereinafter, the embodiment for carrying out the present invention will be described in detail.
[0022] [Protective film]
[0023] Figure 1 1 is a schematic cross-sectional view of an electronic device 1 of the present embodiment. The electronic device 1 has at least an electronic component 4 and a frame 10 that accommodates the electronic component 4. The frame 10 includes a protective film 2 on a frame substrate 3. The protective film 2 of the present embodiment is a protective film of the frame 10 that accommodates the electronic component. The protective film 2 is located on the outermost surface of the frame 10 that is opposite to the inner surface side that accommodates the electronic component 4.
[0024] [film thickness]
[0025] The film thickness of the protective film is 3 μm or more, preferably 4 μm or more, and more preferably 7 μm or more. When the film thickness of the protective film is 3 μm or more, abrasion resistance and solvent resistance can be improved.
[0026] On the other hand, the thickness of the protective film is preferably 20 μm or less. When a protective film having a thickness exceeding 20 μm is formed, foam is likely to remain on the coating surface when the protective film forming paint is applied and baked, which is likely to cause poor appearance of the cured coating film, and is therefore not preferred.
[0027] <Flop Index (FI)>
[0028] The FI of the protective film is used as an index to indicate the glossiness. The higher the FI, the higher the glossiness, and the lower the FI, the lower the glossiness. The FI of the protective film of this embodiment is 9 to 13, preferably 10 to 13, and more preferably 12 to 13. As long as the FI of the protective film is within the above range, the desired glossiness, wear resistance, solvent resistance and other properties of the protective film can be effectively optimized.
[0029] The FI was measured on the coating film surface using a multi-angle colorimeter "BYK-maci" manufactured by BYK Instruments Inc. The FI, or Flop Index, was calculated by the following formula (1).
[0030] FI=2.69×(L * 15° -L * 110° ) 1.11 ÷L * 45° 0.86 Formula (1)
[0031] The FI measurement system is shown in Figure 2 FI is calculated using the following brightness L*, that is, irradiating light at an incident angle of 45° relative to the perpendicular direction of the surface of the measured object (incident light), detecting light reflected at a certain angle (regular reflected light) using a detector, and digitizing the brightness L*. L* is the brightness L* in the L*a*b* color system specified in Japanese Industrial Standards (JIS) Z8729, L* 15° , L* 45° , L* 110° These are L* observed at deviation angles of 15°, 45°, and 110° from regular reflected light of light incident at an angle of 45° to the perpendicular direction of the surface of the measurement object.
[0032] <60° gloss>
[0033] The protective film of the present embodiment has a 60° glossiness of 10 to 50, preferably 10 to 20, more preferably 11 to 17, and still more preferably 14 to 15. When the 60° glossiness is 10 to 50, the glossiness of the protective film is improved, and the abrasion resistance and solvent resistance are improved.
[0034] FI and 60° glossiness can be adjusted according to the amount of wax or inorganic filler added to the protective film. Specifically, if the amount of wax or inorganic filler added is increased, FI and 60° glossiness decrease, and if the amount of wax or inorganic filler added is reduced, FI and 60° glossiness increase. In addition, it can also be adjusted according to the thickness of the protective film. Specifically, if the thickness of the protective film is increased, FI will increase and 60° glossiness will decrease. If the thickness of the protective film is reduced, the opposite tendency will occur.
[0035] In addition, the FI and 60° gloss can be adjusted by adjusting the average particle size of the wax or inorganic filler.
[0036] <Root mean square gradient (Sdq)>
[0037] The root mean square tilt Sdq is defined by the International Organization for Standardization (ISO) 25178-2:2012 standard and is calculated by the following formula (2).
[0038]
[0039] A represents the area of the defined surface, represents the x-axis direction, represents the y-axis direction, Indicates the respective small displacements in the z-axis direction.
[0040] Sdq is a parameter indicating the average magnitude of the local gradient (inclination) of the surface concavity and convexity. The larger its value, the steeper the gradient of the concavity and convexity. That is, the degree of surface roughness can be determined based on the numerical value of Sdq.
[0041] In the present embodiment, from the viewpoint of the appearance of the protective film, Sdq is preferably 1 to 10, and more preferably 1.5 to 8. When Sdq is within the above range, FI and 60° glossiness determined in the present embodiment are easily satisfied.
[0042] <Arithmetic mean altitude (Sa)>
[0043] The arithmetic mean height Sa is defined by ISO 25178-2:2012 as is Sdq, and is a parameter obtained by extending the arithmetic mean height (Ra) of a line to a surface, and represents the average of the absolute values (height differences from the average surface) of Z (x, y) in the measurement target area. In other words, it is a parameter representing the average height of surface irregularities, and is calculated by the following formula (3).
[0044]
[0045] In the present embodiment, from the viewpoint of the appearance of the protective film, Sa is preferably 0.1 μm to 1 μm, and more preferably 0.2 μm to 0.7 μm. When Sa is within the above range, FI and 60° glossiness determined in the present embodiment are easily satisfied.
[0046] Furthermore, both Sdq and Sa can be calculated by processing, using appropriate analysis software, surface shape data obtained by contact surface roughness measurement using a stylus surface roughness measuring machine or the like, or non-contact surface roughness measurement using a laser microscope or the like.
[0047] Sdq and Sa can be controlled by adjusting the type, amount added, and average particle size of the particulate additive or the thickness of the protective film to be formed.
[0048] <Dynamic friction coefficient>
[0049] The frame formed with the protective film needs to be smoothly transported without being damaged. Therefore, the surface of the protective film preferably has an appropriate dynamic friction coefficient. The value of the dynamic friction coefficient is preferably 0.05 to 0.5, and more preferably 0.06 to 0.40. If the value of the dynamic friction coefficient is within the range, appropriate transportability can be exerted, and the frame can be smoothly transported without damaging the protective film, and when the frames are stacked, the possibility of goods scattering due to excessive sliding properties is reduced.
[0050] The dynamic friction coefficient can be controlled mainly by the type and amount of wax component added.
[0051] <Method for producing protective film>
[0052] The protective film of the present embodiment is formed as a cured coating film by applying a protective film-forming coating material on a frame substrate and volatilizing and drying a liquid medium in an oven or the like.
[0053] <Coatings for forming protective films>
[0054] As coatings for forming protective films, in addition to general solvent-based coatings, water-based coatings, solvent-free coatings and other thermosetting coatings, there are also ultraviolet (UV) hardening coatings, etc., and there are no special restrictions. However, if we take into account the environmental restrictions in recent years, especially the restrictions on volatile organic compounds (VOC), water-based coatings, solvent-free coatings, and UV hardening coatings are preferred. However, on the other hand, solvent-free coatings or UV hardening coatings have low film strength as hardened coatings due to the low molecular weight of the constituent materials, and it is difficult to obtain satisfactory performance as a protective film for a frame that requires strong durability. On the other hand, water-based coatings include water-soluble or water-dispersible coatings, and the latter are mainly called emulsions. Both solvent-based coatings and water-based coatings (especially emulsion coatings) can obtain protective films with excellent durability.
[0055] (Structure of coating material for forming protective film)
[0056] Next, the structure and materials of the coating for forming a protective film (hereinafter, also referred to as "coating") are described. The structural components of the coating include a main agent, a hardener, a solvent, a wax, an inorganic filler, etc. In this embodiment, the coating contains at least a main agent, and may also contain other components such as a hardener, a solvent, a wax, an inorganic filler, etc. as needed.
[0057] (Main agent)
[0058] As the main agent, there are epoxy resins, acrylic resins, polyester resins, urethane resins, or acrylic modified epoxy resins described later, etc. In particular, for a protective film that requires durability, especially abrasion resistance, acrylic resins, epoxy resins, or acrylic modified epoxy resins are preferred. The main agent can be used alone or in combination of two or more of these resins.
[0059] (Acrylic resin (A))
[0060] The acrylic resin (A) in the present embodiment is preferably a copolymer obtained from monomers containing N-alkoxymethyl (meth) acrylamide (a-1), (meth) alkyl esters of 8 to 20 carbon atoms (a-2), and monomers having a carboxyl group (a-3). In addition, the so-called "(meth) acrylic group" is a general term for acrylic groups and methacrylic groups, and "(meth) acrylate" is a general term for acrylic esters and methacrylates.
[0061] <N-Alkoxymethyl (meth)acrylamide (a-1)>
[0062] N-Alkoxymethyl (meth)acrylamide (a-1) is a crosslinking monomer and can easily react with other reactive functional groups under heating or acidic conditions.
[0063] Specific examples thereof include N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, N-n-propoxymethyl (meth)acrylamide, N-isopropoxymethyl (meth)acrylamide, N-n-butoxymethyl (meth)acrylamide, N-isobutoxymethyl (meth)acrylamide, N-pentyloxymethyl (meth)acrylamide, N-hexyloxymethyl (meth)acrylamide, N-heptyloxymethyl (meth)acrylamide, N-octyloxymethyl (meth)acrylamide, and N-2-ethylhexyloxymethyl (meth)acrylamide.
[0064] Among them, the alkoxy group preferably has 1 to 8 carbon atoms, and more preferably has 1 to 4 carbon atoms, such as N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, N-n-propoxymethyl (meth)acrylamide, N-isopropoxymethyl (meth)acrylamide, N-n-butoxymethyl (meth)acrylamide, and N-isobutoxymethyl (meth)acrylamide.
[0065] <(Meth)acrylic acid alkyl ester having 8 to 20 carbon atoms in the alkyl group (a-2)>
[0066] The (meth)acrylic acid alkyl ester (a-2) having an alkyl group with 8 to 20 carbon atoms is used for adjusting the glass transition temperature (Tg) of the acrylic resin (A) and the like.
[0067] Specific examples include n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, n-stearyl (meth)acrylate, and isostearyl (meth)acrylate.
[0068] <Monomer having a carboxyl group (a-3)>
[0069] The monomer (a-3) having a carboxyl group imparts moderate hydrophilicity to the acrylic resin (A), and the acrylic resin (A) can be made into an aqueous solution or a water dispersion by neutralizing it with a basic compound.
[0070] Examples of the carboxyl group-containing monomer (a-3) include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, etc. Among these, (meth)acrylic acid is preferred from the viewpoint of copolymerizability with other monomers.
[0071] As the monomer constituting the acrylic resin (A), monomers other than those described above may be used.
[0072] Specific examples thereof include (meth)acrylate alkyl ester monomers having an alkyl group with 1 to 7 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, and hexyl (meth)acrylate;
[0073] A monomer having a hydroxyl group such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, hydroxypentyl (meth)acrylate, and hydroxyhexyl (meth)acrylate;
[0074] Vinyl monomers such as styrene, p-methylstyrene, α-methylstyrene, vinyltoluene, vinyl acetate, and vinyl propionate.
[0075] All monomers that can be used may be used alone or in combination of two or more.
[0076] The acrylic resin (A) can be synthesized by solution polymerization, emulsion polymerization, suspension polymerization, bulk polymerization, or the like.
[0077] Among them, solution polymerization is preferred because the reaction is easily controlled. After the polymerization, the solvent is removed as necessary and water is added to obtain a water-based coating.
[0078] In addition, when synthesizing the acrylic resin (A), a radical polymerization initiator used in synthesizing a general acrylic resin can be used. Among the radical polymerization initiators, an azo compound or a peroxide compound is preferred.
[0079] Examples of the azo compound include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane].
[0080] In addition, examples of peroxide compounds include benzoyl peroxide, tert-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, tert-butyl peroxy-2-ethylhexanoate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, tert-butyl peroxyneodecanoate, tert-butyl peroxytrimethylacetate, di(3,5,5-trimethylhexanoyl)peroxide, dipropionyl peroxide, and diacetyl peroxide.
[0081] The radical polymerization initiator is preferably used in an amount of 0.1 to 10 parts by mass based on 100 parts by mass of the total monomers.
[0082] The weight average molecular weight of the acrylic resin (A) is preferably 1,000 to 100,000, more preferably 10,000 to 50,000. When it is 1,000 or more, the hardness of the coating film is improved, and when it is 100,000 or less, the coating stability during water-based coating is easily ensured.
[0083] (Epoxy resin (B))
[0084] The epoxy resin (B) is preferably an epoxy resin of a bisphenol type, a novolac type, a naphthalene type, a biphenyl type, etc. Among these, if the processability, abrasion resistance, and adhesion to the frame after being made into a protective film are taken into consideration, a bisphenol A type epoxy resin is more preferred. The epoxy resin (B) preferably has a weight average molecular weight of 2500 to 70,000. When the weight average molecular weight is less than 2500, the residual amount of unreacted products such as bisphenol A increases, and physical properties such as durability cannot be fully obtained sometimes. On the other hand, if the weight average molecular weight exceeds 70,000, it is sometimes impossible to fully obtain adhesion to the frame. In the present embodiment, commercially available products of bisphenol A type epoxy resins include, for example, JER1007, JER1009, and JER1010 manufactured by Mitsubishi Chemical (Co., Ltd.).
[0085] (Acrylic modified epoxy resin (C))
[0086] When epoxy resin is used alone, it cannot be dissolved or dispersed in water. Therefore, by modifying it with an ethylenically unsaturated monomer such as an acrylic resin or an acrylic monomer having a carboxyl group, a stable water-based coating can be obtained. Acrylic modified epoxy resin (C) is a composite resin obtained by using an ethylenically unsaturated monomer and an epoxy resin. Examples of its production method include (a) graft polymerization, (b) esterification, and (c) direct polymerization. That is,
[0087] (a) Graft polymerization method: In the presence of an epoxy resin, an ethylenically unsaturated monomer including a carboxyl group-containing monomer such as (meth)acrylic acid as an essential component is polymerized using a free radical polymerization initiator to obtain an acrylic modified epoxy resin in which an acrylic polymer is grafted onto the epoxy resin.
[0088] (b) Esterification method: an ethylenically unsaturated monomer having a carboxyl group such as (meth)acrylic acid as an essential component is polymerized to obtain an acrylic polymer having a carboxyl group, and a part of the carboxyl group of the obtained acrylic polymer is subjected to an esterification reaction with a part of the epoxy group in the epoxy resin in the presence of a basic compound as a catalyst to obtain an acrylic modified epoxy resin.
[0089] (c) Direct polymerization method: a method in which a part of the epoxy groups in the epoxy resin is subjected to an esterification reaction with the carboxyl groups of a carboxyl group-containing monomer such as (meth)acrylic acid, and the reaction product is copolymerized with an ethylenically unsaturated monomer containing the carboxyl group-containing monomer as an essential component to obtain an acrylic modified epoxy resin.
[0090] In addition, the acrylic modified epoxy resin (C) can also be obtained by combining the above methods. For example, there can be mentioned a method in which an ethylenically unsaturated monomer is polymerized in the presence of an epoxy resin to perform graft polymerization, and then a basic compound is added to perform an esterification reaction; or a method in which an ethylenically unsaturated monomer is polymerized in the presence of a reaction product of an epoxy resin and (meth)acrylic acid to perform direct polymerization, and then an esterification reaction is performed.
[0091] (Ethylenically unsaturated monomer)
[0092] In the present embodiment, it is preferable to use a carboxyl group-containing monomer and other ethylenically unsaturated monomers as the ethylenically unsaturated monomer used for acrylic acid modification of the epoxy resin.
[0093] Examples of the carboxyl group-containing monomer include (meth)acrylic acid, maleic acid, itaconic acid, and fumaric acid.
[0094] Examples of other ethylenically unsaturated monomers include:
[0095] Alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate;
[0096] Ethylenically unsaturated monomers having a hydroxyl group, such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, hydroxypentyl (meth)acrylate, and hydroxyhexyl (meth)acrylate;
[0097] Aromatic monomers such as styrene and methyl styrene;
[0098] N-hydroxyalkyl (meth)acrylamide such as N-hydroxymethyl (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, N-hydroxybutyl (meth)acrylamide;
[0099] N-alkoxyalkyl (meth)acrylamide such as N-methoxymethyl (meth)acrylamide, N-ethoxymethyl (meth)acrylamide, N-(n-, iso-)butoxymethyl (meth)acrylamide, N-methoxyethyl (meth)acrylamide, N-ethoxyethyl (meth)acrylamide, and N-(n-, iso-)butoxyethyl (meth)acrylamide;
[0100] And (meth)acrylamide, etc.
[0101] If the solution stability of acrylic modified epoxy resin (C), the coating adaptability of coating, the processability when forming a coating film or the close adhesion with the frame are taken into account, the ethylenically unsaturated monomer is preferably deployed in a manner such that its carboxyl concentration becomes 2.7mmol / g~7.1mmol / g. If the carboxyl concentration is less than 2.7mmol / g, the water dispersibility decreases, and the storage stability as a water-based coating is sometimes impaired. On the other hand, if the carboxyl concentration is greater than 7.1mmol / g, it is sometimes difficult to obtain the processability, metal close adhesion, and durability when forming a protective film. In addition, the carboxyl concentration in the present embodiment is a theoretical value obtained from the amount of carboxyl-containing monomers contained in the deployment composition of the ethylenically unsaturated monomer, and refers to the number of moles of carboxyl groups present per unit weight.
[0102] The ethylenically unsaturated monomer is preferably used in a weight ratio of ethylenically unsaturated monomer / epoxy resin = 10 / 90 to 50 / 50. If the weight ratio of the ethylenically unsaturated monomer is less than 10, the solution stability may decrease or the coating property may be poor. In addition, if the weight ratio of the ethylenically unsaturated monomer is greater than 50, the processability, adhesion to the frame, and durability of the protective film may be poor.
[0103] As the free radical polymerization initiator used when polymerizing the ethylenically unsaturated monomer, for example, organic peroxides, persulfates, azobis compounds, and redox systems in which these are combined with a reducing agent are preferably used. In the present embodiment, a peroxide-based initiator is preferred, and benzoyl peroxide is particularly preferred.
[0104] The free radical polymerization initiator is preferably used in an amount of 1 to 10 parts by weight, more preferably 1 to 6 parts by weight, relative to 100 parts by weight of the total ethylenically unsaturated monomers. In addition, the reaction conditions such as temperature and time during polymerization are not special, and known conditions can be used. It is important to appropriately adjust the reaction conditions so that the viscosity characteristics when the water-based coating is made are optimal, thereby obtaining an acrylic modified epoxy resin.
[0105] In the above method, examples of the basic compound used as a catalyst in the esterification reaction include alcoholamines such as dimethylethanolamine (dimethylaminoethanol), ethanolamine, diethanolamine, and aminomethylpropanol, alkylamines such as trimethylamine, triethylamine, and butylamine, morpholine, and ammonia.
[0106] The basic compound is preferably used in the reaction in a ratio of 1 mol to 80 mol, more preferably 5 mol to 60 mol, relative to 100 mol of the carboxyl group-containing monomer. In addition, the reaction conditions such as temperature and time during the esterification reaction are not special and can be carried out under known conditions, but it is important to appropriately adjust the reaction conditions so that the fluidity of the obtained water-based coating is optimal, thereby obtaining an acrylic modified epoxy resin (C).
[0107] In order to make the obtained acrylic modified epoxy resin (C) into an aqueous dispersion, it can be obtained in the same manner as a conventional method. Specifically, it is a method of neutralizing the carboxyl groups present in the acrylic modified epoxy resin (C) with a basic compound or the like to impart hydrophilicity. More specifically, there can be exemplified a method of adding a basic compound to the acrylic modified epoxy resin (C) and then adding an aqueous medium such as water to make an aqueous dispersion, or a method of adding an aqueous medium such as water containing a basic compound to the acrylic modified epoxy resin (C) to make an aqueous dispersion, etc.
[0108] (Organic Solvent)
[0109] In order to improve the coating properties, the coating material used for forming the protective film of the present embodiment preferably contains an organic solvent, and in particular, in a water-soluble or water-dispersible aqueous coating material, it is preferred that 5 to 30% by weight of an organic solvent be contained.
[0110] The organic solvent may be contained directly in the reaction step when obtaining the acrylic modified epoxy resin (C), or may be added separately as needed.
[0111] The organic solvent is not particularly limited, but in water-based coatings, preferably a solvent with a relatively high hydrophilicity as shown below. Specifically, for example, the following can be cited:
[0112] Alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-pentanol, sec-pentanol, n-octanol, 2-ethyl-1-hexanol, and tridecanol;
[0113] Diols such as ethylene glycol, diethylene glycol, 1,3-butanediol, etc.
[0114] Glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, methyl propylene glycol, methyl propylene diglycol, propyl propylene glycol, propyl propylene diglycol, butyl propylene glycol, and dipropylene glycol monomethyl ether;
[0115] Acetic esters such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, 3-methoxybutyl acetate, ethylene glycol monobutyl ether acetate, and 3-methyl-3-methoxybutyl acetate.
[0116] In the present embodiment, in particular, in a water-dispersible water-based paint, from the viewpoint of storage stability and solvent volatilization rate during coating, the organic solvent used is preferably an alkylene glycol monoalkyl ether having an alkyl group with 1 to 6 carbon atoms, or an alkyl alcohol having an alkyl group with 1 to 10 carbon atoms, and more preferably a combination of the two.
[0117] On the other hand, in solvent-based coatings, it is not limited to the above. In particular, in terms of dissolving epoxy resins, ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, diacetone alcohol, and isophorone are suitable, and in order to impart coating properties, petroleum-based aromatic hydrocarbons and the glycol ethers listed above can be appropriately combined and used.
[0118] Examples of petroleum-based aromatic hydrocarbons include Swasol 1000, Swasol 1500, and Swasol 1800 manufactured by Maruzen Petrochemical, Ipzole 100 and Ipzole 150 manufactured by Idemitsu Kosan, and T-SOL 100 and T-SOL 150 manufactured by ENEOS.
[0119] As the solvent structure in the solvent-based coating, in a total of 100 parts by weight of the solvent, preferably 10 to 50 parts by weight of ketones, 10 to 50 parts by weight of glycol ethers, and 10 to 50 parts by weight of petroleum aromatic hydrocarbons, and more preferably 20 to 40 parts by weight of ketones, 20 to 40 parts by weight of glycol ethers, and 20 to 40 parts by weight of petroleum aromatic hydrocarbons.
[0120] (Hardener)
[0121] To the protective film-forming coating material, one or two or more hardeners such as phenol resins and amino resins may be further added in order to improve the curability of the coating film or the metal adhesion, as necessary.
[0122] (Phenol resin (D))
[0123] In addition to the self-crosslinking reaction, the phenol resin (D) can also react with the carboxyl groups in the acrylic modified epoxy resin (C). In addition, when the acrylic modified epoxy resin has hydroxyl groups, the phenol resin can also react with these hydroxyl groups. Furthermore, when the ethylenically unsaturated monomers include amide monomers and the acrylic modified epoxy resin (C) has crosslinking functional groups derived from the amide monomers, it can also react with these crosslinking functional groups.
[0124] As the phenol resin used in the present embodiment, there can be mentioned a resin obtained by reacting a trifunctional phenol compound such as phenol, m-cresol, 3,5-dimethylphenol, or a difunctional phenol compound such as o-cresol, p-cresol, p-tert-butylphenol with formaldehyde in the presence of a base catalyst, etc. In this case, the phenol compound can be used alone or in combination of two or more.
[0125] The phenol resin (D) is also preferably used in a form in which a part or all of the methylol groups generated by the addition of formaldehyde are etherified with an alcohol having 1 to 12 carbon atoms.
[0126] When the phenol resin (D) is used, it is preferably used in an amount of 0.5 to 20 parts by weight, more preferably 1 to 10 parts by weight, based on 100 parts by weight of the main agent, for example, the acrylic modified epoxy resin (C).
[0127] The phenol resin (D) is preferably used in an amount of 0.5 to 20 parts by weight, more preferably 1 to 10 parts by weight, based on 100 parts by weight of the acrylic resin (A).
[0128] The phenol resin (D) is preferably used in an amount of 5 to 40 parts by weight, more preferably 10 to 30 parts by weight, based on 100 parts by weight of the epoxy resin (B).
[0129] (Amino resin (E))
[0130] The amino resin (E) in the present embodiment refers to a resin in which an aldehyde compound is added to a part or all of the amino groups of the amino component to generate N-methylol groups and a condensation reaction is performed, and then a part or all of the generated N-methylol groups are subjected to a dehydration reaction with an alcohol to etherify to generate N-alkoxymethyl groups. The amino resin (E) can react with the acrylic resin (A) or the epoxy resin (B) and the acrylic modified epoxy resin (C), and thus functions as a curing agent.
[0131] Examples of the amino component include urea, melamine, benzoguanamine (another name: 2,4-diamino-6-phenyl-1,3,5-triazine), acetoguanamine, steroidal guanamine, spiroguanamine, dicyandiamide, etc. In addition, melamine-benzoguanamine cocondensates obtained by reacting melamine with benzoguanamine are also included.
[0132] Examples of the aldehyde compound include formaldehyde, paraformaldehyde, acetaldehyde, and benzaldehyde.
[0133] The alcohol used for N-methylol etherification is preferably a monohydric alcohol having 1 to 6 carbon atoms, and more preferably methanol, ethanol, isobutanol, or n-butanol. The alcohol may be used alone or in combination of two or more.
[0134] Among these, urea, melamine, melamine-benzoguanamine cocondensate, and benzoguanamine are preferably used as the amino component from the viewpoint of the hardness and abrasion resistance of the coating film. The amino resin may be used alone or in combination of two or more.
[0135] The amino resin (E) may be a commercially available product, for example: Cymel 301, 303LF, 304, 323, 325, 328, 370, 659, 1123 manufactured by Allnex;
[0136] Luwipal 014, 015, 018, 066, 070, 052, B017 manufactured by BASF;
[0137] Amidia P-138, Amidia L-105-60, Amidia L-109-65, Amidia L-110-60, Amidia TD-126, Amidia 15-594 manufactured by DIC Corporation;
[0138] Meran 11E, Meran 20, Meran 2029S, Meran 27, Meran 3100K, Meran 33, Meran 36E, Meran 322, Meran 3270, Meran 358D, Meran 359S, Meran 3601, Meran 366, Meran 3708K, Meran 3711, Meran 5757BS, etc. manufactured by Showa Denko Materials Co., Ltd.
[0139] In the protective film forming coating material of the present embodiment, when the acrylic resin (A) is used as the main agent, the amino resin (E) is preferably 25 to 230 parts by weight, more preferably 40 to 150 parts by weight, based on 100 parts by weight of the acrylic resin (A).
[0140] When the epoxy resin (B) is used as the main agent, the amino resin (E) is preferably 5 to 40 parts by weight, more preferably 10 to 25 parts by weight, based on 100 parts by weight of the epoxy resin (B).
[0141] When an acrylic modified epoxy resin (C) is used as the main agent, the amino resin (E) is preferably used in an amount of 30 parts by weight or less, more preferably 1 to 20 parts by weight, based on 100 parts by weight of the acrylic modified epoxy resin (C).
[0142] The protective film-forming coating material in the present embodiment may contain a curing catalyst as needed. The curing catalyst is preferably an acid catalyst.
[0143] Examples of the acid catalyst include p-toluenesulfonic acid, dodecylbenzenesulfonic acid, dinonylnaphthalenesulfonic acid, phosphoric acid, and end-capped types of these acids that are capped with a basic compound.
[0144] The acid catalyst is preferably used in an amount of, for example, 0.001 to 1.0 parts by weight relative to 100 parts by weight of the total of the main agent and the curing agent. The acid catalyst may be used alone or in combination of two or more.
[0145] (wax)
[0146] The wax used in this embodiment is used to ensure abrasion resistance. The wax is dispersed in the coating material for forming a protective film.
[0147] As such wax, animal and plant waxes such as lanolin and carnauba, paraffin, microcrystalline wax, petrolatum such as white vaseline, and synthetic wax-based polyethylene wax can be used. In order to obtain high wear resistance, granular wax is preferred. In the present embodiment, polyethylene wax having a high melting point and being present in the form of particles in the coating film after drying and hardening is preferably used.
[0148] The particle size of the polyethylene wax can be an average particle size of about 3 μm to 6 μm. If the particle size is too large, the cured coating film itself will be in the form of hard spots, the appearance and feel of the coating film will deteriorate, and it cannot be used as a protective film. On the other hand, if the particle size is too small, it will be embedded in the coating film and the wear resistance will not be exerted, which is not preferred.
[0149] The average particle size is a volume average particle size, which can be measured by a conventionally known method such as laser diffraction.
[0150] The amount of polyethylene wax used is preferably 4 to 25 parts by weight relative to 100 parts by weight of the main agent and the curing agent. If it is less than 4 parts by weight, it is difficult to obtain sufficient wear resistance of the protective film, while if it is more than 25 parts by weight, the strength of the protective film is likely to decrease.
[0151] (Inorganic filler)
[0152] The inorganic filler used in the present embodiment is added to the coating material for forming a protective film in order to adjust the FI or glossiness of the protective film.
[0153] As the type of inorganic filler, various inorganic substances can be listed, but there is no particular limitation, and silica particles are preferred. The shape of the silica particles is not particularly limited, and spherical, hollow, porous, rod-shaped, plate-shaped, fibrous or indefinite silica particles can be used, wherein silica particles that can be easily dispersed in water-based paint are preferred.
[0154] Examples of commercially available products that can be used as the silica fine particles include Sylysia series (Sylysia 250N, Sylysia 350, Sylysia 370, Sylysia 380, Sylysia 420, Sylysia 440, etc.) manufactured by Fuji-Silysia Co., Ltd., Sylysia 420, Sylysia 440, etc.), Sylysia 420, Sylysia 440, etc., ... Sylophobic series ("Sylophobic 100", "Sylophobic 200", "Sylophobic 702", "Sylophobic 4004", etc.), Sylosphere series ("Sylosphere 1504", "Sylosphere 1510", etc.), SYLOID series manufactured by Grace Japan ("SYLOID W300", "SYLOID W500", etc.), Evonic Degussa (Evonic Japan) The ACEMATT series manufactured by Degussa Japan ("ACEMATT HK460", "ACEMATT HK400", "ACEMATT OK412", "ACEMATT OK520", "ACEMATT OK607", "ACEMATT TS100", "ACEMATT 3200", "ACEMATT 3300", "ACEMATT 3600", etc.), the NIPGEL series manufactured by Nippon Silica Industries ("NIPGEL The products include: the NIPSIL series ("NIPSIL E-200A", "NIPSIL SS-50B", "NIPSIL SS-178B", etc.), the Mizukasil series ("Mizukasil P-73", "Mizukasil P-526", etc.) manufactured by Mizusawa Chemical Co., Ltd., and the AEROSIL series ("AEROSIL 200", "AEROSIL R805" and "AEROSIL R972", etc.) manufactured by Aerosil Co., Ltd.
[0155] The average particle size of the silica particles is not particularly limited, but is preferably 2 to 9 μm, more preferably 3 to 7 μm. If the average particle size is less than 2 μm, the matte function is likely to be insufficient, and if it is greater than 9 μm, it is likely to become hard spots when the coating dries and remain on the protective film.
[0156] In addition, the average particle size is a volume average particle size.
[0157] The amount of silica particles used is preferably 1 to 25 parts by weight relative to 100 parts by weight of the total of the main agent and the hardener. If it is less than 1 part by weight, the matte function is likely to be insufficient, while if it is more than 25 parts by weight, the viscosity of the coating becomes too high, the fluidity decreases, and the coating becomes difficult. Furthermore, the dispersion of the filler becomes insufficient, and when the coating dries, it is easy to become a hard spot and remain on the protective film.
[0158] Similar to the inorganic filler, polymer microparticles can also be used to adjust FI or glossiness. The addition amount and average particle size are suitable for the same range as the inorganic filler. Inorganic fillers and polymer microparticles can also be used together.
[0159] (Other ingredients)
[0160] The protective film-forming coating material of the present embodiment may contain various additives such as a surfactant and a defoaming agent as needed.
[0161] (Painting method)
[0162] The coating method may be roll coating, spray coating, curtain coating, spin coating, die coating, dip coating or the like, but is not particularly limited and may be appropriately selected according to the purpose.
[0163] (Sintering conditions)
[0164] In order to obtain the protective film of the present embodiment, the applied paint needs to be baked. As a baking method, an electric oven, an infrared oven, a gas oven, etc. can be used appropriately.
[0165] The sintering temperature is preferably 180°C to 220°C, more preferably 190°C to 200°C. The sintering time is preferably 40 seconds to 120 seconds, more preferably 50 seconds to 80 seconds. If the sintering temperature exceeds 220°C, or the sintering time is longer than 120 seconds, the coating film tends to be colored with a yellow tint, which is inappropriate as the appearance of the frame. In addition, if the sintering temperature is lower than 180°C, or the sintering time is shorter than 40 seconds, the drying and hardening properties of the coating tend to become insufficient, and the performance of the protective film such as abrasion resistance or solvent resistance is reduced.
[0166] [Frame]
[0167] As the raw material of the base material of the frame, various metals such as aluminum, magnesium, titanium, or a composite resin system of polycarbonate resin and acrylonitrile-butadiene-styrene resin are used, but aluminum or magnesium is more preferred in notebook personal computers or smart phones that emphasize the balance between strength, portability, and cost. The thickness of the frame base material is not particularly limited, but it is preferably 0.2 mm to 0.8 mm because it is necessary to take both strength and portability into consideration.
[0168] The frame substrate may also have a coating layer. The coating layer may be formed by a single layer or by multiple layers. As an example formed by multiple layers, a resin layer (primer coat) having a pearlescent pigment or a coloring pigment is provided on the surface of the frame substrate according to the desired glossiness and mattness, and a laminated structure of a resin layer (top coat) having a sense of transparency is formed thereon.
[0169] The example in which the coating layer is formed of a single layer is used when a resin layer that does not need to be colored is formed, and in order to impart transparency, the coating layer is formed of a single resin layer containing no filler or containing an inorganic filler.
[0170] When the frame substrate has a coating layer, the protective film is formed on the coating layer. The protective film only needs to be present on at least the outer side surface of the frame, and may also be present on the inner side surface.
[0171] [Electronic equipment]
[0172] In the electronic device of the present embodiment, the electronic components are housed in the interior of the housing covered with the protective film of the present embodiment. The shape, structure, size, etc. thereof can be appropriately selected.
[0173] The electronic components to be stored include circuit boards, transistors, integrated circuits (ICs), central processing units (CPUs), and the like.
[0174] The electronic device is not particularly limited, and examples thereof include personal computers (notebook personal computers, desktop personal computers), telephones, smart phones, copiers, fax machines, various printers, digital cameras, televisions, video recorders, compact disc (CD) devices, digital versatile disc (DVD) devices, etc. Among these, notebook personal computers and smart phones are particularly preferred in terms of portability.
[0175] [Example]
[0176] The present embodiment is further described using examples and comparative examples. Unless otherwise specified, as the unit of the amount of preparation, "part" means "part by weight" and "%" means "% by weight". Unless otherwise specified, the amount of the raw materials (excluding the solvent) described in the example and the table is the non-volatile component conversion value.
[0177] [Production Example 1]
[0178] <Production of phenol resin (D) solution>
[0179]
[0180]
[0181] (8) 120 parts of ion exchange water were used for each washing. Wash four times.
[0182] (9) 52 parts of n-butanol
[0183] Place (1) to (4) in a four-necked flask, react at 60°C for 3 hours under a nitrogen flow, then add (5) and (6) and cool. After cooling to below 55°C, use (7) to adjust the pH to 5. After standing for about 30 minutes and discarding the aqueous phase, use (8) to wash with water. Washing with water is performed by repeating the following operation four times: add (8) and stir for 15 minutes, let it stand for 15 minutes, and then discard the aqueous phase. After the water washing is completed, add (9) for dehydration reaction to obtain a phenol resin (D) solution with a non-volatile component concentration of 50%.
[0184] [Production Example 2]
[0185] <Preparation of base paint 1>
[0186]
[0187]
[0188] (20) 21 parts of the phenol resin (D) solution obtained in Preparation Example 1
[0189] Place (1) to (6) in a four-necked flask, raise the internal temperature to 125°C, and react under a nitrogen stream. Cool when the acid value reaches 0.2 mgKOH / g or less, and add (7) and (8) at 115°C. Add the premixed mixture of (9) to (12) to the dropping funnel dropwise at 117°C to 123°C over 1 hour. After the addition is complete, add (13), (14), and (15) every 45 minutes while maintaining the internal temperature at 117°C to 120°C. Start cooling 45 minutes after the addition of (15), and add the premixed (16) and (17) dropwise over 30 minutes after the temperature reaches 80°C, and then add (18) dropwise over 50 minutes. After standing for a day and night, add Surfynol 104A manufactured by Nissin Chemical Industry Co., Ltd. as (19) and stir. (20) was added and stirred to obtain a base coating material 1 having a non-volatile content concentration of 24%.
[0190] [Production Example 3]
[0191] <Preparation of base paint 2>
[0192]
[0193] (1) to (4) were placed in a four-necked flask, the internal temperature was raised to 90°C, and the mixture was dissolved under a nitrogen stream. After confirming the dissolution, the mixture was cooled to 40°C or less, and the amino resin (E-1) of (5) Meran 11E (manufactured by Showa Denko Materials Co., Ltd.) was mixed and stirred to obtain a base coating 2 having a non-volatile content concentration of 40%.
[0194] [Production Example 4]
[0195] <Preparation of base coating 3>
[0196]
[0197] (1) to (4) were placed in a four-necked flask, the internal temperature was raised to 100°C, and the mixture was dissolved under a nitrogen stream. After confirming the dissolution, the mixture was cooled to 40°C or less, and Meran 11E as the amino resin (E-1) (5) was mixed and stirred to obtain a base coating 3 having a nonvolatile content concentration of 35%.
[0198] [Production Example 5]
[0199] <Synthesis of acrylic resin (A-1)>
[0200] 24.55 parts of diethylene glycol monobutyl ether were placed in a reaction vessel including a thermometer, a stirrer, a reflux cooler, a drip tank, and a nitrogen blowing tube, and stirring was carried out while introducing nitrogen. At the same time, heating was started, and at an internal temperature of 100°C, 45.23 parts of a mixture containing 11.42 parts of N-butoxymethyl acrylamide, 5.53 parts of lauryl methacrylate, 2.21 parts of acrylic acid, 11.05 parts of methyl methacrylate, 6.63 parts of ethyl acrylate, 2.21 parts of benzoyl peroxide, and 8.39 parts of propylene glycol monomethyl ether were uniformly dripped from the drip tank over 2 hours. Thereafter, the internal temperature was heated to 110°C and reacted for 30 minutes. Subsequently, 0.15 parts of benzoyl peroxide was added, the internal temperature was heated to 115°C, and the reaction was carried out for 30 minutes. Furthermore, 0.15 parts of benzoyl peroxide was added, the internal temperature was heated to 120°C, and the reaction was terminated after 30 minutes. Propylene glycol monomethyl ether was distilled off at 120° C. to 110° C. under reduced pressure until the nonvolatile content of the reaction system reached 63%. Thereafter, 3.18 parts of N,N-dimethylethanolamine and ion exchange water were added in appropriate amounts to obtain a solution of acrylic resin (A-1) having a nonvolatile content of 42%.
[0201] [Production Example 6]
[0202] <Synthesis of acrylic resin (A-2)>
[0203] 30.94 parts of diethylene glycol monobutyl ether were placed in a reaction vessel including a thermometer, a stirrer, a reflux cooler, a drip tank, and a nitrogen blowing tube, and nitrogen was introduced while stirring. At the same time, heating was started. At an internal temperature of 120°C, 57.58 parts of a mixture of 17.69 parts of N-butoxymethyl acrylamide, 6.19 parts of lauryl methacrylate, 2.21 parts of acrylic acid, 17.69 parts of methyl methacrylate, 0.44 parts of ethyl acrylate, 1.99 parts of benzoyl peroxide, and 11.37 parts of propylene glycol monomethyl ether were uniformly dripped from the drip tank in 2 hours. Thereafter, the reaction was carried out for 30 minutes. Subsequently, 0.17 parts of benzoyl peroxide were added and the reaction was carried out for 30 minutes. Furthermore, 0.17 parts of benzoyl peroxide were added and the reaction was terminated after 30 minutes. Propylene glycol monomethyl ether was removed by distillation at 120°C to 110°C under reduced pressure until the non-volatile component concentration of the reaction system reached 61%. Thereafter, appropriate amounts of 2.73 parts of N,N-dimethylethanolamine and ion-exchanged water were added to obtain a solution of an acrylic resin (A-2) having a nonvolatile content concentration of 50%.
[0204] [Production Example 7]
[0205] <Preparation of base coating 4>
[0206]
[0207]
[0208] Mix (1) to (5) in a mixing container and stir. As amino resin (E-2) of (4), Meran 3708K manufactured by Showa Denko Materials is used. After stirring for about 15 minutes, add (6). While stirring, add a small amount of Tegoglide 450 manufactured by Evonik Industries as (7) in the mixing container, and continue stirring to obtain a base coating 4 with a non-volatile component concentration of 45%.
[0209] [Production Example 8]
[0210] <Preparation of base paint 5>
[0211]
[0212] Use a mixing container to mix (1) to (6) and stir. As the amino resin (E-2) of (5), Meran 3708K manufactured by Showa Denko Materials is used, and as the amino resin (E-3) of (6), Meran 5757BS manufactured by Showa Denko Materials is used. After stirring for about 15 minutes, add (7). While stirring in the mixing container, add a small amount of Tegoglide 450 manufactured by Evonik Industries as (8), and continue stirring to obtain a base coating 5 with a non-volatile component concentration of 49%.
[0213] [Material]
[0214] Prepare the following materials.
[0215] Silica particles 1: Amorphous silica particles manufactured by Fuji Silicon Chemical
[0216] "SYLYSIA 420" average particle size 2.7μm
[0217] Silica particles 2: Amorphous silica particles manufactured by Fuji Silicon Chemical
[0218] "SYLYSIA 350" average particle size 3.9μm
[0219] Silica particles 3: Amorphous silica particles manufactured by Fuji Silicon Chemical
[0220] "SYLYSIA 250N" average particle size 5.0 μm
[0221] Silica particles 4: Amorphous silica particles manufactured by Fuji Silicon Chemical
[0222] "SYLYSIA 370" average particle size 6.4μm
[0223] Silica particles 5: Amorphous silica particles manufactured by Fuji Silicon Chemical
[0224] "SYLYSIA 380" average particle size 9.0 μm
[0225] Polyethylene wax: "MPP-611AL" manufactured by MicroPowders, average particle size 4.5 μm, melting point 112°C
[0226] [Examples, Comparative Examples]
[0227] The polyethylene wax was added to 416.7 parts (based on 100 parts of the resin component) of the base coating material 1 (non-volatile content 24%) prepared in Production Example 2, and stirred for 10 minutes with a mixer. Subsequently, silica fine particles were added, and stirred for 10 minutes with a mixer.
[0228] For other manufacturing examples 3 (base coating 2, non-volatile component concentration 40%), manufacturing example 4 (base coating 3, non-volatile component concentration 35%), manufacturing example 7 (base coating 4, non-volatile component concentration 45%), and manufacturing example 8 (base coating 5, non-volatile component concentration 49%), the protective film forming coating was prepared using the same method as manufacturing example 2, based on the resin component of each base coating reaching 100 parts.
[0229] The obtained coating was applied to an aluminum plate having a thickness of 0.24 mm using a wire bar coater and sintered in an oven set at 190° C. for 1 minute to obtain a protective film having the film thickness described in the table. For the comparative examples, the same coating and sintering conditions as described in the table were also used.
[0230] In addition, for the purpose of measuring Sa and Sdq, a 0.24 mm thick electrolytic tinned steel sheet (Steel Plate Tin Electrolytic, SPTE) (tin adhesion 5.6 g / m 2 )Tin-plated iron material.
[0231] [Evaluation of physical properties of protective film]
[0232] The coated plates obtained in Examples and Comparative Examples were evaluated for various properties of the protective films in the items shown below.
[0233] [FI]
[0234] The coating film surface was measured using a multi-angle colorimeter "BYK-mac i" manufactured by BYK Instruments.
[0235] [60° gloss]
[0236] The coating film surface was measured using a gloss meter "VG7000" manufactured by Nippon Denshoku Industries Co., Ltd.
[0237] [Evaluation method of wear resistance]
[0238] The number of times when the wear of the base material began to be observed was recorded and evaluated using a Model 7RCA Abrasion Wear TESTER manufactured by Norman Tool.
[0239] <Evaluation Criteria>
[0240] (Excellent): 30 times or more
[0241] ○(Good): 10 times to 29 times
[0242] ×: (Not applicable) Less than 9 times
[0243] [Evaluation method of solvent resistance]
[0244] The gauze folded in four was fixed to a 2-pound hammer, and methyl ethyl ketone as a solvent was impregnated to wipe the protective film. The number of reciprocating strokes of the hammer until the base material began to be observed was recorded and evaluated.
[0245] <Evaluation Criteria>
[0246] (Excellent): More than 200 times
[0247] ○(Good): 50 times to 199 times
[0248] ×: (Not applicable) Less than 49 times
[0249] [Dynamic friction coefficient]
[0250] The friction coefficient was measured using an AB-401 friction coefficient measuring machine manufactured by Tester Sangyo Co., Ltd. in accordance with the method described in JIS K-7125. Specifically, a three-point supported stainless steel ball with a load of 1 kg was used and the measurement was performed at a tensile speed of 100 mm / min.
[0251] [Sa、Sdq]
[0252] Sa and Sdq of the protective film were determined according to the method described in ISO 25178-2: 2012. Specific measurement conditions are shown below.
[0253] (1) Microscope: OPTELICS HYBRID+ laser microscope manufactured by Laser Technology Co., Ltd.
[0254] (2) Image analysis software: software included with the microscope
[0255] (3) Observation magnification: 50 times
[0256] The evaluation results are shown in Tables 1 to 4.
[0257] Table 1
[0258]
[0259] Table 2
[0260]
[0261] Table 3
[0262]
[0263] Table 4
[0264]
[0265] [Summary of Results]
[0266] In Example 1, in the base coating 1 (water-dispersible acrylic modified epoxy resin), the added amount of silica particles 2 was 10 parts by weight relative to the total of 100 parts by weight of the main agent and the hardener, and 4 parts by weight of polyethylene wax were added, and the FI, 60° gloss, abrasion resistance, and solvent resistance were all good.
[0267] In Examples 2 to 5, the particle size of the silica fine particles in the base coating material 1 was varied. As the particle size increased, the FI decreased, but the abrasion resistance and solvent resistance were both at acceptable levels.
[0268] In Examples 6 to 11, the amount of polyethylene wax added to the base coating 1 was varied. As the amount added increased, the FI and 60° gloss decreased, but the solvent resistance and abrasion resistance were both at acceptable levels, and a protective film with particularly excellent abrasion resistance was obtained.
[0269] In Examples 12 to 17, the film thickness of the protective film in the base coating material 1 was varied. As the film thickness increased, the abrasion resistance and solvent resistance tended to improve. In particular, very excellent protective films were obtained when the film thickness was 8 μm or more.
[0270] In Examples 18 to 20, the particle size of the silica particles was varied in the base coating 2 (solvent-based epoxy resin). As the particle size increased, both the FI and 60° gloss decreased, but the abrasion resistance and solvent resistance were both at acceptable levels.
[0271] In Examples 21 to 23, the amount of silica particles with an average particle size of 3.9 μm added to the base coating 3 (solvent-based epoxy resin) was varied. As the amount added increased, both FI and 60° gloss decreased, but both abrasion resistance and solvent resistance were at acceptable levels.
[0272] In Examples 24 to 26, the amount of polyethylene wax added to the base coating 4 (water-soluble acrylic resin) was varied. As the amount added increased, the FI and 60° gloss both decreased, but the solvent resistance and abrasion resistance were both at acceptable levels. In particular, a protective film with very excellent abrasion resistance was obtained.
[0273] In Examples 27 to 29, the thickness of the protective film was varied in base coating 5 (water-soluble acrylic resin). As the film thickness increased, the wear resistance and solvent resistance tended to improve, and particularly when the film thickness was above 7 μm, a very excellent protective film could be obtained.
[0274] In Comparative Example 1, the protective film contained neither polyethylene wax nor silica particles, the 60° glossiness was too high, and the abrasion resistance was very poor, resulting in failure.
[0275] In Comparative Example 2, the protective film did not contain polyethylene wax, and the abrasion resistance was poor and unacceptable.
[0276] In Comparative Example 3, the amount of polyethylene wax added was increased to 30 parts, and the abrasion resistance was very excellent, but the solvent resistance was reduced and failed.
[0277] In Comparative Example 4, although the film thickness was set to 1 μm, the 60° glossiness was too high, and both the abrasion resistance and the solvent resistance were very poor, resulting in failure.
[0278] In Comparative Example 5, the particle size of the silica fine particles varied to the smallest 2.7 μm, and the physical properties and FI were at acceptable levels, but the 60° glossiness was too high and failed.
[0279] In Comparative Examples 6 and 7, the addition amount of the silica particles 2 of Example 1 was changed to 12.5 parts by weight and 15 parts by weight, respectively, relative to 100 parts by weight of the main agent and the hardener. The FI, abrasion resistance, and solvent resistance were all acceptable, but the 60° glossiness was insufficient.
[0280] The present invention is not limited to the above-described embodiments and examples, and design changes can be appropriately made without departing from the gist of the present invention.
Claims
1. A protective film is a protective film for a frame housing electronic components, wherein: The film thickness is 3μm or more, the dynamic index (Flop Index) (FI) is 9 to 13, and the glossiness at 60° is 10 to 50. The protective film is formed by a coating material for forming a protective film, wherein the coating material for forming a protective film comprises a main agent and a hardener. The coating material for forming a protective film comprises 1 to 25 parts by weight of silica particles having an average particle size of 3 to 9 μm and 4 to 25 parts by weight of polyethylene wax, based on 100 parts by weight of the main agent and the curing agent in total.
2. The protective film according to claim 1, wherein: The root mean square gradient (Sdq) of the surface is 1-10.
3. The protective film according to claim 1 or 2, wherein: The arithmetic mean height (Sa) of the surface is 0.1 μm to 1 μm.
4. The protective film according to claim 1 or 2, wherein: The dynamic friction coefficient of the surface is 0.05 to 0.
5. 5 . A frame body comprising the protective film according to claim 1 . 6 . An electronic device, wherein electronic components are housed inside the housing according to claim 5 .
Citation Information
Patent Citations
Precoat aluminum alloy sheet having excellent flaw resistance
JP2004098624A
Precoated aluminum alloy sheet for casing of electric and electronic equipment
JP2010228279A
Bright pigment with gold tone, and cosmetic, paint, ink or resin composition containing the same
CN101410462A
Metal oxide particles containing titanium oxide coated with silicon dioxide-tin(IV) oxide complex oxide?
CN103717535A
Curable resin composition using low-lactone modified hydroxyalkyl (Meth)Acrylic ester composition and coating material therefrom
JP2002167423A