A method of forging a rudder horn
By employing a sloping shoulder design and preheating processes, the problem of uneven stress distribution on the bent rudder stock was solved, improving its strength and fatigue resistance, as well as enhancing material utilization and connection stability.
Patent Information
- Application Number
- CN202310951898.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-31
- Publication Date
- 2026-05-12
- Estimated Expiration
- 2043-07-31
AI Technical Summary
The existing curved rudder stock has uneven stress distribution during processing, resulting in insufficient strength and fatigue resistance, as well as low material utilization.
The design employs a beveled shoulder, combined with preheating, forging, heat treatment, and surface treatment processes. This beveled shoulder reduces stress concentration, improves material utilization and connection stability, and enhances the overall structural strength and rigidity.
This resulted in a more uniform stress distribution, improved the strength and fatigue resistance of the bent rudder stock, reduced material loss, and enhanced connection tightness and overall structural stability.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of curved rudder stock technology, and in particular relates to a forging method for curved rudder stock. Background Technology
[0002] The rudder stock is a critical component on a ship, used to control the steering of the rudder and the operation of the steering gear. It is a rod-like structure connecting the steering gear and the rudder, transmitting the forces and torques generated by the steering gear to achieve ship maneuvering and steering. Rudder stocks are typically forged from high-strength steel or other alloy materials to ensure sufficient strength and rigidity to withstand the forces generated by the steering gear and the hydrodynamic loads on the ship during navigation.
[0003] The shape and size of a curved rudder stock vary depending on the size, type, and operational requirements of the vessel. Generally, a curved rudder stock has a cylindrical or flat rectangular cross-section with a specific length and diameter or width. Its length usually depends on the arrangement requirements of the rudder blades and the vessel to ensure sufficient turning angle within the operating range; the diameter or width of the curved rudder stock depends on the required strength and stiffness, as well as the load it will bear. The manufacturing process of a curved rudder stock generally includes forging, heat treatment, and machining. First, the selected steel is forged to improve the strength and density of the material. Then, heat treatment processes, such as annealing or normalizing, are performed to eliminate internal stress and improve the mechanical properties of the material. Finally, machining, including turning, milling, and grinding, is carried out according to design requirements to obtain the required geometric dimensions and surface precision. However, most existing curved rudder stock machining processes use right-angle chamfering, which results in uneven stress distribution. Summary of the Invention
[0004] The purpose of this invention is to address the problem that existing technologies using right-angle shoulder cutting suffer from uneven stress distribution, and to provide a forging method for curved rudder posts.
[0005] To address the existing problems, this invention provides a forging method for a bent rudder stock, comprising the following steps:
[0006] Step 1: Select steel billets with round or square cross-sections;
[0007] Step two: Preheat the steel billet;
[0008] Step 3, forging operation, including shoulder cutting with a chopping knife, lengthening, and bending; when cutting the shoulder with a chopping knife, a 200mm bevel is used; after shoulder cutting with a chopping knife, the blade is installed on a lengthening machine for lengthening; when bending, the bending rod is placed between a flat anvil and a V-shaped anvil and fixed with a clamp, and force is applied with a hammer.
[0009] Step four: After the forging operation is completed, the dimensions of the bent rudder stock are calibrated.
[0010] Step 5: After dimensional calibration, the bent rudder stock undergoes heat treatment;
[0011] Step 6: After heat treatment, perform a quality inspection on the bent rudder stock;
[0012] Step 7: After quality inspection, the surface of the curved rudder stock is treated and sprayed; the beveled surface of the angled shoulder can make the stress distribution more uniform and reduce the concentration of local stress, thereby improving the strength and fatigue resistance of the ship's curved rudder stock; the angled shoulder can reduce material loss during the cutting process.
[0013] As a further improvement to the above technical solution, the elongation is achieved by using mechanical force or hydraulic pressure to cause the bent rudder rod to elongate and deform. The force and speed of the elongation machine are adjusted to control the elongation deformation of the bent rudder rod. When the length of the forging exceeds 6 meters, the elongation is completed.
[0014] As a further improvement to the above technical solution, the ship's rudder stock is removed from the square-forming machine and installed on the angle-pressing machine; the angle-pressing machine is started to cause the two ends of the ship's rudder stock to bend at an angle; by adjusting the force and position of the angle-pressing machine, the angle and length of the angle at both ends of the rudder stock are controlled.
[0015] As a further improvement to the above technical solution, the bottom of the bent rudder stock is tilted towards the centerline during the pressing process; this minimizes the adverse effects of unbalanced weight distribution and allows for smooth lengthening to the forging process length.
[0016] As a further improvement to the above technical solution, in step three, the bending hammer head applies force from one side of the bending rudder, causing it to gradually bend into the target shape.
[0017] As a further improvement to the above technical solution, the hammer force is perpendicular to the axis of the bent rudder stock, ensuring that the position and positioning of the bent rudder stock meet the requirements.
[0018] As a further improvement to the above technical solution, in step six, the forged curved rudder stock is subjected to quality inspection, including dimensional inspection, non-destructive testing, and chemical composition analysis.
[0019] As a further improvement to the above technical solution, in step seven, the curved rudder stock after forging and heat treatment is surface treated by the following steps: cleaning the surface by using a cleaning agent and tools to clean the surface of the curved rudder stock and remove dirt and oxides generated during forging and heat treatment; shot peening the surface of the curved rudder stock by using shot peening equipment; and spraying an anti-corrosion coating to extend its service life.
[0020] As can be seen from the above technical solutions, the beneficial effects of this invention are: a 200mm beveled shoulder can reduce stress concentration between the shoulder and the axis of the ship's rudder stock. Compared to a right-angle shoulder, the beveled surface of the beveled shoulder allows for a more uniform stress distribution, reducing local stress concentration and thus improving the strength and fatigue resistance of the ship's rudder stock; the beveled shoulder can reduce material loss during the cutting process. Through the design of the beveled shoulder, the amount of material required for cutting can be reduced without decreasing the shoulder length, improving material utilization; simultaneously, the beveled shoulder can improve the connection between the shoulder and other components. The design of the beveled shoulder can increase the contact area between the shoulder and connecting components, improving the tightness and stability of the connection, thereby enhancing the overall structural strength and rigidity of the ship's rudder stock.
[0021] When pressing the pin, tilt the bottom of the bent rudder stick towards the center line to minimize the adverse effects of unbalanced weight distribution and smoothly extend it to the forging process length.
[0022] Preheating promotes the homogenization of the internal structure of steel, reducing the likelihood of stress concentration and stress corrosion. Preheating can reduce the deformation energy and force requirements during forging, making forging easier. By improving the plasticity and toughness of steel, preheating can reduce the strain rate and deformation stress in the forging process, thus reducing energy consumption and equipment load. Detailed Implementation
[0023] To make the objectives, features, and advantages of this invention more apparent and understandable, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the embodiments described below are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this patent, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this patent.
[0024] This invention discloses a forging method for a bent rudder stock, comprising the following steps:
[0025] Step one: Select a suitable high-strength steel for the ship's rudder stock, such as marine steel or special steel, ensuring that the material meets design and specification requirements. Based on the rudder stock bending requirements, process the selected steel into a suitable blank shape; in this application, a circular or square cross-section is used.
[0026] Step two, preheating: Before forging, the steel billet is appropriately preheated to improve its plasticity and toughness. The preheating temperature is above the critical temperature; in this embodiment, the preheating temperature range is 400℃ to 600℃. Preheating within this range improves plasticity and toughness, making it easier to deform during forging and reducing the risk of cracking and fracture. It also helps improve the hot deformation characteristics of the steel, making it more susceptible to mechanical deformation and forming. Preheating also reduces internal stress, eliminating or mitigating internal stresses, and promoting a more homogenized internal structure, reducing the likelihood of stress concentration and stress corrosion. Furthermore, preheating reduces the deformation energy and force requirements during forging, making the process easier. By improving the plasticity and toughness of the steel, preheating reduces the strain rate and deformation stress in the forging process, decreasing energy consumption and equipment load.
[0027] Step 3, forging operation.
[0028] Place the preheated steel billet on forging equipment (such as a hammer or press); perform forging operations on the steel billet, including cutting the shoulder with a cutting tool, drawing, and bending.
[0029] When cutting the shoulder with a cutting tool, use measuring tools and a ruler to mark the positions of the cutting tool and the shoulder on the rudder stock. A 200mm bevel cut is used during shoulder cutting. This 200mm bevel cut reduces stress concentration: it reduces stress concentration between the shoulder and the axis of the rudder stock. Compared to a right-angle shoulder cut, the bevel allows for a more uniform stress distribution, reducing localized stress concentration and thus improving the strength and fatigue resistance of the rudder stock. The bevel cut also reduces material loss during the cutting process. By designing a bevel cut, the amount of material required for cutting can be reduced without decreasing the shoulder length, improving material utilization. Simultaneously, the bevel cut improves the connection between the shoulder and other components. The bevel cut design increases the contact area between the shoulder and connecting components, improving the tightness and stability of the connection, thereby enhancing the overall structural strength and rigidity of the rudder stock.
[0030] During the lengthening process, the ship's curved rudder stock, after being trimmed by the lower chopping blade, is installed on the stretching machine and stably positioned and fixed; ensuring that the middle part of the curved rudder stock is aligned with the clamps of the stretching machine. The stretching machine is started, and mechanical or hydraulic force is used to stretch and deform the ship's curved rudder stock. The stretching deformation is controlled by adjusting the force and speed of the stretching machine, as well as adjusting the support position of the clamps. Lengthening is completed when the forging length exceeds 6 meters. After lengthening, the ship's curved rudder stock is removed from the stretching machine and installed on the beveling machine; the beveling machine is started, and appropriate force is applied to bevele both ends of the ship's curved rudder stock. The beveling angle and length at both ends of the curved rudder stock are controlled by adjusting the force and position of the beveling machine; to reduce the possibility of excessive weight causing the manipulator to malfunction and unable to rotate, the bottom surface of the curved rudder stock is tilted towards the centerline during beveling, minimizing the adverse effects of weight imbalance and successfully stretching to the forging process length.
[0031] During the bending process, prepare a flat anvil and a V-anvil, ensuring the spacing between them is suitable for the rudder stick's dimensions. Determine the target shape and angle for bending, and prepare the appropriate molds and tools according to design requirements and specifications. Prepare a flat hammer, selecting a suitable hammer size and shape to apply appropriate force during bending. Positioning and securing: Place the rudder stick between the flat and V-anvils, ensuring its position and positioning meet requirements. Use clamps or clamping devices to secure the rudder stick, preventing unnecessary movement or twisting during bending. Bending operation: Using the flat hammer, apply force starting from one side of the rudder stick, gradually bending it to the target shape. During bending, control the direction and intensity of the applied force; the direction of the applied force should be determined according to the desired bending shape and angle; the force should be perpendicular to the rudder stick's axis to produce the desired bending effect; the applied force should be gradually increased to control the deformation process of the rudder stick. Initially, apply a smaller force to avoid excessive deformation or damage to the rudder stick. As the bending progresses, the force can be gradually increased to achieve the desired bending angle. During the bending process, it may be necessary to apply force multiple times and make repeated adjustments to achieve the desired bending effect. After each adjustment, check the shape and angle of the bent rudder stock, compare it with the design requirements, and make further operations and adjustments as needed.
[0032] Inspection and repair:
[0033] After bending, the bent rudder stock is inspected, including an assessment of its bending shape, angle, dimensions, and surface quality. If necessary, adjustments are made to meet design and specification requirements. The bending process achieves the desired bending shape and angle for the rudder stock: by gradually applying force and making adjustments, the deformation of the rudder stock can be controlled to ensure it achieves the designed bending shape and angle.
[0034] Step 5, Size Calibration:
[0035] After forging, the bent rudder stock may have dimensional and shape deviations. If necessary, the bent rudder stock should be dimensionally calibrated to ensure it meets design requirements.
[0036] The size and shape of the bent rudder stock can be adjusted by cutting, trimming and grinding operations using machining equipment (such as milling machines, lathes, etc.).
[0037] Step Six, Heat Treatment:
[0038] After forging, the bent rudder stock undergoes appropriate heat treatment to eliminate internal stress and improve its strength and toughness. Common heat treatment methods include quenching and tempering; the appropriate heat treatment process is selected based on the type of steel and specifications.
[0039] Step 7, Inspection and Testing:
[0040] The forged curved rudder stock undergoes quality inspection, including dimensional checks, non-destructive testing, and chemical composition analysis. Physical performance tests, such as tensile and impact tests, are also performed to ensure the curved rudder stock meets design requirements and relevant specifications.
[0041] Step 8, Surface Treatment and Coating: The surface treatment of the forged and heat-treated bent rudder stock can be performed using the following steps:
[0042] Clean the surface: Use appropriate cleaning agents and tools to clean the surface of the bent rudder stock to remove dirt, oxides, etc. generated during forging and heat treatment.
[0043] Shot peening: The surface of the bent rudder stock is shot peened using shot peening equipment to remove surface oxides and improve roughness, providing good adhesion for subsequent coating.
[0044] Anti-corrosion coating: Select appropriate anti-corrosion coatings, such as anti-rust paint and anti-corrosion coatings, according to the requirements of ship engineering and environmental conditions, and spray them to protect the bent rudder stock and extend its service life.
[0045] Surface decoration: Depending on the ship's design and appearance requirements, surface decoration treatments can be carried out, such as painting ship markings and applying decorative paint, to improve the aesthetics of the ship.
[0046] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A forging method for a bent rudder stock, characterized in that, Includes the following steps, Step 1: Select steel billets with round or square cross-sections; Step two: Preheat the steel billet; Step 3, forging operation, including shoulder cutting with a cutting tool, lengthening, and bending; when cutting the shoulder with a cutting tool, a 200mm bevel is used; after shoulder cutting, the cutting tool is installed on the lengthening machine for lengthening; when installing the cutting tool on the lengthening machine, ensure that the middle part of the bent rudder stock is aligned with the clamp of the lengthening machine; after lengthening, remove the bent rudder stock from the lengthening machine and install it on the beveling machine; start the beveling machine to beveling the two ends of the bent rudder stock; control the beveling angle and length of the two ends of the bent rudder stock by adjusting the force and position of the beveling machine; when beveling, tilt the bottom of the bent rudder stock towards the center line to reduce excessive weight and prevent the manipulator from rotating; when bending, place the bent rudder stock between the flat anvil and the V-shaped anvil, fix it with clamps, and apply force with a hammer; Step four: After the forging operation is completed, the dimensions of the bent rudder stock are calibrated. Step 5: After dimensional calibration, the bent rudder stock undergoes heat treatment; Step 6: After heat treatment, perform a quality inspection on the bent rudder stock; Step seven: After quality inspection, perform surface treatment and spraying of the bent rudder post; In step three, the elongation process involves using mechanical force or hydraulic pressure to cause the bent rudder stock to stretch and deform. The force and speed of the forging machine are adjusted to control the elongation deformation of the bent rudder stock. When the length of the forging exceeds 6 meters, the elongation is completed. In step seven, the surface treatment of the forged and heat-treated bent rudder stock is carried out by the following steps: cleaning the surface, using cleaning agents and tools to clean the surface of the bent rudder stock to remove dirt and oxides generated during forging and heat treatment; shot peening, using shot peening equipment to perform shot peening treatment on the surface of the bent rudder stock. Apply anti-corrosion coating.
2. The forging method for the bent rudder stock according to claim 1, characterized in that, In step three, the bending hammer head applies force from one side of the bending rudder, gradually bending it into the target shape.
3. The forging method for the bent rudder stock according to claim 2, characterized in that, The hammer force is perpendicular to the axis of the bent rudder.
4. The forging method for the bent rudder stock according to claim 1, characterized in that, In step six, the forged curved rudder stock undergoes quality inspection, including dimensional inspection, non-destructive testing, and chemical composition analysis.