Preparation method of three-dimensional porous Cu1.81S / carbon composite material for sodium battery
A high-purity three-dimensional porous Cu1.81S/carbon composite material was prepared by simplifying the preparation process, which solved the problems of high preparation cost and insufficient performance in the existing technology and realized the efficient application of sodium-ion batteries.
Patent Information
- Application Number
- CN202310987189.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-01
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-08-01
AI Technical Summary
Existing technologies are difficult to simplify in preparing high-purity three-dimensional porous Cu1.81S/carbon composite materials, resulting in high costs and unsuitability for large-scale production. Furthermore, the electrochemical performance of existing materials in sodium-ion batteries is insufficient.
A pure-phase three-dimensional porous Cu1.81S/carbon composite material was prepared by using a simple solvothermal method combined with freeze-drying and tube furnace treatment, and by controlling the ratio of copper nitrate trihydrate, polyvinylpyrrolidone, and thiourea, for use as a negative electrode material for sodium-ion batteries.
The mass production of high-purity three-dimensional porous Cu1.81S/carbon composite material was achieved, which has good electrochemical performance and cycling stability. The initial discharge specific capacity reached 426.7 mAh/g, and it still had 352.4 mAh/g after 100 cycles.
Smart Images

Figure CN116960302B_ABST
Abstract
Description
Technical Field
[0001] A three-dimensional porous Cu for sodium batteries 1.81 The preparation method of S / carbon composite material belongs to the field of sodium-ion batteries. Technical Background
[0002] With increasing demand for green living spaces and growing environmental awareness, the control over traditional polluting energy sources is becoming increasingly stringent. Conversely, new energy sources such as wind, solar, and tidal power are receiving more and more support and practical application. To overcome the adverse effects of weather and geographical factors on the application of new energy sources, the idea of using secondary batteries to store electricity generated by wind and other new energy sources and then stably transmitting it to users via the power grid has greatly promoted the practical application of new energy sources. Lithium-ion batteries are currently the most widely used type of secondary battery. However, due to the influence of lithium resource reserves, distribution, and price, their large-scale energy storage applications are somewhat limited. With the popularization of new energy electric vehicles, the consumption of lithium resources has been further intensified, leading to higher prices. In contrast, sodium resources in my country have relatively high reserves and relatively low prices. In addition, sodium and lithium belong to the same group of elements and have similar physicochemical properties, making sodium-ion batteries more suitable for large-scale energy storage applications. Therefore, the research and application of sodium-ion batteries has become one of the hot research directions in the field of energy storage.
[0003] Electrode materials are one of the main factors affecting battery performance, especially the development of high-performance anode materials, which is a key element in promoting the large-scale application of sodium-ion batteries. Transition metal sulfides, especially copper transition metal sulfides, have advantages such as high theoretical specific capacity and high electronic conductivity, and have been widely studied and applied. Based on existing methods such as solvothermal methods, hydrothermal methods, and high-temperature treatment, most of the materials prepared are single-phase or mixed-phase materials such as CuS, Cu2S, and Cu9S5; however, Cu... 1.81 S phase, especially Cu with a three-dimensional porous structure 1.81 S / carbon composites have been rarely reported. In addition, existing preparation processes are relatively cumbersome and may result in the presence of impurity phases in the product. Furthermore, some preparation methods may have certain equipment requirements, leading to high costs and hindering practical large-scale preparation. Summary of the Invention
[0004] This invention provides a simple, short-cycle, and batch-producible method for preparing Cu with a three-dimensional porous structure. 1.81 The S / carbon composite material has high purity and exhibits excellent electrochemical performance when used as the negative electrode in sodium-ion batteries.
[0005] This invention provides a three-dimensional porous Cu for sodium batteries. 1.81 The preparation method of S / carbon composite material includes the following steps:
[0006] a) In a 50 mL beaker, add deionized water and polyvinylpyrrolidone; after stirring for 40 min, add copper nitrate trihydrate and thiourea; after stirring for 40 min, freeze dry until the solution becomes powder.
[0007] b) The powder is transferred to a ceramic boat and placed in a tube furnace. The furnace is heated to a specific temperature and held under a nitrogen atmosphere for a period of time. Afterward, it is cooled to room temperature with the furnace to obtain three-dimensional porous Cu. 1.81 S / carbon composite materials;
[0008] c) The above three-dimensional porous Cu 1.81 S / carbon composite materials are used as electrode materials in sodium-ion batteries.
[0009] In step a), under the conditions that the amounts of deionized water, polyvinylpyrrolidone with a molecular weight of 40,000, and thiourea added are 30.0 mL, 1.0 g, and 2.0 g, respectively, the amount of copper nitrate trihydrate added ranges from 0.4 to 1.2 g.
[0010] In step b), under the condition that the nitrogen gas flow rate is 16 sccm, the temperature is increased from 30°C to 690°C at a heating rate of 3°C / min, and then held at that temperature for 70 min.
[0011] In step c), during the sodium-ion battery cycle performance test, the initial discharge specific capacity reached 426.7 mAh / g at 0.1 A / g, and the specific capacity was still 352.4 mAh / g even after 100 cycles.
[0012] This method differs from other methods for preparing three-dimensional porous Cu structures. 1.81 Compared to the S / carbon composite method, this simplifies the preparation process and is suitable for large-scale mass production; more importantly, it integrates pure-phase three-dimensional porous Cu... 1.81 When used in sodium-ion batteries, S / carbon composite materials exhibit high specific capacity and cycle performance.
[0013] A Bruker Advance D8 X-ray powder diffractometer (Cu Kα radiation) was used. The structure of the prepared material was determined using a 2θ = 10⁻⁸⁰° microscope. The surface morphology of the prepared material was observed using a Hitachi S-4800 scanning electron microscope. Battery performance was tested using an electrochemical workstation (CHI660E) and a Neware battery testing system.
[0014] Depend on Figure 1 It can be seen that when the amount of copper nitrate trihydrate added is 0.8g, the prepared three-dimensional porous Cu 1.81The S / carbon composite sample has a pure-phase tetragonal structure (JCPDS card No. 41-0959), in which Cu is the only phase present. 1.81 Apart from the diffraction peaks of S and carbon, no other impurity peaks were detected. Figure 2 It can be seen that when the amount of copper nitrate trihydrate added is 0.4–1.2 g (ac), it is all pure phase Cu. 1.81 Material S; when the amount of copper nitrate trihydrate added is 1.6 g (d), the sample contains Cu 1.81 In addition to the S diffraction peak, there is also a Cu₂S diffraction peak, indicating that the optimal range for the addition of copper nitrate trihydrate is 0.4–1.2 g when the amounts of deionized water, polyvinylpyrrolidone (molecular weight 40000), and thiourea are 30.0 mL, 1.0 g, and 2.0 g, respectively. Figure 3 It can be seen that when the amount of copper nitrate trihydrate added is 0.8g, the product obtained has a three-dimensional porous structure, and Cu 1.81 S particles are evenly distributed on the surface of these pores. Figure 4 It can be seen that Cu with a three-dimensional porous structure 1.81 When the S / carbon composite material was used as an electrode material in sodium-ion batteries, the cyclic voltammetry curves from the second to the third cycle essentially overlapped, indicating stable electrochemical performance. Figure 5 It can be seen that Cu with a three-dimensional porous structure 1.81 The S / carbon composite material has an initial sodium storage capacity of 426.7 mAh / g at 0.1 A / g, and the specific capacity is still 352.4 mAh / g even after 100 cycles. Attached Figure Description
[0015] Figure 1 This is the X-ray diffraction pattern of the product when 0.8g of copper nitrate trihydrate is added.
[0016] Figure 2 The X-ray diffraction pattern of the product is shown when the amount of copper nitrate trihydrate added is in the range of 0.4 to 1.6 g.
[0017] Figure 3 This is a scanning electron microscope image of the product when 0.8g of copper nitrate trihydrate is added.
[0018] Figure 4 The three-dimensional porous Cu was prepared when the amount of copper nitrate trihydrate added was 0.8g. 1.81 CV curve of S / carbon composite material.
[0019] Figure 5 The three-dimensional porous Cu was prepared when the amount of copper nitrate trihydrate added was 0.8g. 1.81 Cyclic curve of S / carbon composite material. Detailed Implementation
[0020] 1. In a 50 mL beaker, add 30.0 mL of deionized water and 1.0 g of polyvinylpyrrolidone (molecular weight 40,000); after stirring for 40 min, add 0.4 g of copper nitrate trihydrate and 2.0 g of thiourea; stir for another 40 min, then freeze-dry until the solution becomes powder; transfer the powder to a ceramic boat and place it in a tube furnace, purge with nitrogen at a rate of 16 sccm, then raise the temperature from 30 °C to 690 °C at a rate of 3 °C / min and hold for 70 min, then cool with the furnace to room temperature to obtain Cu. 1.81 S / carbon composite material (sample a, see...) Figure 2 ).
[0021] 2. In a 50 mL beaker, add 30.0 mL of deionized water and 1.0 g of polyvinylpyrrolidone (molecular weight 40,000); after stirring for 40 min, add 0.8 g of copper nitrate trihydrate and 2.0 g of thiourea; stir for another 40 min, then freeze-dry until the solution becomes powder; transfer the powder to a ceramic boat and place it in a tube furnace, purge with nitrogen at a rate of 16 sccm, then raise the temperature from 30 °C to 690 °C at a rate of 3 °C / min and hold for 70 min, then cool with the furnace to room temperature to obtain Cu. 1.81 S / carbon composite material (sample b, see...) Figure 1-3 ).
[0022] 3. In a 50 mL beaker, add 30.0 mL of deionized water and 1.0 g of polyvinylpyrrolidone (molecular weight 40,000); after stirring for 40 min, add 1.2 g of copper nitrate trihydrate and 2.0 g of thiourea; stir for another 40 min, then freeze-dry until the solution becomes powder; transfer the powder to a ceramic boat and place it in a tube furnace, purge with nitrogen at a rate of 16 sccm, then raise the temperature from 30 °C to 690 °C at a rate of 3 °C / min and hold for 70 min, then cool with the furnace to room temperature to obtain Cu. 1.81 S / carbon composite material (sample c, see...) Figure 2 ).
[0023] 4. In a 50 mL beaker, add 30.0 mL of deionized water and 1.0 g of polyvinylpyrrolidone (molecular weight 40,000); after stirring for 40 min, add 1.6 g of copper nitrate trihydrate and 2.0 g of thiourea; stir for another 40 min, then freeze-dry until the solution becomes powder; transfer the powder to a ceramic boat and place it in a tube furnace, purge with nitrogen at a rate of 16 sccm, then raise the temperature from 30 °C to 690 °C at a rate of 3 °C / min and hold for 70 min, then cool with the furnace to room temperature to obtain Cu.1.81 S / carbon composite material (sample d, see...) Figure 2 ).
Claims
1. A three-dimensional porous Cu for sodium batteries 1.81 The preparation method of S / carbon composite material includes the following steps: a) In a 50 mL beaker, add deionized water and polyvinylpyrrolidone; after stirring for 40 min, add copper nitrate trihydrate and thiourea; after stirring for 40 min, freeze dry until the solution becomes powder. b) The powder is transferred to a ceramic boat and placed in a tube furnace. The furnace is heated to a specific temperature and held under a nitrogen atmosphere for a period of time. Afterward, it is cooled to room temperature with the furnace to obtain three-dimensional porous Cu. 1.81 S / carbon composite material.
2. The three-dimensional porous Cu for sodium ion exchange as described in claim 1 1.81 The method for preparing S / carbon composite materials is characterized by, In step a), under the conditions that the amounts of polyvinylpyrrolidone, thiourea, and deionized water added are 1.0 g, 2.0 g, and 30.0 mL, respectively, the amount of copper nitrate trihydrate added ranges from 0.4 to 1.2 g, wherein the molecular weight of polyvinylpyrrolidone is 40,000.
3. The three-dimensional porous Cu for sodium ion exchange as described in claim 1 1.81 The method for preparing S / carbon composite materials is characterized by, In step b), under the condition that the nitrogen gas flow rate is 16 sccm, the temperature is increased from 30°C to 690°C at a heating rate of 3°C / min, and then held for 70 min.
Citation Information
Patent Citations
Preparation method of three-dimensional porous Fe3N / carbon composite material for sodium electricity