A method and application for preparing OPV active layer using sulfur-containing compounds as solvents
By using sulfur-containing compound solvents and thiophene structural unit-terminated polymers to prepare the OPV active layer, the problems of solubility and efficiency of environmentally friendly solvents in organic solar cells were solved, achieving high-efficiency, environmentally friendly device performance and stable mass production.
Patent Information
- Application Number
- CN202310943823.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-07-28
AI Technical Summary
In existing technologies, environmentally friendly solvents are difficult to meet the requirements of high solubility and photoelectric conversion efficiency of active layer materials in organic solar cells. Furthermore, traditional solvents are harmful to the environment and human health, which limits the fabrication and commercial application of devices.
Using sulfur-containing compounds as solvents, and combining thiophene structural units with end-capped polymers and non-fullerene acceptors, an OPV active layer is prepared. The solubility is improved by utilizing the similarity-to-mix property, and the device performance is optimized through a multilayer structure.
It achieves efficient dissolution with environmentally friendly and low-toxicity solvents, improves the generation and collection efficiency of photogenerated carriers, ensures stable device performance, is suitable for mass production, and reduces manufacturing costs.
Smart Images

Figure CN116981323B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of organic optoelectronic device technology, specifically to a method for preparing an active layer using a sulfur-containing compound as a solvent, and its application. Background Technology
[0002] Conjugated polymers, due to their rigid aromatic backbones and strong π-π stacking, often exhibit poor solubility. Solubility is typically improved by introducing alkyl chains, and solution processing is achieved using solvents with good solubility such as chloroform, chlorobenzene, and toluene. These polymer thin-film photovoltaics are used in the fabrication of solar cells, light-emitting diodes (LEDs), and field-effect transistors (FETs). Among them, organic solar cells (OPVs) possess outstanding advantages such as simple fabrication processes, light weight, flexibility, and ease of large-area production, demonstrating enormous application potential and thus becoming one of the research hotspots in the energy field in recent years. In particular, the development of novel active layer materials, interface layer materials, and new device fabrication processes has yielded remarkable achievements in the OPV field, with conversion efficiency (PCE) increasing from less than 1% to over 19%, demonstrating excellent development potential and application prospects. Given that the ultimate goal of organic solar cell development is practical application, in addition to focusing on conversion efficiency, the environmental impact of the production process cannot be ignored.
[0003] In existing technologies, the solvents used in the preparation of high-efficiency OPV active layers, such as halogenated hydrocarbons, aromatic hydrocarbons, ethers, or amides, pose significant hazards to the environment and human health. For example, chloroform and chlorobenzene, solvents containing halogen elements, are generally highly toxic. Furthermore, tetrahydrofuran and N-methylpyrrolidone still exhibit considerable teratogenic and reproductive toxicity. Large-scale production generates large quantities of toxic gases, leading to substantial increases in treatment and emission costs, as well as significant damage to human health and the environment, thus severely limiting their large-scale preparation and commercial application.
[0004] Currently available environmentally friendly solvents, such as toluene, o-xylene, and 1,2,4-trimethylbenzene, still have adverse effects on the environment and human health. For example, the application of water / ethanol solvents in the preparation of OPV active layers has been studied to some extent. However, the molecules of water / ethanol environmentally friendly solvents are highly polar, while high-efficiency active layer materials usually have weak polarity and strong molecular packing. According to the principle of "like dissolves like," the solubility of active layer materials in these highly polar environmentally friendly solvents is very poor. Moreover, the photoelectric conversion efficiency of photoactive materials prepared by dissolving or dispersing in water or ethanol is generally low. For example, Lee, S. et al. disclosed in ACS nano 2020, 14(11), 14493-14527 that the photoelectric conversion efficiency of the active layer material prepared using the aforementioned environmentally friendly solvents was less than 7.6%. This no longer meets the requirements of photoelectric materials and optical devices for the photoelectric conversion efficiency of active layer materials. Furthermore, in order to improve the performance of the active layer material, existing technologies have enhanced the water solubility of the active layer material by introducing anions and cations. However, the low oxidation potential of nitrogen atoms can trap holes, which has an adverse effect on the performance of OPV devices. Changing the side chains to nonionic building blocks such as strongly polar polyethylene glycol monomethyl ether can not only achieve the environmentally friendly solvent solubility or dispersibility of conjugated polymers, but also avoid the adverse effects on the conductivity of materials and device performance. It has significant advantages in realizing the water / alcohol homogeneous solution processing of active layer polymers, but the photoelectric conversion efficiency is already difficult to meet the requirements. Ye, L. et al. disclosed an OPV based on (R)-(+)-limonene and 2-methyltetrahydrofuran in Adv. Mater. 2019, 31(17), 1808153, with the highest conversion efficiency reaching 12.2%.
[0005] In summary, research on the use of environmentally friendly and low-toxicity organic solvents for dissolving or dispersing polymer active materials is still in its early stages. Currently, the performance of active layers prepared with available organic solvents does not meet market requirements for device performance. In particular, the material systems for preparing OPV active layers using environmentally friendly organic solvents are relatively limited, and their structure-property relationships are unclear. Furthermore, the molecular orientation of the solvent and the internal morphology of the active layer film have a significant impact on carrier generation and transport. Therefore, studying the micro-ordered structure of the thin film under specific organic solvent molecular structure conditions and its impact on device performance, as well as the structure-property relationship between environmentally friendly organic solvents and active materials, is of great significance for improving device performance.
[0006] Clearly, the solvents and active layer materials available in existing technologies cannot simultaneously meet both environmental protection requirements and device performance. Chinese invention patent CN 114883500 A discloses an organic solar cell based on a polythiophene system processed with non-halogen solvents and its preparation method. This invention utilizes the similarity and miscibility between thiophene solvents and polythiophene derivative donor materials to develop a high-efficiency organic solar cell based on a polythiophene system processed with non-halogen solvents, achieving device performance comparable to that reported with halogen solvents, while reducing the toxicity of the solvent generated during processing. However, this invention only studied thiophene and 3-methyl-thiophene, achieving performance comparable to existing halogenated solvents. It does not provide further technical support regarding whether solvents for other thiophene, tetrahydrothiophene, and thioether compounds can achieve the same effect. Based on this, further research was conducted on the aforementioned environmentally friendly solvents based on existing technologies. This invention expands the types of thiophene organic solvents that can be used to prepare OPV active layers with high conversion efficiency, meeting environmental protection requirements while satisfying the performance and environmental needs of the active layer materials. Summary of the Invention
[0007] In view of this, and based on the problems existing in the prior art, the present invention provides a method and application for preparing OPV active layers using sulfur-containing compounds as solvents, providing a highly efficient and environmentally friendly solvent for preparing OPV active layers, reducing the cost of organic optoelectronic device fabrication. Furthermore, to achieve the above technical objectives, the present invention provides the following technical solutions:
[0008] A method for preparing an OPV active layer using a sulfur-containing compound as a solvent involves spin-coating a solution of an active layer material dissolved in a sulfur-containing compound onto a substrate based on PEDOT:PSS or zinc oxide film, followed by heating to form the OPV active layer.
[0009] Preferably, the active layer material is a binary mixture formed by a capped polymer containing thiophene structural units and an organic compound containing non-fullerene acceptors.
[0010] Preferably, the molar ratio of the end-capped polymer containing thiophene structural units to the organic compound containing non-fullerene acceptors is 0.5 to 2:1.
[0011] More preferably, the molar ratio of the end-capped polymer containing thiophene structural units to the organic compound containing non-fullerene acceptors is 1:1.2.
[0012] Preferably, the end-capping polymer containing thiophene structural units includes at least an end-capping agent and thiophene structural units;
[0013] The thiophene structural unit includes the structure shown in formula (I):
[0014]
[0015] The structure of the end-capped polymer containing thiophene structural units is shown in formula (II) and / or formula (III) and / or formula (IV):
[0016]
[0017] Where n is a natural number from 1 to 10000;
[0018] R1, R2, R3, and R4 are independently hydrogen atoms, fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, cyano groups, or alkyl groups with 1 to 30 carbon atoms; or, one or more carbon atoms on the C1 to C30 alkyl groups are substituted by one or more functional groups selected from oxygen atoms, alkenyl groups, alkynyl groups, aryl groups, or ester groups; or one or more hydrogen atoms on the C1 to C30 alkyl groups are substituted by one or more functional groups selected from fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.
[0019] X1 and X2 are each independently one of the following: hydrogen atom, fluorine atom, chlorine atom, bromine atom, iodine atom, cyano group or alkoxy chain substituent.
[0020] The main structural formula of the end-capping agent 1 or end-capping agent 2 is independently shown in any one of the following formulas:
[0021]
[0022] Wherein, m is a natural number from 1 to 10000; R, R1, R2, R3, R4, R5, R6, R7, R8, and R9 are independently hydrogen atoms, fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, cyano groups, or alkyl groups with 1 to 30 carbon atoms, or groups in which one or more carbon atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of oxygen atoms, alkenyl, alkynyl, aryl, or ester groups, or groups in which one or more hydrogen atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, oxygen atoms, nitrogen atoms, alkoxy chains, alkenyl, alkynyl, aryl, carbonyl, amide groups, acid anhydride groups, or ester groups.
[0023] Y and Y1 are independently oxygen atoms, sulfur atoms, selenium atoms, and nitrogen atoms attached to R7, wherein R7 is an alkyl group with 1 to 30 carbon atoms, or a group in which one or more carbon atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of alkoxy chain, alkenyl, alkynyl, aryl or ester group, or a group in which one or more hydrogen atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atom, chlorine atom, bromine atom, iodine atom, alkoxy chain, alkenyl, alkynyl, aryl or ester group.
[0024] Preferably, the capping agent is a bromoanthracene capping agent.
[0025] Preferably, the organic compound containing a non-fullerene acceptor has the structural formula shown in formula (V):
[0026]
[0027] Wherein, R5, R6, R7, and R8 are independently hydrogen atoms, fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, cyano groups, or alkyl groups with 1 to 30 carbon atoms, or groups in which one or more carbon atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of oxygen atoms, alkenyl, alkynyl, aryl, or ester groups, or groups in which one or more hydrogen atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, oxygen atoms, nitrogen atoms, alkoxy chains, alkenyl, alkynyl, aryl, carbonyl, amide, anhydride, or ester groups;
[0028] X3, X4, X5, X6, X7, X8, X9, X 10 The substituent is independently a hydrogen atom, fluorine atom, chlorine atom, bromine atom, iodine atom, or alkoxy chain; Y1, Y2, Y3, Y4, and Z are independently oxygen atoms, sulfur atoms, selenium atoms, or nitrogen atoms connected to R7, wherein the R7 group is an alkyl group with 1 to 30 carbon atoms, or a group in which one or more carbon atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of alkoxy chain, alkenyl, alkynyl, aryl, or ester group, or a group in which one or more hydrogen atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atom, chlorine atom, bromine atom, iodine atom, alkoxy chain, alkenyl, alkynyl, aryl, or ester group.
[0029] Preferably, the organic compound containing a non-fullerene acceptor is BO-4Cl, with the following structural formula:
[0030]
[0031] Preferably, the sulfur-containing compound has at least one of the following structural formulas:
[0032]
[0033] Among them, R9, R 10 R 11 R 12 R 13 R 14 R 15 R 16 R 17 R 18Independently, it is a group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkoxy chain, an alkenyl group, an alkynyl group, an aryl group, an alkyl group with 1 to 30 carbon atoms, or a group in which one or more carbon atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of an oxygen atom, an alkenyl group, an alkynyl group, an aryl group, or an ester group, or a group in which one or more hydrogen atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkoxy chain, an alkenyl group, an alkynyl group, an alkynyl group, an aryl group, or an ester group.
[0034] Preferably, the sulfur-containing compound includes derivatives of thiophene, tetrahydrothiophene, and thioethers.
[0035] Preferably, it is a mixed solvent of any one or more of 2-ethylthiophene, 3-methylthiophene, 2-propylthiophene, 2-butylthiophene, 3-ethylthiophene, 2,4-dimethylthiophene, 2,5-dimethylthiophene, 3,4-dimethylthiophene, 3,4-dimethylthiophene, tetrahydrothiophene, 2-methyltetrahydrothiophene diethyl sulfide, dipropyl sulfide, and dibutyl sulfide, or a mixture thereof in any proportion.
[0036] Based on the OPV active layer provided by the above technical solution, it is applied to organic solar cells to prepare a device structure with a multilayer structure. Specifically, the multilayer structure of the organic solar cell includes, from bottom to top, a stacked ITO glass substrate, a hole (electron) transport layer, an OPV active layer, an electron (hole) transport layer, and a metal electrode.
[0037] The specific preparation method of organic solar cells includes the following steps:
[0038] S1. Preparation of ITO glass substrate: The ITO glass substrate is obtained by cleaning and drying ITO glass;
[0039] S2. Preparation of hole (electron) transport layer: PEDOT:PSS (zinc oxide nanoparticles or sol-zinc salt solution) is spin-coated onto the ITO glass substrate prepared in S1, and the hole (electron) transport layer is obtained after thermal annealing.
[0040] S3. Preparation of the OPV active layer: The end-capped polymer containing thiophene structural units and BO-4Cl are dissolved in a sulfur-containing solvent and spin-coated onto the hole (electron) transport layer prepared in S2 to obtain the OPV active layer;
[0041] S4. Preparation of electron (hole) transport layer: Dissolve PFN-Br solid powder in methanol and spin-coat it onto the surface of the OPV active layer to obtain the electron transport layer, thereby forming a device structure with multiple layers; deposit molybdenum trioxide by vapor deposition or spin-coat a molybdenum-containing solution to obtain the hole transport layer.
[0042] S5. Fabrication of metal electrodes: The multi-layered device structure obtained in S4 is vacuum-deposited to form a metal electrode layer on the surface of the electron (hole) transport layer.
[0043] Thus, a forward (inverted) device structure of an organic solar cell with multiple stacked layers was prepared.
[0044] Preferably, the solid content of the PEDOT:PSS solution is 1.3% to 1.7%.
[0045] Preferably, the weight ratio of PEDOT to PSS is 1:6.
[0046] The beneficial technical effects obtained by this invention are as follows:
[0047] 1. The present invention uses thiophene-based environmentally friendly solvents combined with organic active materials based on end-capped polymers containing thiophene units to prepare OPV active layers and organic solar cells. Utilizing the principle of "like dissolves like," the solubility of thiophene solvents in end-capped polymers containing thiophene units and BO-4Cl as organic active materials is increased. Furthermore, the combined use of thiophene solvents with end-capped polymers and organic materials containing non-fullerene acceptors not only offers advantages such as environmental friendliness and low toxicity but also superior efficiency, thereby further improving the photochemical stability of the OPV active layer and obtaining an optical device structure with excellent conversion efficiency.
[0048] 2. By employing the technical solution of this invention, using a sulfur-containing compound with low toxicity as a solvent, and selecting an active material with the same structural unit as the sulfur-containing compound to prepare the active layer, at least the same results as those obtained with halogen-containing organic reagents (such as chloroform) in the prior art can be obtained, including higher generation and collection efficiency of photogenerated carriers, resulting in an ideal J-shaped device. sc And FF.
[0049] 3. By adopting the technical solution of this invention and summarizing the production efficiency through multiple batch productions, it can be found that the batch efficiency is stable at 15-16%, which has good production stability. In other words, the batch difference is very small, which provides technical support for the stability of device quality and is suitable for mass production promotion and application.
[0050] 4. The technical solution of this invention provides a wider range of environmentally friendly reagents, reduces the cost of optical device fabrication, and provides an economic foundation for its commercial promotion and application. Attached Figure Description
[0051] Figure 1a In Example 1 of this invention, PEDOT:PSS was used as a substrate to prepare... ofFlowchart of the structure of an organic solar cell forward (inverted) device.
[0052] Figure 1b In Example 1 of this invention, a zinc oxide thin film was used as a substrate to prepare... of Flowchart of the structure of an organic solar cell forward (inverted) device.
[0053] Figure 2a A schematic diagram of the structure of the organic solar cell positive-position device based on PEDOT:PSS in Embodiment 1 of the present invention.
[0054] Figure 2b A schematic diagram of the structure of the inverted organic solar cell device based on zinc oxide thin film in Embodiment 1 of the present invention.
[0055] Figures 3a-3e AFM images of the OPV active layers prepared in the embodiments and control examples of the present invention, respectively.
[0056] Figure 4 The figures show the current density-voltage characteristic curves of organic solar cells prepared using different solvents in Examples 1-4 of this invention and comparative documents 1-2.
[0057] Figure 5 The external quantum efficiency diagrams are shown for organic solar cells prepared using different solvents in Examples 1-4 and Comparative Documents 1-2 of this invention.
[0058] Figures 6a-6f V values of devices prepared using different thiophene solvents in Examples 1-4 and Comparative Documents 1-2, respectively. OC J SC The relationship between light intensity and carrier dynamics. Detailed Implementation
[0059] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are some embodiments of this application, but not all embodiments.
[0060] This invention provides a method for preparing an OPV active layer using a sulfur-containing compound as a solvent. The method involves spin-coating a solution of an active layer material prepared by dissolving a sulfur-containing compound as a solvent onto a substrate based on PEDOT:PSS or zinc oxide film, followed by heating to form the OPV active layer.
[0061] Specifically, the active layer material is a binary mixture formed by a capped polymer containing thiophene structural units and an organic compound containing non-fullerene acceptors.
[0062] In some preferred embodiments, the active layer material is a binary mixture of a thiophene-containing end-capped polymer and BO-4Cl.
[0063] The molar ratio of the end-capped polymer containing thiophene structural units to BO-4Cl is 0.5 to 2.0:1.
[0064] More preferably, the molar ratio of the end-capped polymer containing thiophene structural units to BO-4Cl is 1:1.2.
[0065] In some preferred embodiments, the end-capping polymer containing thiophene structural units includes at least an end-capping agent and thiophene structural units;
[0066] In some preferred embodiments, the thiophene structural unit has the structure shown in formula (I):
[0067]
[0068] In some preferred embodiments, the structure of the end-capped polymer containing thiophene structural units is shown in formula (II):
[0069]
[0070] Or, as shown in equation (III):
[0071] Or, as shown in equation (IV):
[0072] Or, including two or more of the structural formulas (II), (III), and (IV);
[0073] Wherein, n is a natural number from 1 to 10000; R1, R2, R3, and R4 are independently alkyl groups with 1 to 30 carbon atoms, or one or more carbon atoms on a C1 to C30 alkyl group are substituted by one or more functional groups selected from oxygen, alkenyl, alkynyl, aryl, or ester groups, or one or more hydrogen atoms on a C1 to C30 alkyl group are substituted by one or more functional groups selected from fluorine, chlorine, bromine, and iodine atoms; X1 and X2 are hydrogen, fluorine, chlorine, bromine, iodine, or alkoxy chain substituents;
[0074] In some preferred embodiments, the bulk structural formula of the capping agent is shown in any of the following formulas:
[0075]
[0076] In the above structural formula, one or more carbon atoms on the aromatic ring can be replaced with N atoms or NR atoms;
[0077] One or more carbon atoms on the aromatic ring in the above structural formula can be replaced with N atoms or NR atoms;
[0078] m is a natural number from 1 to 10000;
[0079] R, R1, R2, R3, R4, R5, R6, R7, R8, and R9 are independently hydrogen atoms, fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, cyano groups, or alkyl groups with 1 to 30 carbon atoms, or groups in which one or more carbon atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of oxygen atoms, alkenyl, alkynyl, aryl, or ester groups, or groups in which one or more hydrogen atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, oxygen atoms, nitrogen atoms, alkoxy chains, alkenyl, alkynyl, aryl, carbonyl, amide, anhydride, or ester groups.
[0080] Y and Y1 are independently oxygen atoms, sulfur atoms, selenium atoms, and nitrogen atoms with R7 attached, wherein R7 is an alkyl group with 1 to 30 carbon atoms, or a group in which one or more carbon atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of alkoxy chain, alkenyl, alkynyl, aryl or ester group, or a group in which one or more hydrogen atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atom, chlorine atom, bromine atom, iodine atom, alkoxy chain, alkenyl, alkynyl, aryl or ester group;
[0081] In some preferred embodiments, the capping agent is a bromoanthracene capping agent.
[0082] In some preferred embodiments, the end-capped polymer containing thiophene structural units is bromoanthracene-terminated PM6.
[0083] In some preferred embodiments, the organic compound containing a non-fullerene acceptor has the structural formula shown in formula (V):
[0084]
[0085] Wherein, R5, R6, R7, and R8 are independently alkyl groups with 1 to 30 carbon atoms, or groups in which one or more carbon atoms of a C1 to C30 alkyl group are substituted by one or more functional groups selected from oxygen, alkenyl, alkynyl, aryl, or ester groups, or groups in which one or more hydrogen atoms of a C1 to C30 alkyl group are substituted by one or more functional groups selected from fluorine, chlorine, bromine, iodine, alkoxy chain, alkenyl, alkynyl, aryl, or ester groups; X3, X4, X5, X6, X7, X8, X9, X 10Independently, it is a substituent of hydrogen atom, fluorine atom, chlorine atom, bromine atom, iodine atom, or alkoxy chain; Y1, Y2, Y3, Y4, and Z are independently substituents of oxygen atom, sulfur atom, selenium atom, or nitrogen atom connected to R7, wherein R7 group is an alkyl group with 1 to 30 carbon atoms, or a group in which one or more carbon atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of alkoxy chain, alkenyl, alkynyl, aryl, or ester group, or a group in which one or more hydrogen atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atom, chlorine atom, bromine atom, iodine atom, alkoxy chain, alkenyl, alkynyl, aryl, or ester group.
[0086] In some preferred embodiments, the sulfur-containing compound has the following structural formula:
[0087]
[0088] Among them, R9, R 10 R n R 12 R 13 R 14 R 15 R 16 R 17 R 18 Independently, it is a group consisting of a hydrogen atom, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkoxy chain, an alkenyl group, an alkynyl group, an aryl group, an alkyl group with 1 to 30 carbon atoms, or a group in which one or more carbon atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of an oxygen atom, an alkenyl group, an alkynyl group, an aryl group, or an ester group, or a group in which one or more hydrogen atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, an alkoxy chain, an alkenyl group, an alkynyl group, an alkynyl group, an aryl group, or an ester group.
[0089] In some preferred embodiments, the organic compound containing the non-fullerene acceptor is BO-4Cl, with the following structure:
[0090]
[0091] In some preferred embodiments, the molar ratio of bromoanthracene-terminated PM6:BO-4Cl is 1:1.2.
[0092] In some preferred embodiments, the sulfur-containing compound is an organic solvent containing a thiophene structure.
[0093] In some preferred embodiments, the environmentally friendly solvents include, but are not limited to, derivatives such as thiophene, tetrahydrothiophene, and sulfides.
[0094] In some preferred embodiments, the environmentally friendly solvent includes, but is not limited to, any one or more of 2-methylthiophene, 2-ethylthiophene, 3-methylthiophene, 2-propylthiophene, 2-butylthiophene, 2-ethyl-5-methylthiophene, 3-ethylthiophene, 2,4-dimethylthiophene, 2,5-dimethylthiophene, 3,4-dimethylthiophene, 3,4-dimethylthiophene, tetrahydrothiophene, 2-methyltetrahydrothiophene, diethyl sulfide, dipropyl sulfide, dibutyl sulfide, etc.
[0095] The PFN-Br, PEDOT:PSS, zinc oxide, and molybdenum oxide of this invention are universally applicable interface materials for photovoltaics. PFN-Br is poly[(9,9-bis(3′-(N,N-dimethylamino)propyl)fluorenyl-2,7-diyl)-ALT-[(9,9-di-n-octylfluorenyl-2,7-diyl)]-bromine. PEDOT:PSS is poly(3,4-ethylenedioxythiophene) / polystyrene sulfonate. Using PFN-Br or zinc oxide (PEDOT:PSS or molybdenum oxide) for electrode modification can significantly improve the electron (hole) extraction and transport performance of the negative electrode and suppress the extraction and transport of holes (or electrons), thereby improving the charge recombination problem at the interface and contributing to the improvement of photovoltaic efficiency.
[0096] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains. While similar or equivalent methods and materials described in this application may be used in the practice or testing of the disclosed embodiments, suitable methods and materials are those described below. All publications, patent applications, patents, and other references mentioned herein, except for specific cited paragraphs, are incorporated herein by reference in their entirety. In case of any conflict, this specification and its included definitions shall prevail. Furthermore, materials, methods, and examples are illustrative only and not restrictive.
[0097] The technical solution, implementation process, and principle of the present invention will be further explained and illustrated below through specific embodiments. It should be noted that the following detailed descriptions are exemplary and intended to provide further explanation of the present invention. The described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise stated, the reagents and raw materials used in the following embodiments are commercially available, and the test methods without specific conditions are generally performed under conventional conditions or according to the conditions recommended by the respective manufacturers. Furthermore, unless otherwise stated, the experimental methods, detection methods, and preparation methods disclosed in the present invention all employ conventional techniques in this technical field. These techniques have been well described in existing literature.
[0098] When describing the elements of the embodiments described herein, the articles “a,” “an,” “the,” and “the” are intended to mean that one or more of the stated elements are present. The terms “comprising,” “including,” and “having” are intended to be inclusive and mean that additional elements may be present in addition to the listed elements.
[0099] The term “halogen” or “halogenated” as used alone or as part of another group in this article refers to chlorine, bromine, fluorine, and iodine.
[0100] The technical solution of the present invention will be further described in detail below through specific embodiments.
[0101] Example 1
[0102] Referring to Figure 1, this embodiment provides an upright structure device, which sequentially includes a substrate, a hole transport layer, an active layer, an electron transport layer, and a cathode electrode. The process includes preparing a substrate material (ITO glass) to connect to the anode; spin-coating a 20nm layer of PEDOT:PSS onto the surface of the substrate to obtain a hole transport layer (i.e., the anode interface layer); dissolving the active layer material in an environmentally friendly solvent containing sulfur compounds; the active layer material comprising a binary mixture of a capped polymer (bromoanthracene-capped PM6) and BO-4Cl (bromoanthracene-capped PM6:BO-4Cl molar ratio = 1:1.2); spin-coating the active layer material onto the surface of the hole transport layer to obtain a 100nm OPV active layer; finally, dissolving PFN-Br solid powder in methanol and spin-coating it onto the surface of the active layer to obtain a 10nm cathode interface layer; and finally, performing metal evaporation to obtain a cathode electrode on the surface of the cathode interface layer. Thus, the upright device is fabricated.
[0103] The structural formula of the bromoanthracene-terminated PM6 in this embodiment is as follows:
[0104]
[0105] The structural formula of BO-4Cl is:
[0106]
[0107] Specifically, the fabrication process of the upright device includes the following steps:
[0108] (1) Cleaning of the ITO glass substrate: First, gently rub the purchased ITO glass with a lint-free cloth dampened with detergent, and rinse off the detergent residue with clean water; then add deionized water and detergent, and ultrasonically clean it for 30 minutes in an ultrasonic cleaner before taking it out; add deionized water again, and ultrasonically clean it for 30 minutes before taking it out; ultrasonically clean it twice with ethanol for 30 minutes each time, and finally dry it with a nitrogen gun before use.
[0109] (2) Preparation of the anode interface layer: The filtered PEDOT:PSS solution with a solid content of 1.5% (purchased from Heraeus Company, model Clevios-4083, the same material was used in other examples, wherein the weight ratio of PEDOT to PSS was 1:6) was spread on the ITO glass surface after cleaning in step (1), and spin-coated at 4000 rpm for 30s, and then annealed at 150°C for 10min to form a 30nm PEDOT:PSS film as the anode interface layer on the substrate surface. The substrate loaded with the PEDOT:PSS film was removed and transferred to a nitrogen glove box.
[0110] (3) Preparation of active layer: This step is completed in a nitrogen glove box; the active layer is prepared on the substrate loaded with PEDOT:PSS film prepared in step (2).
[0111] First, the active layer material (PM6:BO-4Cl, molar ratio 1:1.2) was dissolved in 2,5-methylthiophene and spin-coated onto a substrate loaded with a PEDOT:PSS film. The film thickness was 100 nm. Then, it was placed on a hot plate and annealed at 100 °C for 10 min. Finally, it was removed.
[0112] (4) Cathode interface PFN-Br solution: PFN-Br solid powder was directly dissolved in methanol, with a total concentration of 0.5 mg / ml. -1 The solution was stirred at room temperature for more than 2 hours. Then, the PFN-Br solution was used to prepare an interface layer on the surface of the active layer material prepared in the previous step using a dynamic spin coating method. The spin speed was 3000 rpm and the spin time was 30 s to form a 10 nm thin film without annealing.
[0113] (5) Fabrication of the Al electrode: After the cathode interface layer is fabricated, the device is transferred to the evaporation chamber, and the chamber pressure is kept below 5 × 10⁻⁶. -5 Evaporation was performed under Pa conditions, and the evaporation rate was controlled within... The following steps ensure that the evaporation thickness is above 100 nm, and then the deposited material is removed, resulting in a final device with an effective area of 4 mm². 2 .
[0114] Example 2
[0115] This embodiment provides a fabrication process for an inverted device, specifically including:
[0116] (1) Cleaning of the ITO glass substrate: First, gently rub the purchased ITO glass with a lint-free cloth dampened with detergent, and rinse off the detergent residue with clean water; then add deionized water and detergent, and ultrasonically clean it for 30 minutes in an ultrasonic cleaner before taking it out; add deionized water again, and ultrasonically clean it for 30 minutes before taking it out; ultrasonically clean it twice with ethanol for 30 minutes each time, and finally dry it with a nitrogen gun before use.
[0117] (2) Preparation of cathode interface layer: Take out the methanol ZnO solution (concentration 15mg / mL) cooled to room temperature and spread it on the ITO glass surface cleaned in step (1). Spin coat at 2500rpm, acceleration 1000rpm / s, time 30s to form a 15nm thin film. After spin coating, place the device on a hot stage at 130℃ for annealing for 10 minutes. After removing it, transfer it to an N2 glove box.
[0118] (3) Preparation of active layer: This step is completed in a nitrogen glove box; the active layer is prepared on the substrate loaded with ZnO film prepared in step (2).
[0119] First, the active layer material (PM6:BO-4Cl, molar ratio 1:1.2) was dissolved in 2,5-dimethylthiophene and spin-coated onto a ZnO-loaded substrate. The film thickness was 100 nm. Then, it was placed on a hot plate and annealed at 100 °C for 10 min. Finally, it was removed.
[0120] (4) Anode interface MoO3 evaporation: The device is directly transferred to the vacuum evaporation chamber, and the chamber pressure is below 5×10⁻⁶. -5 Evaporation was performed under Pa conditions, and the evaporation rate was controlled within... The following is a 10nm hole transport layer, MoO3, is deposited by vapor deposition.
[0121] (5) Preparation of Al electrodes: Similarly, when the cavity pressure is below 5 × 10⁻⁶, -5 Evaporation was performed under Pa conditions, and the evaporation rate was controlled within... The following steps ensure that the evaporation thickness is above 100 nm, and then the deposited material is removed, resulting in a final device with an effective area of 4 mm². 2 .
[0122] Example 3
[0123] The difference between this embodiment and Example 1 is that the organic environmentally friendly solvent used in step (3) is 2-methylthiophene (2-MeT).
[0124] Example 4
[0125] The difference between this embodiment and Example 1 is that the organic environmentally friendly solvent used in step (3) is 2-ethylthiophene (2-EtT).
[0126] Example 5
[0127] The difference between this embodiment and Example 1 is that the organic environmentally friendly solvent used in step (3) is 3-methylthiophene (3-MeT).
[0128] Example 6
[0129] The difference between this embodiment and Example 1 is that the organic environmentally friendly solvent used in step (3) is 3-ethylthiophene (3-EtT).
[0130] Example 7
[0131] The difference between this embodiment and Embodiment 1 is that the organic environmentally friendly solvent used in step (3) is 2-ethyl-5-methylthiophene.
[0132] Comparative Example 1
[0133] The difference between this comparative example and Example 1 is that the solvent used in step (3) is chloroform (CF).
[0134] Comparative Example 2
[0135] The difference between this comparative example and Example 1 is that the solvent used in step (3) is o-xylene (o-XY).
[0136] Performance characterization and testing:
[0137] 1. Appearance
[0138] See Figures 3a-3e The figures shown are AFM phase diagrams of the active layers prepared in the comparative example and the example, respectively.
[0139] Obviously, Figure 3b In this process, the substituted thiophene solvent at the 3-methyl position can promote the binary mixed system in the active layer to achieve a suitable degree of phase separation, making the phase distribution of the binary mixed system more continuous and uniform, which is conducive to the formation of a better interpenetrating network structure in the film. Figure 3a , Figure 3b , Figure 3c The morphology is similar, but the 3-methylthiophene fibrous structure is more three-dimensional and obvious, and the fiber size is more suitable. Figure 3d Only a small amount of 2-methylthiophene aggregated. Figure 3e The presence of 3-ethylthiophene in the form of blocky aggregates may be one of the main reasons for its performance differences.
[0140] 2. Device performance
[0141] Refer to Table 1, which is a comparison table of Examples 1-7 and their performance parameters. As shown in Table 1, the photoelectric conversion efficiency of Examples 1, 2, 4, 5, and 6 is greater than 10%, while the photoelectric conversion efficiency of 2-methylthiophene and 2-ethyl-5-methylthiophene is around 5%.
[0142] Further analysis, referring to Table 2 which shows the physical properties of each solvent, reveals that the sulfur-containing compounds used as solvents have different boiling points, dipole moments, steric hindrance, and volatility due to their different structures. This has a significant impact on the dissolution of the active layer material, resulting in significant differences in the performance of the prepared devices.
[0143] Figure 4 and Figure 5 The JV and EQE curves of different thiophene solvents visually represent the photovoltaic performance of the devices fabricated from them. It can be seen that 3-methylthiophene has high photovoltaic performance, reaching 16.87% PCE, which is significantly higher than other thiophene derivatives (such as 2-methylthiophene, 3-ethylthiophene, etc.).
[0144] Further, see Figure 6b and Figure 6e V, respectively, for devices prepared using different solvents OC and J SC Dependence of light intensity on the device's performance. For the V value characterized by the device in this experiment... OC -P light The curve. In the figure, the fitted n value represents: the n value is the ideality factor; the n value determines whether the carrier recombination type is unimolecular or bimolecular recombination. The closer the n value is to 1, the more predominantly bimolecular recombination is. The closer the n value is to 2, the more predominantly defect-assisted recombination is.
[0145] in, Figure 6b and Figure 6e The fitted n values for chloroform (CF), 3-methylthiophene, o-xylene (o-XY), 2-methylthiophene, 2,5-methylthiophene, and 3-ethylthiophene were 1.02, 1.08, 1.13, 1.27, 1.18, and 1.22, respectively. The n values for thiophene-based organic solvents were closer to 1 than those for chloroform (CF) and o-xylene (o-XY), indicating that single-molecule recombination in the device was effectively suppressed, and bimolecular recombination was the main mechanism.
[0146] See Figure 6a and Figure 6d J SC The relationship between light intensity and the fitted α value in the figure represents the following: α is typically in the range of 0.85 to 1. When α is close to 1, it means that the carrier loss within the battery due to molecular recombination and space charge effects is relatively small. Conversely, if α is much less than 1, it indicates that there is more carrier loss within the battery.
[0147] The fitted α values for 3-methylthiophene, chloroform (CF), o-xylene (o-XY), 2-methylthiophene, 2,5-methylthiophene, and 3-ethylthiophene were 0.937, 0.937, 0.936, 0.932, 0.935, and 0.933, respectively. The fitted α value for 3-MeT devices was closer to 1, indicating that bimolecular recombination was effectively suppressed in the device. Thiophene-based non-halogen solvents achieved superior efficiency in the preparation of the active layer compared to other halogen solvents (such as CF) in existing technologies. Furthermore, the combined use of thiophene solvents with end-capping polymers and organic compounds containing non-fullerene acceptors not only offers advantages such as environmental friendliness and low toxicity but also superior efficiency.
[0148] In other words, both bimolecular and monomolecular recombination in devices made with thiophene solvents (especially 3-methyl-substituted thiophene solvents) are effectively suppressed, which is beneficial to improving the efficiency of charge transport and extraction in the devices, thereby effectively increasing the current J. sc And the fill factor FF, thus ultimately achieving the desired efficiency.
[0149] See Figure 6c For Example 5 and Comparative Examples 1-2, the J of the device ph -V eff Dependency diagram; 6f represents the J-axis relationship of the device in Examples 5, 3, and 6. ph -V eff Dependency graph; J of the device is analyzed through the graph. ph -V eff Analysis of the dependence of these components can further reveal the generation and collection efficiency of photogenerated carriers in the device. As shown in the figure, the collection efficiencies of 3-methylthiophene, chloroform, and o-xylene are 86.4%, 85.2%, and 84%, respectively, while the generation efficiencies of photogenerated carriers are 97.5%, 97.5%, and 97.4%, respectively, showing relatively similar results. Overall, 3-methylthiophene exhibits slightly better exciton dissociation and charge collection efficiency than chloroform and o-xylene.
[0150] Furthermore, through Figure 6f It can be observed that 3-methylthiophene exhibits significantly higher photogenerated carrier generation and collection efficiencies compared to 2-methylthiophene and 3-ethylthiophene. This is due to its high exciton dissociation and charge collection efficiencies, thus enhancing the device's J... scAnd FF increases. For specific analysis, refer to Table 2. The dipole moment, spatial size, boiling point, vapor pressure, and electrostatic field distribution of the solvents listed in the table have certain differences, resulting in different molecular morphology and stacking of the active layer, thus leading to different crystallinity, mobility, and photovoltaic performance. Obviously, due to the higher dipole moment, suitable boiling point, and vapor pressure of 3-MeT, it stands out among the thiophene series solvents, resulting in devices with higher efficiency. Furthermore, as can be seen from the results in Table 2, its dipole moment is one of the influencing factors, but the effect, such as collection efficiency, needs to be considered from the comprehensive effect of multiple aspects.
[0151] Table 1 Comparison of performance parameters in Examples 1-7
[0152]
[0153]
[0154] Table 2. Dipole moment, spatial dimensions, and boiling point of the different solvents used in the examples and comparative examples.
[0155]
[0156] This invention also summarizes the production efficiency of multiple batches of different bromoanthracene PM6 and BO-4Cl, as shown in Table 3. Table 3 shows the production efficiency of each batch of bromoanthracene PM6 and BO-4Cl produced in Example 5, from batches 5-1 to 5-7 (7 batches in total). The average batch efficiency is between 15% and 16%. Table 3 shows that the batch-to-batch variability is low among different raw materials and batches, indicating good production stability in practical applications and playing a crucial role in ensuring the stable quality of the prepared devices. Clearly, the technical solution of this invention, utilizing thiophene-based solvents and active layer materials with thiophene structural units, can enhance the bonding stability between the solvent and the active layer material through the solvent effect, maintaining good stability during the preparation process and providing more stable and superior results for device fabrication. Furthermore, thiophene-based organic solvents, compared to chloroform (halogen-containing solvents) in the prior art, have low toxicity and are environmentally friendly, offering advantages in both processing and use.
[0157] Furthermore, based on the principle of like dissolves like, the excellent solubility of thiophene solvents and active layer materials with the same thiophene structure enables them to provide a stable solution system for the active layer material. It can be inferred that derivatives with the thiophene structure can also achieve the same result as solvents. Furthermore, thioether solvents should also be able to achieve similar effects.
[0158] Table 3 shows the efficiency of each batch (5-1 to 5-7) of bromoanthracene PM6 and BO-4Cl produced in Example 5.
[0159]
[0160] It should be understood that the technical solution of this application is not limited to the specific implementation examples mentioned above. Any technical modifications made to the technical solution of this application without departing from the spirit and scope of protection of the claims shall fall within the scope of protection of this application.
Claims
1. A method for preparing an OPV active layer using a sulfur-containing compound as a solvent, characterized in that, A solution prepared by dissolving the active layer material using a sulfur-containing compound as a solvent is spin-coated onto a substrate based on PEDOT:PSS or zinc oxide film, and then heated to form the OPV active layer. The structural formula of the sulfur-containing compound is: ; Among them, R9, R 10 R 11 R 12 R 13 R 14 R 15 R 16 R 17 R 18 A group that is independently a hydrogen atom, fluorine atom, chlorine atom, bromine atom, iodine atom, alkoxy chain, alkenyl, alkynyl, cyano, aryl, ester group, alkyl group with 1 to 30 carbon atoms, or a group in which one or more carbon atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of oxygen atom, alkenyl, alkynyl, aryl or ester group, or a group in which one or more hydrogen atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atom, chlorine atom, bromine atom, iodine atom, alkoxy chain, alkenyl, alkynyl, cyano, aryl or ester group; The active layer material is a binary mixture formed by a capped polymer containing thiophene structural units and an organic compound containing non-fullerene acceptors. The molar ratio of the end-capped polymer containing thiophene structural units to the organic compound containing non-fullerene acceptors is 0.5~2.0:1; The end-capped polymer containing thiophene structural units includes at least an end-capping agent and thiophene structural units; The thiophene structural unit has the structure shown in equation (Ⅰ): (Ⅰ); The structure of the end-capped polymer containing thiophene structural units is shown in formulas (II) and / or (III) and / or (IV): (Ⅱ)、 (Ⅲ)、 (Ⅳ); Where n is a natural number from 1 to 10000; R1, R2, R3, and R4 are independently hydrogen atoms, fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, cyano groups, or alkyl groups with 1 to 30 carbon atoms, or one or more carbon atoms on a C1 to C30 alkyl group are substituted by one or more functional groups selected from oxygen atoms, alkenyl groups, alkynyl groups, aryl groups, or ester groups, or one or more hydrogen atoms on a C1 to C30 alkyl group are substituted by one or more functional groups selected from fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms; X1 and X2 are substituents of hydrogen, fluorine, chlorine, bromine, iodine, cyano, or alkoxy chains; The main structural formula of the end-capping agent 1 or end-capping agent 2 is independently shown in any one of the following formulas: ; In the above structural formula, one or more carbon atoms on the aromatic ring can be replaced with N atoms or NR atoms; m is a natural number from 1 to 10000; R, R1, R2, R3, R4, R5, R6, R7, R8, and R9 are independently hydrogen atoms, fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, cyano groups, or alkyl groups with 1 to 30 carbon atoms, or groups in which one or more carbon atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of oxygen atoms, alkenyl, alkynyl, aryl, or ester groups, or groups in which one or more hydrogen atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, oxygen atoms, nitrogen atoms, alkoxy chains, alkenyl, alkynyl, aryl, carbonyl, amide, anhydride, or ester groups. Y and Y1 are independently oxygen atoms, sulfur atoms, selenium atoms, and nitrogen atoms with R7 attached, wherein R7 is an alkyl group with 1 to 30 carbon atoms, or a group in which one or more carbon atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of alkoxy chain, alkenyl, alkynyl, aryl or ester group, or a group in which one or more hydrogen atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atom, chlorine atom, bromine atom, iodine atom, alkoxy chain, alkenyl, alkynyl, aryl or ester group; The structural formula of the organic compound containing a non-fullerene acceptor is shown in formula (V): (Ⅴ), R5, R6, R7, and R8 are independently hydrogen atoms, fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, cyano groups, or alkyl groups with 1 to 30 carbon atoms, or groups in which one or more carbon atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of oxygen atoms, alkenyl, alkynyl, aryl, or ester groups, or groups in which one or more hydrogen atoms on a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, oxygen atoms, nitrogen atoms, alkoxy chains, alkenyl, alkynyl, aryl, carbonyl, amide, anhydride, or ester groups. X3, X4, X5, X6, X7, X8, X9, X 10 It can be a hydrogen atom, fluorine atom, chlorine atom, bromine atom, iodine atom, or alkoxy chain substituent independently; Y1, Y2, Y3, Y4, and Z are independently oxygen atoms, sulfur atoms, selenium atoms, and nitrogen atoms connected to R7, wherein R7 is an alkyl group with 1 to 30 carbon atoms, or a group in which one or more carbon atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of alkoxy chain, alkenyl, alkynyl, aryl, or ester group, or a group in which one or more hydrogen atoms of a C1 to C30 alkyl group are replaced by one or more functional groups of fluorine atom, chlorine atom, bromine atom, iodine atom, alkoxy chain, alkenyl, alkynyl, aryl, or ester group.
2. The method for preparing the OPV active layer using a sulfur-containing compound as a solvent according to claim 1, characterized in that, The molar ratio of the end-capped polymer containing thiophene structural units to the organic compound containing non-fullerene acceptors is 1:1.
2.
3. The method for preparing the OPV active layer using a sulfur-containing compound as a solvent according to claim 1, characterized in that, The capping agent is a bromoanthracene capping agent.
4. The method for preparing the OPV active layer using a sulfur-containing compound as a solvent according to claim 1, characterized in that, The organic compound containing a non-fullerene acceptor is BO-4Cl, and its structure is shown in formula (VI): (Ⅵ)。 5. The method for preparing the OPV active layer using a sulfur-containing compound as a solvent according to claim 1, characterized in that, The sulfur-containing compound includes any one or more of 2-ethylthiophene, 3-methylthiophene, 2-propylthiophene, 2-butylthiophene, 3-ethylthiophene, 2,4-dimethylthiophene, 2,5-dimethylthiophene, 3,4-dimethylthiophene, 3,4-dimethylthiophene, tetrahydrothiophene, 2-methyltetrahydrothiophene, diethyl sulfide, dipropyl sulfide, and dibutyl sulfide, mixed in any proportion as a mixed solvent.
6. An OPV active layer, prepared by the preparation method according to any one of claims 1-5.
7. An organic solar cell, characterized in that, From bottom to top, the layers consist of a stacked ITO glass substrate, a hole or electron transport layer, an OPV active layer, an electron or hole transport layer, and a metal electrode. The OPV active layer is the OPV active layer as described in claim 6.
8. A method for preparing an organic solar cell as described in claim 7, characterized in that, Includes the following steps: S1. Preparation of ITO glass substrate: The ITO glass substrate is obtained by cleaning and drying ITO glass; S2. Preparation of hole or electron transport layer: PEDOT:PSS or zinc oxide solution is spin-coated onto the ITO glass substrate prepared in S1, and the hole transport layer is obtained after thermal annealing. S3. Preparation of the OPV active layer: The end-capped polymer containing thiophene structural units and BO-4Cl are dissolved in a sulfur-containing solvent and spin-coated onto the hole transport layer prepared in S2 to obtain the OPV active layer; S4. Preparation of electron or hole transport layer: PFN-Br solid powder is dissolved in methanol and spin-coated onto the surface of the OPV active layer to obtain the electron transport layer, forming a multilayer device structure; Alternatively, the hole transport layer can be obtained by vacuum thermal evaporation of molybdenum oxide, forming a multilayer device structure; S5. Preparation of metal electrodes: The multi-layered device structure obtained in S4 is subjected to alkaline vacuum evaporation to form a metal electrode layer on the surface of the transport layer; Thus, organic solar cells with multilayer structures, upright structures, or inverted structures have been prepared.
Citation Information
Patent Citations
Organic solar cell processed by non-halogen solvent and based on polythiophene system and preparation method of organic solar cell
CN114883500A
Organic photovoltaic devices comprising fullerenes and derivatives thereof
CN101529610A
Dithienyldiazosulfide unit-containing polymer, preparation method thereof and solar cell device
CN103848977A