Method for producing microporous carbon material

By using halogen gas and hydrogen to treat metal carbide materials in a fluidized bed reactor, the problem of the pore size of microporous carbon materials increasing with temperature is solved, and the production of microporous carbon materials with excellent pore structure is achieved, which is suitable for For high-performance supercapacitors and secondary battery electrodes.

CN117120368BActive Publication Date: 2024-10-15SKELETON TECH GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280024075.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-24
Filing Date
2022-03-16
Publication Date
2024-10-15
Estimated Expiration
2042-03-16

AI Technical Summary

Technical Problem

In the existing process for manufacturing microporous carbon materials, the pore size increases as the synthesis temperature increases, resulting in the pore size of the microporous carbon material being not small enough, affecting its high volume capacity performance in batteries and supercapacitors.

Method used

The metal carbide material is fluidized using halogen gas or a gas mixture containing halogen gas in a fluidized bed reactor, followed by desorption of the halogen gas under vacuum, passivation treatment in a hydrogen atmosphere, and finally pulverization to obtain D90 of 10 μm to 30 μm. Particle size and microporous carbon material with D10 particle size of 1.5 μm to 2 μm.

Benefits of technology

The production of microporous carbon materials with suitable pore structure has been achieved, which improves its performance in the field of energy storage. It is especially suitable for electrode materials of supercapacitors and secondary batteries to enhance energy storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117120368B_ABST
    Figure CN117120368B_ABST
Patent Text Reader

Abstract

In order to improve the production of microporous carbon materials, especially microporous carbon materials for electrodes of supercapacitors and secondary batteries, a method is proposed, in which a granular metal carbide material is fluidized with a halogen gas at high temperature in a fluidized bed reactor, the halogen gas is desorbed at a lower temperature of 150°C to up to 250°C under vacuum, and the material is then passivated using hydrogen and then ground.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for manufacturing microporous carbon material. Background Art

[0002] The terms macropores, mesopores and micropores are used herein based on the classification adopted by IUPAC, according to which macropores have a pore size greater than 50 nm, mesopores have a pore size between 2 nm and 50 nm, and micropores have a pore size less than 2 nm.

[0003] The particle size is measured here by laser diffraction in a liquid medium. Auxiliary materials such as surfactants can be used. The measurement is evaluated according to Mie and / or Fraunhofer.

[0004] Methods for producing microporous carbon materials from metal carbide materials are known, for example, from WO 98 / 54111 A1 and US Pat. No. 8,137,650 B2.

[0005] Microporous carbon materials are popular electrode materials for applications in batteries and supercapacitors. It has been found that smaller pore sizes are essential for high volumetric capacity (farad / cm 3 However, a problem with conventional manufacturing processes is that the pore size increases with increasing synthesis temperature.

[0006] However, higher temperature is advantageous during the reaction because it causes the reaction to proceed faster, thereby increasing productivity. Summary of the invention

[0007] The object of the present invention is to disclose an improved method for manufacturing microporous carbon materials.

[0008] This object is achieved by the subject matter of the independent claim. Preferred further embodiments are subject matter of the dependent claims.

[0009] The present invention provides a method for manufacturing a microporous carbon material, the method comprising the following steps:

[0010] a) fluidizing a granular metal carbide material by a halogen gas or a gas mixture containing a halogen gas at a temperature of 800° C. to 1300° C. (inclusive) in a fluidized bed reactor;

[0011] b) maintaining the product obtained in step a) at a temperature of 150° C. to a maximum of 250° C. (inclusive) and under a vacuum of 1 mbar to 300 mbar (inclusive); and thereafter or subsequently

[0012] c) maintained under an atmosphere of hydrogen or a gas mixture at a temperature of 800° C. to 1300° C., inclusive, the gas mixture comprising at least 30% by volume of hydrogen based on the total volume of the gas mixture; and

[0013] d) crushing to a D90 particle size of 10 μm to 30 μm (both inclusive), and a D10 particle size of 1.5 μm to 2 μm (both inclusive).

[0014] Preferably, the halogen gas is a gas containing at least one halogen atom. HCl and Cl2 are examples of halogen gases.

[0015] Preferably, in step a), the gas mixture consists of a halogen gas and an inert gas which is inert at the temperature.

[0016] Preferably, in step a), the gas mixture consists of a halogen gas and a reaction gas which reacts with the metal carbide material at the temperature.

[0017] Preferably, in step a), the gas mixture consists of a halogen gas, an inert gas and a reactive gas.

[0018] Preferably, the inert gas is selected from the group consisting of helium, neon, argon, krypton and xenon. Preferably, the inert gas is argon.

[0019] Preferably, the reaction gas is selected from the group consisting of carbon monoxide, carbon dioxide and water.

[0020] Preferably, the halogen gas is a gas containing at least one halogen atom. HCl and Cl2 are examples of halogen gases.

[0021] Preferably, in step a), the gas mixture consists of a halogen gas and an inert gas which is inert at the temperature.

[0022] Preferably, in step a), the gas mixture consists of a halogen gas and a reaction gas which reacts with the metal carbide material at the temperature.

[0023] Preferably, in step a), the gas mixture consists of a halogen gas, an inert gas and a reactive gas.

[0024] Preferably, the inert gas is selected from the group consisting of helium, neon, argon, krypton and xenon. Preferably, the inert gas is argon.

[0025] Preferably, the reaction gas is selected from the group consisting of carbon monoxide, carbon dioxide and water.

[0026] Preferably, the D90 particle size of the metal carbide material is greater than 10 μm to 500 μm (including 500 μm), preferably 50 μm (including 50 μm) to 200 μm, more preferably 120 μm to 180 μm. The particle size distribution may be unimodal or multimodal, preferably bimodal.

[0027] Preferably, in step a), after fluidization with the halogen gas or gas mixture, fluidization with a purge gas is carried out in a fluidized bed reactor at a temperature of 800° C. to 1300° C. (inclusive), wherein the purge gas does not react with carbon at least at this temperature.

[0028] Preferably, in step a), during the fluidization process, the temperature is 900°C to 1200°C (inclusive), preferably 1000°C to 1100°C (inclusive), preferably 950°C to 1050°C (inclusive), preferably 980°C to 1020°C (inclusive).

[0029] Preferably, the purge gas is selected from the group consisting of helium, neon, argon, krypton and xenon. Preferably, the purge gas is argon.

[0030] Preferably, the metal carbide material is selected from the group consisting of ternary carbide materials, vanadium carbide materials, titanium carbide materials, molybdenum carbide materials, silicon carbide materials, tungsten carbide materials, tantalum carbide materials and niobium carbide materials. Preferably, the metal carbide material is selected from the group consisting of VC, TiC, MoC, SiC, WC, TaC and NbC. Preferably, the metal carbide material is silicon carbide material or SiC. Preferably, the halogen gas is chlorine.

[0031] Preferably, in step a), the halogen gas is supplied in an amount of 100% to 110% (inclusive) of the stoichiometrically required amount. Preferably, in step b), the vacuum degree is 5 mbar to 200 mbar (inclusive) of the stoichiometrically required amount.

[0032] Preferably, in step b), the vacuum degree is 5 mbar to 200 mbar (both inclusive), preferably 5 mbar to 80 mbar (both inclusive), more preferably 8 mbar to 15 mbar (both inclusive), more preferably 10 mbar.

[0033] Preferably, step a) is performed for a duration of 8 hours to 13 hours (both inclusive).

[0034] Preferably, step b) is performed for a duration of 12 hours to 30 hours (both inclusive).

[0035] Preferably, step c) is performed for a duration of 2 hours to 4 hours (both inclusive).

[0036] Preferably, in step a), the duration of fluidization with the halogen gas or gas mixture is 9 hours to 13 hours (both inclusive), and the duration of fluidization with the purge gas is 1.5 hours to 2.5 hours.

[0037] Preferably, in step a), the duration of the fluidization with the halogen gas or gas mixture is from 2.5 hours / kg to 3.5 hours / kg of metal carbide material.

[0038] Preferably, step b) is performed for a duration of 22 hours to 26 hours (both inclusive).

[0039] Preferably, step b) is performed for a duration of 22 hours to 26 hours (both inclusive).

[0040] Preferably, step c) is performed before step d). Preferably, step d) is performed before step c). Preferably, step c) is performed before step d), and then step c) is performed again with a shorter duration, preferably a duration of not less than 15 minutes.

[0041] Preferably, step b) is performed using a fluidized bed reactor.

[0042] Preferably, step c) is carried out using a fluidized bed reactor or using a tubular kiln or a rotary kiln.

[0043] One concept of the present invention is to produce microporous carbon materials for use in the field of energy storage. In particular, an increase in the yield of carbon materials will be achieved, as well as a pore structure that is particularly useful for energy storage applications. The present invention follows the basic principle of treating metal carbide materials with halogen gases and producing microporous carbon materials through the reaction. This type of carbon material is called "carbide-derived carbon" or CDC for short.

[0044] Metal carbide material, such as silicon carbide, is fed into the fluidized bed reactor as particles with a particle size of about 150 μm. Preferably, 90% of the particles have a size less than 150 μm, referred to as D90 of 150 μm. In principle, other particle sizes up to about 500 μm are also conceivable. In order to achieve acceptable fluidization of the metal carbide powder in the fluidized bed reactor, the gas flow rate should be adjusted.

[0045] During the treatment with halogen gas (e.g. chlorine), the metal is removed from the metal carbide material and blown out of the reactor as gaseous metal halide due to the high temperature. What remains is a carbon material that must be processed in further steps in order to finally obtain the properties required for energy storage manufacturing. These properties are influenced, among other things, by the polymer size, particle size and carbon surface functional groups.

[0046] In order to remove excess halogen gas from the reactor and materials, the fluidized bed reactor is preferably purged with an inert gas (eg, argon) at elevated temperature.

[0047] Advantageously, after the halogen treatment and purging with an inert gas, the material is heated under vacuum to a moderate temperature of up to about 250° C. In this way, halogen-containing impurities can be removed from the material more effectively.

[0048] The dehalogenated material may still have cleaved bonds or unsaturated bonds, also known as "dangling bonds". Treating the material with hydrogen at high temperature can saturate the cleaved bonds, effectively removing them. Therefore, the possibility of undesirable substances accumulating on the carbon material due to cleaved bonds can be reduced.

[0049] Advantageously, the carbon material is used to manufacture energy storage batteries, such as supercapacitors and secondary batteries. In particular, the carbon material is used in at least one electrode of the battery. For this reason, it is advantageous to be able to produce a fine suspension or slurry, also referred to as "slurry", with the carbon material. This particle size also allows the production of so-called dry electrodes. The carbon material can be pulverized before or after treatment with hydrogen, for example in a grinder such as a ball mill or a jet mill.

[0050] A D90 particle size of 10 to 30 μm has proven to be particularly useful in practice. Preferably, the particles should have a D10 particle size of greater than 1.5 to 2 μm.

[0051] In general, the concepts described herein can be used to produce microporous carbon materials suitable for use in the fabrication of supercapacitors and secondary batteries.The microporous carbon materials disclosed herein have all three types of pores, namely micropores, mesopores, and macropores. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Examples of embodiments are explained in more detail with reference to the accompanying schematic diagrams.

[0053] Figure 1 A schematic flow chart depicting the manufacturing process;

[0054] Figure 2 Scanning electron micrographs depicting cross-sections of particles after synthesis and before size reduction; and

[0055] Figure 3 The pore size distribution of the material is depicted. DETAILED DESCRIPTION

[0056] Reference below Figure 1 , which shows an embodiment of a method for making a microporous carbon material.

[0057] The method comprises a processing step S100. In the processing step S100, a particulate metal carbide material, such as silicon carbide, is first fed into a fluidized bed reactor. The reactor and the metal carbide material are heated to a temperature of about 1000° C. Lower temperatures starting from 800° C. are also conceivable. The heating process preferably takes 1 to 1.5 hours.

[0058] The metal carbide material is then fluidized by a halogen gas, preferably chlorine. The volumetric flow rate of the chlorine gas is adjusted so that about 100% to 110% of the stoichiometrically required amount of chlorine gas flows through the fluidized bed reactor.

[0059] The high temperature fluidization is performed in a fluidized bed reactor for about 2.5 hours / kg to 3.5 hours / kg of the metal carbide material.

[0060] After the halogen treatment is completed, the fluidized bed reactor is fluidized with a purge gas at a constant high temperature. In this way, the purge gas will not react with the carbon even at a high temperature of 1000° C. A preferred purge gas is, for example, argon. The purge gas can also be a mixture of multiple substances.

[0061] The method further comprises a desorption step S102. In the desorption step, the product obtained in the previous step is taken out of the fluidized bed reactor and maintained under a low vacuum of about 10 mbar, preferably at a temperature of 195° C. to 205° C. During this process, excess halogen gas escapes from the material. The halogen gas decomposed from the material can obviously move the powder material.

[0062] Preferably, the desorption step S102 is performed at least until the visible movement of the material stops. The desorption step S102 can still have a small safety period of about 15 minutes to 30 minutes, through which the step is performed longer. The desorption step can also be performed without separate monitoring. In this case, the desorption step S102 is performed for (for example) 12 hours to 24 hours.

[0063] The method further comprises a passivation step S104 and a grinding step S106. These steps are performed after the processing step S100 and the desorption step S102.

[0064] For the passivation step S104, the material obtained from the previous step is charged into a rotary kiln or a fluidized bed reactor. The material is heated to a temperature of about 1000° C. and contacted with hydrogen or a gas mixture containing at least 50% by volume of hydrogen in the total volume of the gas mixture. In the case of a fluidized bed reactor, the material is fluidized with hydrogen or a gas mixture.

[0065] The duration of the passivation step is preferably based on the total dissolved solids (TDS) value of the passivation material. To determine the TDS value, the carbon is boiled in distilled water for 10 minutes and the filtered water is measured at 25°C using a conductivity probe. The passivation step S104 is carried out at least until the TDS value reaches or falls below 50pS / cm. This is because in this case, the risk of damaging the electrode due to corrosion of the slurry increases. The passivation step S104 is preferably carried out to a TDS value between 2.5μS / cm and 50μS / cm, preferably at most 10μS / cm, and more preferably at most 5μS / cm.

[0066] Then, in the crushing step S106, the passivation material is crushed into a D90 particle size of 10 μm (including 10 μm) to 15 μm (including 15 μm) and a D10 particle size of greater than 1.5 μm to 2 μm. These particle sizes allow the formation of a slurry that is particularly suitable for further processing to produce supercapacitors and secondary batteries or their electrodes.

[0067] The crushing step S106 may be performed before or after the passivation step S104. If the crushing step S106 is performed after the passivation step S104, it is advantageous to perform the passivation step S104 again, but for a shorter duration than the first time.

[0068] Example 1: Carbon material made of SiC

[0069] Reference below Figure 2 and Figure 3 , which shows the characteristics of microporous carbon materials obtained by the aforementioned SiC-based method.

[0070] Figure 2 A scanning electron microscope image of a cross section of a single particle prepared according to the invention is shown. Macropores are clearly present in the material.

[0071] from Figure 3 It can be seen that carbon materials have a large number of pores and The most common pore size is about

[0072]

[0073] In addition to these micropores, the material also has pores larger than to almost The most common micropores in this range are about to It has been shown that this pore distribution, including macropores, is particularly suitable for the fabrication of supercapacitors and secondary batteries.

[0074] The porosity is determined by nitrogen physical adsorption combined with Brunauer-Emmet-Teller (BET) and Rouquerol evaluation methods as described by Thommes et al. in the lUPAC Technical Report "Physisorption of gases, with special reference to the evaluation of surface area and pore size distribution (IUPAC Technical Re-port)", Pure Appl. Chem. Chem. 2015; 87 (9-10): 1051-1069. This disclosure is specifically incorporated herein by reference. The total pore volume is determined using BET, while the micropore volume is determined using density functional theory (DFT). Since not all assumptions of the BET method apply to microporous materials, the surface areas determined by the BET method and the DFT method may conflict. Observing the pore size distribution can correctly estimate the ratio between the surfaces, that is, how much of the surface area of ​​the carbon material is caused by micropores.

[0075] Using the method proposed in this paper, the microporous carbon material produced from SiC has a 2 / g surface area and 0.6cm 3 / g of total pore volume. According to IUPAC, the total pore volume is determined at a relative pressure of 0.95. In this paper, the micropore volume accounts for about 0.5cm 3 / g, the micropore surface area is about 1334m 2 / g. Consider Figure 3 From the pore size distribution in Figure 1, we can conclude that almost the entire surface area is caused by micropores, and the diameter of most micropores is and between.

[0076] In addition, the microporous carbon material produced by the method has an ash content of less than 1 wt % based on the total mass of the microporous carbon material. The bone density is about 2.277 g / cm 3 Up to 2.451g / cm 3 Bone density was measured by constant volume helium pycnometer (using a gas pycnometer AccuPyc II from Micromeritics).

[0077] Using standard spectroscopic techniques, the carbon material was shown to contain graphitic and amorphous structures (Raman spectroscopy) and to be free of oxygen-containing groups on the surface (infrared spectroscopy).

[0078] Example 2: Carbon material made of TiC

[0079] TiC was used as the carbide material and the method described above was followed. The pore size distribution was similar to that of SiC, but the main peak was at The surface area of ​​the carbon material is about 1681 m 2 / g, with a total pore volume of 0.8 cm 3 / g. Among them, the micropore volume accounts for 0.6cm 3 / g, the micropore surface area is about 1448m 2 / g

[0080] Comparative Example: Commercially available activated carbon

[0081] Commercial activated carbon is available from Kuraray under the trade name YP-50F. The surface area of ​​carbon is about 1707m 2 / g, with a total pore volume of 0.9 cm 3 / g. The micropore volume accounts for 0.6cm 3 / g, micropore surface area is 1289m 2 / g.

[0082] In order to improve the production of microporous carbon materials, especially microporous carbon materials for electrodes of supercapacitors and secondary batteries, a method is proposed, in which a granular metal carbide material is fluidized with a halogen gas at high temperature in a fluidized bed reactor, the halogen gas is desorbed at a lower temperature of 150°C to up to 250°C under vacuum, and the material is then passivated using hydrogen and then ground.

Claims

1. A method for manufacturing a microporous carbon material, the method comprising the following steps: a) fluidizing a particulate metal carbide material by a halogen gas or a gas mixture comprising a halogen gas at a temperature of 800° C. to 1300° C. in a fluidized bed reactor; b) maintaining the product obtained in step a) at a temperature of 150° C. to a maximum of 250° C. and under a vacuum of 1 mbar to 300 mbar pressure, inclusive; and thereafter or subsequently c) maintained under an atmosphere of hydrogen or a gas mixture at a temperature of 800° C. to 1300° C. inclusive, the gas mixture comprising at least 30% by volume of hydrogen based on the total volume of the gas mixture; and d) crushing to a D90 particle size of 10 μm to 30 μm and a D10 particle size of 1.5 μm to 2 μm; The microporous carbon material has all three types of pores, namely micropores, mesopores and macropores; in: Step a) is carried out for a duration of 8 hours to 13 hours, inclusive; Step b) is carried out for a duration of 12 hours to 30 hours inclusive; and Step c) is carried out for a duration of 2 hours to 4 hours inclusive.

2. The method according to claim 1, wherein step a) comprises: After fluidization with the halogen gas or gas mixture, fluidization is carried out in a fluidized bed reactor at a temperature of 800° C. to 1300° C. with a purge gas which at least does not react with the carbon at this temperature and is selected from the group consisting of helium, neon, argon, krypton and xenon. The method according to claim 2 , wherein the purge gas is argon.

4. The method according to claim 1, wherein the metal carbide material is selected from the group consisting of vanadium carbide material, titanium carbide material, molybdenum carbide material, silicon carbide material, tungsten carbide material, tantalum carbide material and niobium carbide material; or wherein the metal carbide material is silicon carbide material, and wherein the halogen gas is chlorine gas.

5. The method according to claim 1, wherein in step a), the halogen gas is supplied in an amount ranging from 100% to 110% inclusive of the stoichiometrically required amount.

6. The method according to claim 1, wherein in step b), the vacuum is from 5 mbar to 200 mbar inclusive.

7. The method according to claim 1, wherein in step b), the vacuum is between 5 mbar and 80 mbar inclusive.

8. The method according to claim 1, wherein in step b), the vacuum is comprised between 8 mbar and 15 mbar.

9. The method according to claim 1, wherein in step b), the vacuum is 10 mbar.

10. The method of claim 1, wherein: In step a), the duration of fluidization with halogen gas is from 9 hours to 11 hours, and the duration of fluidization with purge gas is from 1.5 hours to 2.5 hours; and Step b) is carried out for a duration of 22 to 26 hours.

11. The method according to any one of claims 1 to 10, wherein step c) is performed before step d); or wherein step d) is performed before step c); or wherein step c) is performed before step d) and then step c) is performed again for a shorter duration.

12. The process according to any one of claims 1 to 10, wherein step b) is performed using a fluidized bed reactor.

13. The method according to any one of claims 1 to 10, wherein step c) is performed using a fluidized bed reactor or using a rotary kiln.