A production method for in-situ synthesis of zinc oxide-containing emulsion foaming material
Zinc oxide is generated in emulsion foam materials through in-situ synthesis, which solves the problem of filler agglomeration, achieves efficient foaming and foam stability, expands the applicable scope of the material, and has various performance advantages.
Patent Information
- Application Number
- CN202310977790.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-04
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-08-04
AI Technical Summary
When adding fillers to existing emulsion foaming materials, it is easy to cause particle agglomeration, which affects the utilization rate of the foaming agent and material strength. The application range is narrow, making it difficult to prepare low-density foaming materials.
Using in-situ synthesis method, zinc oxide is generated in the metal matrix through the reaction of basic zinc carbonate with polymer emulsion and hydrogen peroxide solution, which avoids the agglomeration of fillers and forms a uniform foaming layer or coating under high temperature conditions. layer, acting as a foaming and cross-linking accelerator.
It achieves uniform distribution and efficient foaming of zinc oxide, improves the foam stability and applicable range of the material, reduces production costs, and has antibacterial, photosensitive degradation and other properties, and is suitable for polymer emulsions and continuous fabric surfaces that are not resistant to high temperatures. foaming treatment.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of zinc oxide materials, in particular to a production method for in-situ synthesizing zinc oxide-containing emulsion foaming material. Background Art
[0002] Emulsion foaming materials have many uses in the fields of three-dimensional foaming printing, emulsion foaming elastic pads, emulsion foaming coating smoke filter materials, emulsion foaming camouflage materials, etc. The better the dispersion of the filler in the matrix, the smaller the degree of agglomeration and the smaller the pores. In addition, the addition of a large amount of filler will inevitably cause the filler to partially agglomerate, and the loose structure of the agglomerated part will become the main channel for the escape of the foaming agent gas, resulting in low utilization of the final foaming agent and difficulty in preparing low-density foaming materials. The additional addition of fillers has a great impact on the pore structure of emulsion foaming materials. At present, most manufacturers choose to stop boiling with soup and abandon the additional addition of fillers, but the strength of the foaming material is low and the function given by the filler cannot be realized. The in-situ synthesis method is a method in which chemical reactions between elements or compounds react in the metal matrix to generate reinforcement particles during the preparation of metal composite materials. This method was developed in the 1980s. In the past, the in-situ synthesis method was almost only used for metal-based composite materials. Among them, the patent title of CN113621164B is "A method for producing an in-situ synthesized zinc oxide emulsion foaming material". The in-situ synthesized zinc oxide emulsion foaming material uses a precursor basic zinc carbonate emulsion to avoid the particle agglomeration caused by the addition of filling zinc oxide in the past. At the same time, the uniformly distributed zinc oxide is generated, and it is used for foaming treatment of the surface of high-temperature resistant fibers such as aramid, polybenzimidazole, rock carbon fiber fabric, or foaming of the surface coating of high-temperature resistant filter materials. Its polymer emulsion is a polyimide emulsion and a polytetrafluoroethylene emulsion, which are high-temperature resistant polymers. It is not suitable for polymer emulsions and filter materials that are not resistant to high temperatures, and its application range is narrow and greatly limited. In order to solve the above problems, those skilled in the art are in urgent need of developing a method for producing an in-situ synthesized zinc oxide emulsion foaming material and its application to meet the existing market demand and performance requirements. Summary of the invention
[0003] In view of the above problems, the present invention aims to provide a production method and application of an in-situ synthesized zinc oxide-containing emulsion foaming material.
[0004] A method for in-situ synthesizing a zinc oxide-containing emulsion foaming material comprises the following steps:
[0005] The first step is to prepare basic zinc carbonate and add it into water to form basic zinc carbonate paste; the second step is to mix the basic zinc carbonate paste with the polymer emulsion and add hydrogen peroxide solution to obtain a basic zinc carbonate paste foaming emulsion;
[0006] After basic zinc carbonate and polymer emulsion are mixed, hydrogen peroxide solution is added, the reaction releases carbon dioxide, and zinc peroxide is formed, and initial foaming occurs;
[0007] In the past, zinc peroxide was used as 510 ointment to sterilize and astringe, and was used for disinfection and cleaning of skin and wounds. After the zinc peroxide is formed, it is further evenly scraped to form a foaming layer or evenly filled in the cavity or to form a foaming coating. Further cross-linking is carried out by heating, and hydrogen peroxide decomposes at a higher temperature, while generating zinc oxide in situ and releasing oxygen, forming a foaming effect, and can also act as a cross-linking accelerator;
[0008] The third step is to evenly scrape the basic zinc carbonate foaming emulsion on the stainless steel belt to form a foaming layer; or add the basic zinc carbonate paste foaming emulsion into the mold to evenly fill the basic zinc carbonate paste foaming emulsion in the mold cavity to obtain expandable material; or apply the basic zinc carbonate paste foaming emulsion on the continuous fabric by using the foaming coating process to form a foaming coating; the fourth step is heat treatment foaming: heating the foaming layer obtained in the previous step to crosslink and foam; heating the foaming coating obtained in the previous step to crosslink and foam; heating the expandable material obtained in the previous step to crosslink and foam; cooling to room temperature after foaming to obtain the in-situ synthesized zinc oxide emulsion foaming material.
[0009] Furthermore, the mass fraction of the basic zinc carbonate paste is 50% to 60%.
[0010] Furthermore, the polymer emulsion is one of natural rubber emulsion, phenolic resin emulsion and polytetrafluoroethylene emulsion.
[0011] Furthermore, the mass ratio of basic zinc carbonate paste, polymer emulsion and hydrogen peroxide solution is 3-5:1-2:6-7.
[0012] Furthermore, the mass concentration of the hydrogen peroxide solution is 33-35%.
[0013] Furthermore, the uniform coating amount on the stainless steel belt is 400g / m 2 .
[0014] Furthermore, the continuous fabric is polyester non-woven fabric or polyimide non-woven fabric.
[0015] Furthermore, the foam density of the basic zinc carbonate paste foaming emulsion in the second step is 350-550 g / L.
[0016] Furthermore, the foaming coating process is a scraping amount of 150 to 190 g / m 2 , and then pre-bake at 80-90°C for 60-120s.
[0017] Beneficial effects of the present invention:
[0018] In daily production practice, it is found that the fillers added to the emulsion foaming material are not only easy to agglomerate, but also require the addition of additional dispersants and foaming agents, and the composition is complex. In addition, the additional powdered solid fillers usually have a certain foam breaking effect. For example, fillers such as heavy calcium will settle when the slurry is placed, which will reduce the foam stability and cause a large number of bubbles to burst. The density of wood powder is small and basically has no charge. Fillers such as wood powder fibers are distributed in large quantities on the surface of the liquid film, changing the local tension of the liquid film. Therefore, during the drying process, the bubbles are mostly incomplete, affecting the molding. Adding additional fillers such as zinc oxide still cannot change the above disadvantages.
[0019] The production method of the zinc oxide-containing emulsion foaming material disclosed in the present invention adopts basic zinc carbonate as a raw material and is prepared by an in-situ synthesis method, thereby avoiding the disadvantage of agglomeration of additionally added zinc oxide fillers to a great extent, and does not affect the foaming and foam stability of the emulsion foaming material. The pore structure is complete, and multiple functions of fillers, foaming agents, and co-vulcanizing agents are exerted in the process.
[0020] Relying on the in-situ reaction, zinc oxide filler is generated inside the emulsion foaming material, and it also has the foaming function. Compared with the additional addition of zinc white filler, the in-situ synthesis method has lower production cost, simple material formula and simple production process. Zinc oxide is formed in the production process of emulsion foaming material. The size of zinc oxide prepared by the in-situ synthesis method is also smaller and more evenly distributed. While generating zinc oxide, it also acts as a foaming agent and is evenly dispersed, avoiding the agglomeration of particles caused by the addition of filling zinc oxide in the past. At the same time, while the uniformly distributed zinc oxide is generated, the gas escape is also uniform, the emulsion expands evenly, forming pores of uniform size, and better uniform foaming. It has a wide applicable temperature range and is applicable to many types of polymer emulsions. It can be used for foaming treatment of the surface of polyester non-woven fabrics that are not resistant to high temperature continuous fabrics. After drying and baking, the pattern is foamed and thickened, presenting a three-dimensional state, or the surface coating is foamed to obtain antibacterial, photosensitive degradation and other properties, as well as natural rubber emulsion and other polymer emulsions that are not resistant to high temperature foaming molding. DETAILED DESCRIPTION
[0021] The present invention is described below with specific examples, but is not intended to be limiting of the present invention. Example 1
[0022] Raw materials and equipment: Jiangsu Jiahe JH830 foaming furnace, coating scraper JLTD20×120×2000, Kuntai industrial grade high-quality basic zinc carbonate; Dongzhi Huaertai industrial hydrogen peroxide; sea glue natural rubber latex with a solid content of 62%,
[0023] The production method of in-situ synthesized zinc oxide-containing emulsion foaming material comprises the following steps:
[0024] The first step is to prepare basic zinc carbonate and add it to water to form basic zinc carbonate paste, and the mass fraction of the basic zinc carbonate paste is 50%; the second step is to mix the basic zinc carbonate paste with natural rubber emulsion at a mass concentration of 33% of the hydrogen peroxide solution, and add the hydrogen peroxide solution, and the mass ratio of the basic zinc carbonate paste, the natural rubber emulsion, and the hydrogen peroxide solution is 3:1:6 to obtain a basic zinc carbonate paste foaming emulsion, and the foam density of the basic zinc carbonate paste foaming emulsion is 350g / L; the third step is to evenly scrape the basic zinc carbonate foaming emulsion on the stainless steel belt to form a foaming layer, and the evenly scraped amount on the stainless steel belt is 400g / m 2 ; The fourth step is heat treatment and foaming: the foaming layer obtained in the previous step is heated to cross-link and foam; after foaming, it is cooled to room temperature to obtain the in-situ synthesized zinc oxide emulsion foaming material.
[0025] Product: Apparent density 413.2kg / m 3 , compression permanent deformation 40.2%; tensile strength 20.4kPa; elongation at break 95.6%; indentation hardness 320N; moisture content 3.0%; indentation ratio 3.0;
[0026] Note: Compression set determination Compression set determination is carried out according to method A in GB / T6669-2008, compressing 50% of the sample thickness. Before the test, the sample should be conditioned at a temperature of 27°C and a relative humidity of 65% for 16 hours. Determination of tensile strength and elongation at break The determination of tensile strength and elongation at break is carried out according to the provisions of GB / T6344-2008. Before the test, the sample should be conditioned at a temperature of 27°C and a relative humidity of 65% for 16 hours. Aging performance is carried out according to the provisions of GB / T9640-2008, with an aging time of 22 hours and an aging temperature of 100°C. The determination of surface hardness is carried out according to method A in GB / T10807-2006. Before the test, the sample should be conditioned at a temperature of 27°C and a relative humidity of 65% for at least 16 hours. Determination of tear strength The tear strength is determined according to the provisions of GB / T10808-2006. Before the test, the sample should be conditioned at a temperature of 27°C and a relative humidity of 65% for at least 16 hours. The moisture content is determined using a moisture tester. Example 2
[0027] The basic zinc carbonate paste foaming emulsion obtained in the second step of Example 1 was coated on a 80g / m2 2 The hot-rolled non-woven fabric TDB-80 polyester non-woven continuous fabric is used to form a foaming coating. The foaming coating process is a foaming ratio of 1:3 and a coating amount of 150g / m 2, and then pre-bake at 80°C for 120s; the fourth step, heat treatment and foaming: heat the foaming coating obtained in the previous step to 150°C for cross-linking and foaming and bake for 5 minutes; cool to room temperature after foaming to obtain a polyester non-woven fabric coated with an in-situ synthesized zinc oxide emulsion foaming material. Example 3
[0028] Raw materials and equipment: Jiangsu Jiahe JH830 foaming furnace, coating scraper JLTD20×120×2000, Kuntai industrial-grade superior basic zinc carbonate; Dongzhi Huaertai industrial hydrogen peroxide; JF-4DCAF4 polytetrafluoroethylene dispersion emulsion.
[0029] The production method of in-situ synthesized zinc oxide-containing emulsion foaming material comprises the following steps:
[0030] The first step is to prepare basic zinc carbonate and add it to water to form basic zinc carbonate paste, and the mass fraction of the basic zinc carbonate paste is 55%; the second step is to mix the basic zinc carbonate paste with polytetrafluoroethylene dispersion emulsion with a mass concentration of 34% of the hydrogen peroxide solution, and add the hydrogen peroxide solution, the mass ratio of the basic zinc carbonate paste, the polytetrafluoroethylene dispersion emulsion, and the hydrogen peroxide solution is 4:2:7, and the basic zinc carbonate paste foaming emulsion is obtained, and the foam density of the basic zinc carbonate paste foaming emulsion is 350-550g / L; the third step is to apply the basic zinc carbonate paste foaming emulsion on the Litongda P84 polyimide non-woven fabric with an average pore size of 90μm, a filtration efficiency of 42%, and a filtration resistance of 43Pa by a foaming coating process to form a foaming coating, and the foaming coating process is a scraping amount of 190g / m 2 , and then pre-bake at 90°C for 60s; the fourth step, heat treatment foaming: the foaming coating obtained in the previous step is heated to 390°C for 30min for cross-linking and foaming; after foaming, it is cooled to room temperature to obtain the in-situ synthesized zinc oxide emulsion foaming material.
[0031] The obtained PTFE foam coated polyimide nonwoven fabric had an average pore size of 76 μm, a filtration efficiency of 63%, and a filtration resistance of 44 Pa. Example 4
[0032] Raw materials and equipment: Jiangsu Jiahe JH830 foaming furnace, coating scraper JLTD20×120×2000, Kuntai industrial grade superior basic zinc carbonate; Dongzhi Huaertai industrial hydrogen peroxide; Yoshida 803L phenolic resin emulsion.
[0033] The production method of in-situ synthesized zinc oxide-containing emulsion foaming material comprises the following steps:
[0034] The first step is to prepare basic zinc carbonate and add it to water to form basic zinc carbonate paste, and the mass fraction of the basic zinc carbonate paste is 60%; the second step is to mix the basic zinc carbonate paste with the phenolic resin emulsion with a mass concentration of 35% of the hydrogen peroxide solution, and add the hydrogen peroxide solution, the mass ratio of the basic zinc carbonate paste, the phenolic resin emulsion and the hydrogen peroxide solution is 5:2:7, and the basic zinc carbonate paste foaming emulsion is obtained, and the foam density of the basic zinc carbonate paste foaming emulsion is 550g / L; the third step is to fill the basic zinc carbonate paste foaming emulsion evenly in the mold cavity to obtain the foamable material; the fourth step is heat treatment foaming: the foaming coating obtained in the previous step is heated to 150°C for 15min for cross-linking and foaming; after foaming, it is cooled to room temperature to obtain the in-situ synthesized zinc oxide emulsion foaming material.
[0035] Product performance: density 72.3kg / m 3 ; Compression strength 0.15MPa; Thermal conductivity 0.035W / m·k; Dimensional stability 1.38%; Water vapor permeability 3.5 (Ng / (Pa·m·s)); Water absorption (volume fraction) 5.5%; Combustion performance oxygen index 40%; Combustion classification B1.
[0036] Note: The density shall be determined according to the method specified in GB / T6343. The compression strength shall be determined according to the method specified in GB / T8813. The thermal conductivity shall be determined according to the provisions of GB / T10294. The dimensional stability shall be determined according to the method specified in GB / T8811. The temperature is 70℃, and the time is 48h; the dimensional stability result is the average value of the absolute value of the dimensional change rate in each direction. The water vapor permeability coefficient shall be determined according to the provisions of QB / T2411-1998, with a sample thickness of 25mm, a temperature of 23℃, a relative humidity gradient of 50%, Δp=1404.4Pa, and 5 samples. The water absorption rate shall be determined according to the method specified in GB / T 8810. The oxygen index of the combustion performance shall be determined according to the method specified in GB / T 2406. The combustion classification shall be determined according to the method specified in GB 8624-2012.
Claims
1. A method for producing an in-situ synthesized zinc oxide-containing emulsion foaming material, characterized in that: The following steps are involved: The first step is to prepare basic zinc carbonate and add it to water to form basic zinc carbonate paste, wherein the mass fraction of the basic zinc carbonate paste is 50% to 60%; the second step is to mix the basic zinc carbonate paste with a polymer emulsion, and add a hydrogen peroxide solution to obtain a basic zinc carbonate paste foaming emulsion, wherein the polymer emulsion is one of a natural rubber emulsion, a phenolic resin emulsion, and a polytetrafluoroethylene emulsion, and the mass ratio of the basic zinc carbonate paste, the polymer emulsion, and the hydrogen peroxide solution is 3 to 5:1 to 2:6 to 7, the mass concentration of the hydrogen peroxide solution is 33% to 35%, and the foam density of the basic zinc carbonate paste foaming emulsion is 350 to 5 50g / L; the third step, evenly scraping the basic zinc carbonate foaming emulsion on the stainless steel belt to form a foaming layer; or adding the basic zinc carbonate paste foaming emulsion into the mold, so that the basic zinc carbonate paste foaming emulsion is evenly filled in the mold cavity to obtain expandable material; or the basic zinc carbonate paste foaming emulsion is coated on the continuous fabric by a foaming coating process to form a foaming coating; the fourth step, heat treatment foaming: heating the foaming layer obtained in the previous step for cross-linking foaming; or heating the foaming coating obtained in the previous step for cross-linking foaming; or heating the expandable material obtained in the previous step for cross-linking foaming; cooling to room temperature after foaming to obtain the in-situ synthesized zinc oxide emulsion foaming material.
2. The method for producing an in-situ synthesized zinc oxide-containing emulsion foaming material according to claim 1, characterized in that: The uniform coating amount on the stainless steel belt is 400g / m 2 .
3. The method for producing an in-situ synthesized zinc oxide-containing emulsion foaming material according to claim 1, characterized in that: The continuous fabric is polyester non-woven fabric or polyimide non-woven fabric.
4. The method for producing an in-situ synthesized zinc oxide-containing emulsion foaming material according to claim 1, characterized in that: The foaming coating process is a scraping amount of 150 to 190 g / m 2 , and then pre-bake at 80-90°C for 60-120s.