Additive manufacturing support materials

By using a condensed phase separation method to manufacture uniform gel particles and embed them in fluid ink, the problem of low efficiency in traditional mechanical blending technology is solved, enabling high-fidelity additive manufacturing printing and improving the quality of printed structures.

CN117205850BActive Publication Date: 2026-11-10CARNEGIE MELLON UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310921092.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-09-28
Filing Date
2018-04-05
Publication Date
2026-11-10
Estimated Expiration
2038-04-05

AI Technical Summary

Technical Problem

The traditional mechanical blending technology for existing additive manufacturing support materials is inefficient and has low yield, resulting in defects, voids and irregularities in the printed structure, making it difficult to achieve high-fidelity printing.

Method used

The support material is manufactured using a condensed phase separation method. By forming uniform gel particles and embedding them in fluid ink, phase separation is used to drive the formation of gel particles. Combined with stirring and centrifugation techniques, the particle morphology and rheological behavior are controlled to form a support material with a specific yield stress.

Benefits of technology

It enables high-yield, low-cost, large-scale manufacturing of uniform support materials, improves the fidelity of printed structures, reduces defects and irregularities, and enhances printing accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117205850B_ABST
    Figure CN117205850B_ABST
Patent Text Reader

Abstract

This invention relates to additive manufacturing support materials. This document describes a method for manufacturing gel microparticles with consistent size and morphology. Large quantities of gel microparticle slurry can be manufactured by increasing the reactor size through agglomeration. The particles can be repeatedly dehydrated and rehydrated according to their environment, allowing the particles to be stored in non-solvents such as ethanol. The gel slurry exhibits Bingham plastic behavior, where the slurry behaves as a solid below a critical shear stress. Upon reaching the critical shear stress, the slurry experiences a rapid decrease in viscosity and behaves as a liquid. The rheological behavior of these slurries can be tuned by altering the yield stress through changes in the compaction method, such as centrifugal force. The narrower particle distribution and reduced size allow for increased fidelity in fresh printing.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the application filed on April 5, 2018, with application number 201880037168.6 and invention title "Additive Manufacturing Support Material".

[0002] Priority Statement

[0003] This application claims priority to U.S. Patent Application Serial No. 62 / 601,949, filed April 5, 2017, and U.S. Patent Application Serial No. 62 / 606,578, filed September 28, 2017, the entire contents of which are incorporated herein by reference.

[0004] Government support terms

[0005] This invention was developed with government support from the National Institutes of Health (NIH) No. HL117750. The government holds specific rights to this invention. Technical Field

[0006] This application relates to additive manufacturing, and more specifically to a support material for additive manufacturing. Background Technology

[0007] Additive manufacturing can be used to create three-dimensional objects or structures. Material can be printed into support frames that temporarily support the structure during assembly. Once assembly is complete, the support frames are removed. Summary of the Invention

[0008] This application describes a support material for additive manufacturing and a method for manufacturing the same. A method for additive manufacturing fluids, called a free and reversible embedding (FRESH) of a suspended hydrogel, involves embedding a fluid material (e.g., alginate, collagen, fibrous protein, etc.) into a short-lived support material (e.g., comprising a microparticle slurry). The support material and its manufacturing method described below overcome the limitations imposed by conventional mechanical blending techniques for manufacturing support materials. The support material described below comprises microparticles having approximately uniform size and uniform geometry. For additive manufacturing methods (e.g., embedded printing in a support material), the support material enables the production of printed structures with higher fidelity (e.g., fewer defects, fewer voids, fewer irregularities, etc.) than existing versions using the support material.

[0009] The methods for providing support materials described below are more efficient than existing methods for producing polymeric microgels and nanogels for drug encapsulation and / or delivery using basic chemical principles of emulsification or coagulation. Existing methods may include blending and emulsification. These existing methods are less efficient, have lower yields, produce small-volume particles, and rely on chemicals and polymers that are less suitable for bioprinting.

[0010] This paper describes a method for producing a support material containing microparticles that overcomes the limitations of conventional mechanical blending techniques used to produce particles for support materials. By using a stretchable phase separation called coagulation, a large number of monodisperse microparticles can be manufactured from a variety of pristine, reversible gelling materials, with strict control over particle morphology and bulk rheological behavior. Phase separation is used to drive the formation of gel particles. These particles can then be further separated to form the support material. By embedding a gelling fluid “ink” within this support material, the ink is allowed to fuse into three-dimensional objects.

[0011] These methods rely on dissolving a gel in a mixture of a solvent (such as water) and a co-solvent (such as ethanol) under stirring. By changing the mixing conditions, the solubility of the gel decreases until gel particles nucleate from the solution. These particles can then be washed and separated to form a support material slurry.

[0012] This method produces gel microparticles in a simple, one-step, high-yield, and inexpensive manner. Due to its chemically driven nature, it is also easily scalable to large volumes, which is difficult for other methods that rely on mechanical blending, emulsification, or ultracentrifugation. This method allows for the large-scale fabrication of support materials, enabling the rapid adoption of 3D-printed gel fluids.

[0013] The support material includes a slurry comprising a solution and aggregated particles in the solution, the aggregated particles having a substantially uniform geometry; wherein at least a portion of the slurry forms a rigid body when subjected to stress below a threshold stress; and wherein at least a portion of the slurry forms a viscous fluid when subjected to stress above a threshold stress.

[0014] In some embodiments, the solution contains a surfactant configured to reduce the number of dendritic aggregate particles formed in the surfactant-containing solution relative to the number formed in a surfactant-free solution. In some embodiments, each of the aggregate particles contains at least one of gelatin, alginate, and cellulose. In some embodiments, the aggregate particles contain two or more different polymers. In some embodiments, one of the two or more different polymers contains gum arabic, and another of the two or more different polymers contains gelatin. In some embodiments, the solution contains one or more of water and ethanol.

[0015] In some embodiments, the blended average size of the aggregated particles is between about 0.5 μm and about 60 μm. In some embodiments, the blended average size variation of the aggregated particles is less than about 35%.

[0016] In some embodiments, the threshold stress includes a critical shear stress, wherein the cohesive force between the first and second aggregate particles of the slurry is approximately equal to the external shear force applied to the aggregate particles of the slurry. In some embodiments, the value of the critical shear stress is between about 20 Pa and about 140 Pa. The value of the critical shear stress is based on the viscosity of the additive manufacturing ink in the slurry. In some embodiments, the ink contains collagen.

[0017] This document describes a method for manufacturing the support material, the method comprising generating aggregates from a polymer, the aggregates comprising particles with substantially uniform geometry, wherein generating the aggregates comprises: forming a solution of a solvent and a co-solvent; stirring the solution and dissolving the polymer in the solution; adjusting the pH of the solution to a specific value based on the type of polymer; and forming a slurry from the aggregates having a specific yield stress value, the forming comprising compacting the aggregates during one or more centrifugal cycles.

[0018] In some embodiments, the method includes selecting one or more parameters and adjusting one or more parameters during the generation of the aggregates, each of the one or more parameters including: gelatin Bloom value, polymer processing method, polymer precipitation rate, polymer solubility, polymer molecular weight, polymer concentration, volume ratio of solvent and co-solvent, surfactant type, surfactant concentration, cooling rate, or stirring rate.

[0019] In some embodiments, the method includes selecting one or more parameters; and adjusting one or more parameters during the formation of the slurry, the one or more parameters including: the type of washing solution, the centrifugation time of the one or more centrifugation cycles, the centrifugation force of the one or more centrifugation cycles, and the number of the one or more centrifugation cycles.

[0020] In some embodiments, the polymer is gelatin, having a gelatin Bloom value selected from 200 Bloom, 250 Bloom, and 275 Bloom. The polymer is gelatin, and the gelatin comprises one or both of acid-cured gelatin and lime-cured gelatin. The solution comprises a solvent to co-solvent ratio of approximately 52.5:47.5, wherein the solvent comprises water, and the co-solvent comprises ethanol.

[0021] In some embodiments, the method includes adding a surfactant to the solution. The operation includes dehydrating the slurry in ethanol. In some embodiments, the method includes rehydrating the slurry in water, wherein the slurry maintains the specific yield stress value after dehydration and rehydration.

[0022] In some embodiments, the polymer is a first polymer, and generating the aggregate further includes: adding a second polymer to the solution, selecting the isoelectric point of either the first polymer or the second polymer, and adjusting the pH based on the selected isoelectric point. In some embodiments, the first polymer comprises gelatin, the second polymer comprises gum arabic, and the pH is about 5 to 6.

[0023] In some embodiments, the method includes adjusting the one or more centrifugal cycles to achieve a specific yield stress value for the slurry. In some embodiments, the specific value is between about 20 Pa and about 140 Pa. In some embodiments, the specific value is based on the viscosity of the additive manufacturing ink in the slurry.

[0024] In some embodiments, the ink contains collagen. In some embodiments, the method includes washing the aggregates in a washing solution. In some embodiments, the aggregate particles are approximately monodisperse in the solution.

[0025] In some embodiments, the support material comprises a gelatin slurry containing: a colloidal solution of ethanol and water; a surfactant; and aggregated microparticles in the colloidal solution, the aggregated microparticles being monodisperse in the solution, the aggregated microparticles having an average size between 0.5 and 60 micrometers and a size variation of less than 35%; wherein at least a portion of the slurry forms a rigid body when subjected to shear stress below the yield stress value; and wherein at least a portion of the slurry forms a viscous fluid when subjected to shear stress above the yield stress value.

[0026] Details of more than one embodiment of the support material are depicted in the accompanying drawings and the description below. Other features, objects, and advantages will become apparent from the specification, drawings, and claims. Attached Figure Description

[0027] Figure 1A The printing system is shown.

[0028] Figure 1B This shows the appearance of gelatin particles.

[0029] Figures 2-6 Each example illustrates the manifestation of gelatin microparticles as an exemplary support material.

[0030] Figure 7 A bar chart showing the particle size distribution of an exemplary support material is provided.

[0031] Figure 8 A graph is shown representing the gelatin concentration relative to particle size of an exemplary support material.

[0032] Figures 9-10 Each shows an exemplary support material.

[0033] Figure 11 An example of the hydration process of the supporting material is shown.

[0034] Figures 12A-12B Examples of particle size and yield control of the support material are shown.

[0035] Figures 13-15 Exemplary rheological data for the supporting material are shown.

[0036] Figure 16 The yield stress value of an exemplary support material is shown.

[0037] Figure 17 The stages of an additive manufacturing method using an exemplary support material are shown.

[0038] Figure 18 An exemplary print is shown in an exemplary support material.

[0039] Figure 19 A flowchart illustrating an exemplary method for forming a support material is shown.

[0040] In the various figures, the same reference numerals denote the same elements. Detailed Implementation

[0041] Figure 1A A printing system 100 is shown. The printing system 100 is constructed to print material 110 (e.g., collagen, fibrous protein, etc.) embedded in a support material 130, such as via an injector 120. During printing and while the material is hardening (e.g., gelling), the support material 130 forms a scaffold to support the material 110. When the viscosity and yield stress of the support material 130 are similar to those of the printing material (also called ink), the printing system 100 can print with better accuracy than when the viscosity and yield stress of the support material do not match or are not similar to those of the support material. Furthermore, the support material forming a slurry with smaller particles facilitates high-fidelity printing of structures within the support material via the printing system 100.

[0042] The support material 130 includes a support material for forming a support in the additive manufacturing method. This support material comprises a slurry that supports an embedded material (e.g., ink) used in embedded 3D printing of the structure. The support material temporarily supports the printing ink embedded within it. Once the structure is formed by the printing method, the support material is removed.

[0043] The support material (also called a support bath) exhibits at least some of the properties of Bingham plasmons. For example, when the support material is not subjected to stress above its yield stress (e.g., shear stress), it exhibits the properties of a solid material. When a portion of the support material is subjected to stress above its yield stress (e.g., shear stress), at least a portion of the support material behaves as a viscous liquid. In some embodiments, the printer injector applies stress to the support material as it moves through it. This allows the printhead to inject ink into the support material, which supports the ink in place until the structure is formed. The ink may include tissues such as collagen or other materials such as materials that undergo gelation after being injected into the support material. The support material supports the ink until gelation is complete. The support material can then be removed (e.g., melted away).

[0044] The yield stress of the support material is a crucial factor enabling precise shape printing. The uniformity of the support material also affects the quality of the printed structure. The support materials described herein can have a yield stress set to a specific value (e.g., based on the application, ink type, etc.). The support materials described herein comprise particles of a specific size, designed to improve print fidelity and enable precise 3D embedded printing of structures.

[0045] Figure 1B An example of a gelatin support material 150 manufactured using a blending technique is shown. This example illustrates the production of a gelatin microparticle support using the mechanical blending of gelatin blocks to create smaller gelatin particles. Due to the nature of the blending method, the manufactured gelatin microparticles are random in both their size and shape distribution. Support material 150 shows particles with irregular sizes and shapes. These particles are not uniformly dispersed in the support bath slurry. For embedded printing applications, approximately uniform particle size, shape, and dispersion are preferred. The support material and the method of manufacturing the support material described below overcome or reduce the limitations imposed by conventional mechanical blending techniques for manufacturing support materials. The support material described below comprises microparticles with approximately uniform size and uniform geometry. For additive manufacturing methods (e.g., embedded printing in the support material), the support material enables the production of printed structures with higher fidelity (e.g., fewer defects, fewer voids, fewer irregularities, etc.) than printed structures using existing versions of the support material. Figure 1B As shown, gelatin microparticles 150 manufactured by mechanical blending exhibit a random size and shape distribution. The scale bar is 50 micrometers.

[0046] Figures 2-6 The illustrations show the forms of exemplary support materials 200, 300, 400, 500, and 600 manufactured by a cohesive method. (Relative to...) Figure 1BThe support material 150 shown is manufactured by mechanical blending, while the particles manufactured by agglomeration are smaller and more uniform in morphology.

[0047] The substrate forming the particles of the support material comprises a polymer. This polymer may include one or more of gelatin, alginate, cellulose, and similar polymers. The substrate undergoes an aggregation process to produce an aggregate containing the material. The aggregate comprises particles of material with a substantially uniform geometry. Particles having a substantially uniform geometry have substantially the same shape, size, structure, and arrangement, particularly uniformity between particles. For example, the particles have a substantially uniform size. Here, substantially uniform size means that the particles (e.g., droplets) exhibit a particle size distribution having a coefficient of variation (i.e., the standard deviation of the population divided by the population mean) of less than about 35% or about 10, 15, 20, 25, or about 30%. A coefficient of variation of less than about 15% is preferred. In some embodiments, about 70% or about 90% of the beads have a volumetric particle size of about 0.90 to about 1.1 times the average volumetric particle size. In some embodiments, the particles are monodisperse in the aggregate.

[0048] Agglomerated support synthesis scheme for forming support materials for embedded printing applications includes material agglomeration and material compaction. Parameters of the support material can be selected based on the specific application of the support material (e.g., based on the ink used in the embedded printing method). These parameters (size, yield, etc.) affect the yield stress of the support material. The yield stress of the support material is based on the size of the particles produced during the agglomeration process and can be adjusted to a specific value. Properties of the substrate (e.g., polymer) can be selected and / or adjusted to adjust the size of the agglomerated particles, thereby adjusting the yield stress of the support material. These properties may include the type of substrate, the material processing method, the polymer precipitation rate (e.g., during agglomeration), polymer solubility, the molecular weight of the material, the polymer concentration, the volume ratio of the solution (e.g., solvent relative to co-solvent), the type of surfactant, the surfactant concentration, the cooling rate, and the stirring rate.

[0049] The aggregation of the support material is carried out according to the following exemplary method. An ethanol-water solution is prepared. The substrate to be used (e.g., gelatin, alginate, cellulose, etc.) is measured. The amount of this material dissolved in the solution can be set to change the particle size and yield of the support material. Heating and cooling rates can affect the precipitation rate of the polymer into the solution, which will affect the particle size. The mixing rate also affects the particle size, as described in further detail below. For example, a faster mixing rate results in a smaller average size of the precipitated particles. As mentioned above, the particle size can be measured as a harmonized average size. While dissolving the substrate (e.g., the polymer), a surfactant can be added and dissolved in the solution. Once the polymer is dissolved, the pH of the solution can be lowered (e.g., by adding an acid) until the isoelectric point of the polymer is reached, and the polymer begins to precipitate into the solution. The solution is stirred until the polymer precipitation is complete or substantially complete, causing the solution to aggregate.

[0050] The aggregate solution is compacted to form a support material. The aggregate solution is placed in a centrifuge. The number of centrifugation cycles, duration, speed (e.g., RPM setting), and other centrifugation settings are based on the desired yield stress of the support material, the amount of aggregate, the polymer used, etc. After compaction, the aggregate is washed in a washing solution. The type of washing solution used may depend on the material to be printed in the support material (e.g., collagen, alginate, etc.).

[0051] The following is an exemplary method for preparing the support material. A solution is prepared by measuring a 50:50 ethanol-water solution. The ethanol to water ratio can be adjusted to regulate the particle size of the support material. For example, this ratio can include 47.5:52.5 ethanol and water, or a similar ratio. For example, 500 mL of deionized (DI) water and 500 mL of 200 standard anhydrous ethanol (EtOH) can be used for a 50:50 ratio. For gelatin-based support materials, 20 g of type B gelatin (2 wt%) and 2.5 g of F127 pluronic (0.25 wt%) surfactant are measured. 500 mL of DI water is heated to 45°C. The warm water is mixed into the EtOH container. While stirring, the gelatin and pluronic powder are slowly added. Sufficient time (e.g., about ten minutes) allows the gelatin and pluronic powder to completely dissolve in the solution. While stirring, the pH of the solution is adjusted to 5.6–5.7 with an acid (e.g., 1 M HCl). The turbidity of the solution indicates coagulation. At this stage, increase the stirring speed to at least 500 RPM. The stirring speed should be high enough to avoid drawing air bubbles into the solution.

[0052] The following are exemplary steps for preparing the support material. Place the “raw” aggregate solution in a centrifuge. For example, the support material can be placed in a centrifuge tube and centrifuged at 175 G for approximately 2 minutes. Remove the supernatant. Yellowish-white pellets of gelatin remain at the bottom of the tube and are refilled with the raw aggregate solution. Break up any loose pellets (e.g., by shaking the container). Centrifuge the solution at 175 G for, for example, two minutes. Remove the supernatant. Add DI to the gelatin in a 2:1 ratio. Disperse the pellets to break up any clumps. Centrifuge the solution at 225 G for, for example, two minutes. Remove the supernatant and replace it with 1X PBS containing 25 mM HEPES solution. Centrifuge the solution at 450 G for, for example, two minutes. The solution forms a gelatin slurry, which should begin to swell as it becomes more neutral through washing. The swelling ratio can be up to 3:1.

[0053] In some embodiments, if printing alginate, the supernatant is replaced with DI water. The solution is centrifuged at 450G for, for example, two minutes. The supernatant is removed and washing solution is added. For alginate printing, the washing solution may include 0.16 wt% CaCl2. Other washing solutions can be used for fibrin and collagen printing. In some embodiments, the slurry may be refrigerated. In some embodiments, additional centrifugation may be performed, for example, at 450G for two minutes. In some embodiments, a vacuum chamber may be used for 20–30 minutes. In some embodiments, additional centrifugation may be performed, for example, at 750G for five minutes. The supernatant is then removed.

[0054] Figure 2 An example of gelatin microparticles 200 formed by the above-described coagulation method is shown. The scale bar is 100 micrometers. Figure 3 An example of gelatin microparticles 300 formed by the above-described agglomeration method is shown. The scale bar is 25 micrometers. The microparticles have substantially the same geometry, including size, shape, etc.

[0055] The method of gelatin coagulation can be further modified by adding other charged polymers to the coagulated solution; otherwise, it is called complex coagulation. In simple coagulated polymers with a single amphoteric polyelectrolyte polymer, the polymer's own charge is completely neutralized at its isoelectric point. In complex coagulated polymers, the charges between the two individual polymers recombine.

[0056] For example, Figure 4 An example of gelatin microparticles 400 formed through composite coagulation is shown. The addition of gum arabic allows for composite coagulation between the two polymers, resulting in microparticles with very consistent size, morphology, and individuality. Gelatin carries a more positive charge in acidic solutions, while gum arabic carries a negative charge in any solution with a pH > 2.2–3. Thus, these two polymers are optimal for composite coagulation and can coagulate close to the isoelectric point of gelatin. Figure 4 The gelatin microparticles shown are produced by the composite coagulation of 2.0 wt% gelatin B and 0.1 wt% gum arabic. The scale bar is 50 micrometers.

[0057] As mentioned above Figure 2 The stirring rate affects the size of gelatin particles formed by applying higher shear forces to the particles during particle formation. Higher shear forces disrupt the formation of gelatin particles above a critical size by making larger particles less stable. Therefore, higher stirring rates produce smaller particles. Stirring at nearly four times the standard speed (e.g., 100 RPM) produces particles smaller than one-third of their original size. Rapidly stirred aggregates reduced the average particle size from 42.85 ± 13.89 μm to 13.66 ± 4.41 μm. This shows a particle size variation of less than 35%.

[0058] Figure 5 An example of the formation of smaller gelatin particles 500 is shown compared to gelatin particles 200, 300, and 400.

[0059] Changing other chemical parameters, such as the solvent / non-solvent ratio, can also be used to control particle size. The initial coagulation method used a water-ethanol ratio of 50:50. Changing the water-ethanol ratio to 52.5:47.5 resulted in a reduction in particle size of 6.42 ± 1.68 μm and a narrower size distribution.

[0060] For example, Figure 6 The image shows 600 gelatin particles made from water and ethanol in a ratio of 52.5:47.5. The scale bar is 100 micrometers. Other ratios of water and ethanol can be used, such as 60:40, 55:45, 50:50, etc. Figure 7 The bar chart shows the particle size distribution. The blended gelatin particles (labeled as blended) show a broad particle size distribution. Particles from a 50:50 water and ethanol coagulation (labeled as coagulates) show a narrower distribution of smaller particles. A 52.5:47.2 water and ethanol coagulation (labeled as modified coagulates) exhibits an even narrower size distribution of smaller particles (e.g., less than about 10 micrometers in diameter).

[0061] When using the same manufacturing conditions, the average particle size remains consistent across different weight percentages of gelatin. Provided the critical manufacturing conditions remain consistent, increasing the weight percentage of gelatin increases the overall yield of particles from the coagulation method, not their morphology. Figure 8Image 800 is shown. Image 800 illustrates that increasing the concentration of gelatin in the agglomerates has no significant effect on particle size (<10 micrometers). Several manufacturing conditions affecting particle size include the Bloom concentration of the gelatin and the processing method (e.g., acid curing, lime curing, etc.), the pH of the agglomeration solution, the volume ratio of water to ethanol, the use of the surfactant (F127 Pluronic), the cooling rate of the agglomerates, and the stirring rate of the agglomerates. By controlling these conditions of the agglomeration solution, the solubility of the gelatin (and the particle geometry) is thus controlled. The formation of agglomerates is highly dependent on controlling the solubility of gelatin between the fluid and gel phases after it has dissolved in the solution. Subsequent reduction of gelatin solubility prevents the formation of a single gelatin matrix, but rather the formation of gelatin particles as solubility continues to decrease.

[0062] The Bloom strength of gelatin depends on the average molecular weight of the gelatin molecules. Higher molecular weight gelatin is less soluble in water-ethanol solutions than its lower molecular weight counterparts and is therefore more likely to precipitate from the solution. As the system cools and the solubility of gelatin decreases, gelatin molecules precipitate from the solution in order of their molecular weight, starting with the highest molecular weight. High Bloom gelatin, with its higher average molecular weight compared to lower molecular weight gelatin, will therefore precipitate from the solution at different time points, thus affecting the time and temperature at which stable particles form.

[0063] Animal tissues treated with acid or alkali produce acidic (A) or basic (B) gelatin, respectively. These gelatins have different isoelectric points, resulting in varying solubilities at specific pH values. Adjusting the pH of the solution to the isoelectric point (pI) of the molecule represents the minimum solubility. At the isoelectric point, gelatin molecules undergo successive charge neutralization with their own charged residues and those residues of other gelatin molecules, causing the molecules to fold and detach from the solution. Thus, the pH of the coagulation solution also affects the solubility of gelatin and the formation of particles.

[0064] Gelatin is soluble in water and practically insoluble in organic solvents such as alcohols. If gelatin is first dissolved in water at a temperature above its melting point and then cooled, it forms a continuous gel. In a coagulation solution with a mixture of approximately 50:50 ethanol and water, gelatin becomes less soluble as the temperature of the coagulation solution decreases and as the binding of alcohol and water strengthens. Therefore, due to its insolubility in alcohol, gelatin cannot form a continuous matrix in an aqueous-ethanol solution at lower temperatures. Controlling the water-to-ethanol ratio in the coagulation solution significantly affects the solubility of gelatin when agglomerates form.

[0065] The use of surfactants (e.g., F127 Pluronic) prevents the formation of agglomerates in gelatin particles. Without surfactants, gelatin particles tend to adhere to each other, forming large, coarse, dendritic agglomerates, such as... Figure 9The particle shown is 900. The use of surfactants prevents or reduces the formation of these dendritic particles, resulting in smooth, round particles, such as... Figures 2-6 Particle sizes are 200, 300, 400, 500, and 600. Figure 9 This illustrates the formation of large dendritic particles due to the absence of surfactant. The scale bar is 100 micrometers.

[0066] Rapid cooling of the agglomerated solution rapidly reduces the solubility of gelatin. Rapid cooling of the solution (e.g., faster than 1°C / min) causes the gelatin to precipitate out of the solution more quickly. If the gelatin precipitates out of the solution too quickly, it cannot slowly adhere to existing gelatin particles, resulting in rapid accumulation of gelatin on individual particles and the formation of coarse, dendritic particles. Figure 10 The image shows particle size 1000. (Compared to...) Figures 2-6 Compared to the larger particles, particles 1000 are large and irregularly dendritic. Particles 1000 are formed by rapidly cooling the aggregate solution with ice. The scale bar is 100 micrometers.

[0067] Controlled hydration

[0068] Figure 11 An exemplary process 1100 for controlling particle hydration is shown. Particle hydration can be operated by the composition of the solution of the supporting material. Gelatin particles are hydrated according to osmotic pressure and pH. Utilizing the same dehydration principle in their formation, gelatin particles derived from aggregates can be dehydrated by transferring them from water (as shown in particle 1110) to ethanol (as shown in particle 1120). The hydrophilic gelatin particles 1120 aggregate together to reduce their surface energy. Since gelatin is insoluble in ethanol, particles 1120 can be stored in a dehydrated state and cannot melt into the solution. Storing particles 1120 in ethanol also allows for storage below 0°C without the risk of ice crystal formation in the supporting material. Transferring the gelatin slurry back to water rehydrates particles 1130 and allows particles 1130 to dissociate from each other. The dehydration / hydration process is repeatable and allows gelatin particles derived from aggregates to be stored in a dehydrated state for extended periods, which can be easily reversed to the initial state.

[0069] Figure 12AExamples of gelatin-supported material particles formed using different pH values ​​and different gum arabic concentrations are shown. For each example, the scale bar is 50 micrometers. Particle 1200 was formed using a solution of gum arabic at pH 6 and a concentration of 0.1%. Particle 1210 was formed using a solution of gum arabic at pH 6.5 and a concentration of 0.1%. Particle 1220 was formed using a solution of gum arabic at pH 7 and a concentration of 0.1%. Particle 1230 was formed using a solution of gum arabic at pH 6.5 and a concentration of 0.1%. Particle 1240 was formed using a solution of gum arabic at pH 6.5 and a concentration of 0.25%. Particle 1250 was formed using a solution of gum arabic at pH 6.5 and a concentration of 0.5%. Particle 1260 was formed using a solution of gum arabic at pH 6.5 and a concentration of 0.75%. Figure 12A It can be seen that the particle size decreases when the pH of the solution deviates from the isoelectric point of gelatin (5-6 pH). From... Figure 12A It can be seen that as the concentration of gum arabic increases, the particle size decreases. This is because the concentration increases the number of nucleation sites, and the same amount of gelatin precipitates from the water / ethanol solution.

[0070] Figure 12B Examples of controlling particle size and yield in a support material are shown. Particle 1270 was formed using a solution of gum arabic at pH 5.5 and a concentration of 0.1%. Particle 1275 was formed using a solution of gum arabic at pH 6.0 and a concentration of 0.1%. Particle 1280 was formed using a solution of gum arabic at pH 6.5 and a concentration of 0.1%. Particle 1285 was formed using a solution of gum arabic at pH 6 and a concentration of 1%. Particle 1290 was formed using a solution of gum arabic at pH 6.5 and a concentration of 1%. Figure 12B As can be seen, pH and gum arabic concentration can be adjusted simultaneously to regulate particle size and slurry yield. pH 6 and 1% gum arabic concentration maintain a particle size of approximately 8–12 μm while producing a relatively larger amount of support material slurry. Comparing the yield of particles of roughly the same size, pH 6 and 1% gum arabic concentration produce approximately 57.15 million particles / mL, while pH 6.5 and 0.1% gum arabic concentration produce approximately 18.98 million particles / mL. If the support material derived from gum arabic includes any fragments, these dense and often large particles can be removed using a brief centrifugation step, and any remaining particles should be washed away before cell seeding.

[0071] rheology

[0072] After compaction, the supporting material particles form a slurry that behaves as a yield stress fluid. Upon applying a critical stress to the slurry, it begins to flow. This behavior can be analyzed using a rheometer to precisely deform the slurry sample and monitor its deformation using parameters such as shear stress and shear rate to calculate viscosity. When the stress is too low to initiate flow, the yield stress fluid exhibits a constant instantaneous viscosity profile. This is because the yield stress fluid behaves as a solid at stresses below the near-yield stress required to initiate flow. Once the critical yield stress is reached, the material rapidly transitions from a solid to a fluid. At this level of applied stress, the material experiences a rapid decrease in viscosity with increasing shear rate, demonstrating a deviation from high instantaneous viscosity. The transition from solid to fluid behavior is initiated by the critical yield stress applied to the material to trigger particle movement. Below the critical shear stress, the cohesive forces between particles are greater than the external shear forces applied to them, resulting in stationary particles and solid-like behavior. Particle movement is initiated at the critical yield stress when the forces applied to the particles overcome the total cohesive forces and the particles begin to slide past each other. When shear stress is maintained above the critical yield stress, the particles will continue to slide past each other and exhibit fluid-like behavior. When the shear stress decreases below the critical yield stress, the particles re-adhere to each other by the same force that initially held them together.

[0073] Figure 13 Image 1300 shows the yield stress characteristics of the support material manufactured from the aforementioned cohesive material. If deformation is allowed for an extended period, the viscosity of the material eventually begins to level off at a much lower viscosity because it reaches its fluid-like viscosity under high shear stress. Viscosity measurement data can be obtained from samples of gelatin microparticle slurries manufactured using the cohesion method described herein. Figure 13 In the diagram, the circle indicates the moment when the critical yield stress is applied, which causes a rapid decrease in the sample viscosity, confirming that the support exhibits shear-thinning behavior.

[0074] The deviation from the continuous region of viscosity can be correlated with the instantaneous shear stress required to induce flow in Bingham plastic fluids. Additional rheological tests, such as amplitude and frequency sweeps, can more accurately determine the yield stress of the linear viscoelastic region (LVR) and non-Newtonian fluids, respectively. The LVR is determined by the linear region of the elastic modulus (G'). The strain from the LVR is then selected for a frequency sweep; for this sample, a frequency sweep of 0.035 is chosen.

[0075] Figure 14 An exemplary image 1400 shows amplitude scan data of a gelatin support material. The linear plateau of the elastic storage modulus (G') represents the LVR, from which the strain used for frequency scanning can be selected. Figure 15An exemplary image 1500 showing frequency scan data of a gelatin support material is provided. The elastic storage modulus (G') and viscosity loss modulus (G”) are measured. The intersection represents the frequency at which the support material yields and transitions from behaving as an elastic solid to a viscous fluid. The intersection thus corresponds to the yield stress of the support material.

[0076] It has been shown that the yield stress of this slurry is variable through a centrifugal compaction step. Higher centrifugal forces force the particles together, thus compacting them. The yield stress of the slurry can be adjusted by changing these centrifugal forces, thereby altering the degree of particle compaction. When higher G-forces further compact the slurry, the yield stress of the slurry increases. This behavior can be seen in various brands of gelatin used to produce particulate slurries via the coagulation method outlined above.

[0077] Figure 16 Image 1600 shows exemplary yield stresses of support materials centrifuged at different speeds or RPMs. The slurry was centrifuged at a final centrifugation speed of "Low" (1100 RPM = 227 G), "Medium" (2000 RPM = 751 G), or "High" (4500 RPM = 3803 G), and their yield stresses were measured using a rheometer. Yield stresses of various brands of gelatin are shown below. Figure 16 As shown, the yield stress of the samples increased with increasing RPM centrifugation speed, regardless of the Bloom value of the gelatin. Controlling the yield stress of the support broadens the range of materials that can be used with the slurry. Adjusting the yield stress of the slurry allows for a wider range of ink compatibility by making the ink viscosity more closely match the viscosity and yield stress of the support. Printing accuracy increases when the ink viscosity is similar to the viscosity and yield stress of the support, compared to the lower accuracy of in-line printing in support materials with different viscosities and yield stresses.

[0078] Improving the fidelity of fresh 3D printing

[0079] Because particles derived from aggregates can form Bingham plastic fluids, they can be used in fresh printing. One limitation to extrusion accuracy and precision in fresh printing is the size and shape distribution of the particles in the sacrificial support bath. Irregular particle sizes and shapes (such as...) Figure 1B The particles prevent consistent extrusion and result in lower print fidelity. When the support material is removed, the particles act as pore-forming agents, leaving voids and defects in the print. Figure 17 Image 1710).

[0080] Because gelatin particles derived from aggregates are smaller and more uniform in size and shape compared to gelatin particles manufactured using existing technologies (e.g., blending, emulsification, etc.), extrusion accuracy and precision are improved, and void defects in printing are reduced. This results in a significant improvement in print fidelity. To illustrate this, the "window frame" model was sliced ​​and guided using standard 3D printing software.

[0081] Figure 17 Examples of high print fidelity using the support material described herein are shown, compared to the lower print fidelity of existing support materials. Image 1700 shows a model of a 3D printed mesh. Collagen ink was used, and the model was then printed in a blended support bath as shown in Image 1710 and a gelatin particle bath derived from aggregates as shown in Image 1720. Confocal images of the labeled collagen ink highlight the increased feature resolution of the collagen printed in the aggregate support in Image 1740, compared to the collagen printed in the blended support bath in Image 1730. The collagen structure printed in the aggregate support material has fewer voids and a more regular structure compared to the collagen structure printed in the blended support material.

[0082] Because of the condensation into a stretchable chemical process, large quantities of gelatin supports can be produced more efficiently than with mechanical blending. This allows for the manufacture of larger fresh prints more quickly and with less labor. Large prints (e.g., structures) still benefit from the ability to... Figure 17 The improved fidelity of FRESH printing at the sub-millimeter level is shown. The result is the ability to print objects on a macroscopic scale with higher fidelity than before.

[0083] Figure 18 An example of a high-fidelity structure printed using the support material described herein is shown. An adult heart model obtained from patient-specific MRI data was converted into a 3D printable format, as shown in image 1800. This heart model was then fresh-printed in a scaled-down form, producing pure, unmodified bovine collagen, such as... Figure 18 As shown in image 1810.

[0084] Figure 19 A flowchart 1900 illustrates an exemplary method for manufacturing a support material. A solution with a specific solvent and co-solvent ratio and a specific pH is formed (1910). After selecting a polymer (e.g., gelatin, alginate, fibroin, etc.), the polymer is dissolved in the solution at a specific rate (1920). The pH is adjusted based on the type of polymer to precipitate aggregates from the polymer (1930). The aggregates are compacted during more than one centrifugal cycle (1940). The aggregates are washed in a washing solution selected based on the type of polymer in the aggregates (1950).

[0085] Several embodiments have been described. However, it should be understood that various modifications may be made without departing from the spirit and scope of the claims. Therefore, other embodiments are also within the scope of the appended claims.

Claims

1. A support material for additive manufacturing, the support material comprising: Slurry, the slurry comprising: Solution; and The aggregated particles in the solution, wherein the harmonic mean size of the aggregated particles is between 0.5 µm and 60 µm and the aggregated particles exhibit a particle size distribution with a coefficient of variation of less than 35%. When subjected to stress below a threshold stress, at least a portion of the slurry forms a rigid body; and When subjected to stress exceeding a threshold stress, at least a portion of the slurry forms a viscous fluid.

2. The support material of claim 1, wherein the solution comprises a surfactant, the surfactant being configured to reduce the number of dendritic aggregate particles formed in the solution containing the surfactant relative to the number of dendritic aggregate particles formed in a solution without a surfactant.

3. The support material according to claim 1, wherein each of the aggregate particles comprises at least one of gelatin, alginate and cellulose.

4. The support material according to claim 1, wherein the aggregate particles comprise two or more different polymers.

5. The support material according to claim 4, wherein one of the two or more different polymers comprises gum arabic, and wherein another of the two or more different polymers comprises gelatin.

6. The support material according to claim 1, wherein the solution comprises water as a solvent and ethanol as a co-solvent, and wherein the solution comprises the solvent and the co-solvent in a ratio of 52.5:47.5, 50:50, 60:40, or 55:

45.

7. The support material according to claim 1, wherein the threshold stress includes the critical shear stress, and when the external shear force reaches the critical shear stress, the cohesive force between the first aggregate particles and the second aggregate particles of the slurry is equal to the external shear force applied to the aggregate particles of the slurry.

8. The support material according to claim 7, wherein the value of the critical shear stress is between 20 Pa and 140 Pa.

9. The support material according to claim 7, wherein the value of the critical shear stress is based on the viscosity of the additive manufacturing ink in the slurry.

10. The support material of claim 9, wherein the ink comprises collagen.

11. The support material according to claim 9, wherein the aggregated particles are monodisperse in the solution.

12. A method for forming a support material for additive manufacturing, the method comprising: Agglomerates are generated from a polymer, the agglomerates comprising particles with substantially uniform geometry, wherein generating the agglomerates includes: A solution that forms a solvent and a co-solvent; The solution is stirred and the polymer is dissolved in the solution to form particles with a substantially uniform geometry; and The agglomerates are formed into a slurry with a specific yield stress value, the formation of which includes compacting the agglomerates during one or more centrifugal cycles. The particles have a harmonic average size between 0.5µm and 60µm and exhibit a particle size distribution with a coefficient of variation of less than 35%.

13. The method of claim 12, further comprising: Select one or more parameters, and During the generation of the agglomerate, one or more parameters are adjusted, each of the one or more parameters including: Gelatin Bloom value, polymer processing method, polymer precipitation rate, polymer solubility, polymer molecular weight, polymer concentration, volume ratio of solvent and co-solvent, type of surfactant, surfactant concentration, cooling rate, or stirring rate.

14. The method of claim 12, further comprising: Select one or more parameters; and During the formation of the slurry, one or more parameters are adjusted, including: The type of washing solution, the centrifugation time of the one or more centrifugation cycles, the centrifugation force of the one or more centrifugation cycles, and the number of the one or more centrifugation cycles.

15. The method of claim 14, further comprising adding a surfactant to the solution.

16. The method of claim 14, further comprising dehydrating the slurry in ethanol.

17. The method of claim 16, further comprising rehydrating the slurry in water, wherein the slurry maintains the specific yield stress value after dehydration and rehydration.

18. The method of claim 12, wherein the polymer is a first polymer, and wherein generating the aggregate further comprises: Add a second polymer to the solution. Select the isoelectric point of either the first polymer or the second polymer, and pH is adjusted based on the selected isoelectric point.

19. The method of claim 12, further comprising adjusting the one or more centrifugal cycles to give the slurry a specific yield stress value.

Citation Information

Patent Citations

  • Additive manufacturing of embedded materials

    US20160167312A1