A dimethyl disulfide gas sensor and its preparation method
By using copper-iron oxide CuGaO2 nanoparticles as the gas-sensitive material, the problems of high temperature, humidity interference, and poor selectivity of existing dimethyl disulfide sensors are solved, and high sensitivity and selectivity of dimethyl disulfide gas detection are achieved.
Patent Information
- Application Number
- CN202311221561.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-09-21
AI Technical Summary
Existing semiconductor dimethyl disulfide sensors have drawbacks such as high operating temperature, susceptibility to humidity interference, and poor gas selectivity.
The copper-iron oxide CuGaO2 nanoparticles are used as gas-sensitive materials. The preparation method includes dissolving copper and gallium nitrates in deionized water to form a transparent and clear solution, adjusting the pH value, adding ethylene glycol and reacting at high temperature, washing and dispersing in anhydrous ethanol, coating on a substrate, and setting Pt or Au test electrodes and heating electrodes.
It achieves a high-sensitivity response to dimethyl disulfide gas, with good selectivity, strong resistance to humidity interference, and can operate at low temperatures. It is suitable for rapid detection of dimethyl disulfide gas in various mixed gas environments.
Smart Images

Figure CN117309952B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of gas sensor technology, specifically relating to a dimethyl disulfide gas sensor using spinel-structured oxide CuGaO2 as the sensitive material and its preparation method. Background Technology
[0002] Dimethyl disulfide (DMD) is a toxic gas or liquid with an unpleasant odor that irritates the eyes, skin, and respiratory tract. Inhaling excessive amounts can cause dizziness or suffocation. It primarily originates from the decomposition of sulfur-containing substances (such as proteins) and emissions from industrial processes in paper mills, tanneries, and other similar facilities. According to the "Odor Pollutant Emission Standard (GB14554-1993)," DMD is one of the eight mandatory odorous gases monitored for pollution sources such as municipal sewage, sludge treatment and waste disposal facilities, paper mills, and tanneries, with emission concentrations required to be below 0.42 mg / m³. 3 This corresponds to approximately 110 ppb.
[0003] Based on their detection principles, dimethyl disulfide (DMD) sensors can be mainly divided into two types: semiconductor and electrochemical. Semiconductor DMD sensors offer advantages such as low cost, simple operation, compatibility with semiconductor processes, and ease of miniaturization and integration. The gas-sensing performance of semiconductor DMD sensors primarily depends on the gas-sensing material. Currently, commercially available semiconductor DMD sensors suffer from drawbacks such as high operating temperature, susceptibility to humidity interference, and poor gas selectivity. Summary of the Invention
[0004] One objective of this invention is to provide a dimethyl disulfide (DMD) gas sensor that exhibits high sensitivity to DMD, good selectivity, low operating temperature, and strong resistance to humidity interference. This overcomes the shortcomings of existing DMD sensors, such as high operating temperature, susceptibility to humidity interference, and poor gas selectivity.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: a dimethyl disulfide gas sensor, comprising a substrate, a gas-sensitive material uniformly coated on the surface of the substrate, a Pt or Au test electrode disposed on the surface of the substrate, and a heating electrode, wherein the substrate is an Al2O3 substrate, and the gas-sensitive material is CuGaO2 nanoparticles with a copper-iron oxide structure.
[0006] As a further improvement to the dimethyl disulfide gas sensor:
[0007] Preferably, the thickness of the gas-sensitive material is 500nm-20μm.
[0008] Preferably, the CuGaO2 nanoparticles have a particle size of 10 nm to 10 μm.
[0009] Preferably, the CuGaO2 nanoparticles are prepared as follows:
[0010] S1. Weigh out copper nitrate trihydrate Cu(NO3)3·3H2O and gallium nitrate Ga(NO3)2·xH2O in a molar ratio of (0.7-1.5):1, and dissolve them in deionized water in sequence to obtain a transparent and clear CuGaO2 precursor solution.
[0011] S2. Adjust the pH of the CuGaO2 precursor solution to 3-8 to obtain a blue suspension;
[0012] S3. Slowly add ethylene glycol to the blue suspension, wherein the molar ratio of ethylene glycol to the sum of the molar amounts of metal ions Cu and Ga in the blue suspension is (18-54):1. After thorough stirring, transfer the mixture to a high-pressure reactor with a polytetrafluoroethylene liner. The reactor is filled to 35%-70% and heated in an oven at 180-200℃ for 42-64 hours to obtain a crude powder.
[0013] S4. The crude powder was ultrasonically cleaned and dried sequentially with dilute ammonia solution, dilute nitric acid solution, deionized water and anhydrous ethanol to obtain CuGaO2 nanoparticles.
[0014] Preferably, in step S2, NaOH solution or KOH solution is added to adjust the pH value of the CuGaO2 precursor solution.
[0015] Preferably, the total concentration of metal ions Cu and Ga in the blue suspension of step S2 is 0.05-0.2 mol / L.
[0016] Preferably, when the sensor is used to monitor dimethyl disulfide gas, the gas-sensitive material is heated to 20-320°C by heating electrodes.
[0017] The second objective of this invention is to provide a method for preparing the dimethyl disulfide gas sensor described in any one of the above-mentioned methods, comprising the following steps: uniformly dispersing CuGaO2 nanoparticles in anhydrous ethanol at a concentration of 0.05 g-0.3 g / ml to obtain a gas-sensitive material slurry; coating the gas-sensitive material slurry onto a substrate with a coating thickness of 0.5 μm-20 μm, and then aging it in air at 150-450°C for 12-168 h; and then setting a Pt or Au test electrode and a heating electrode on the substrate to obtain the CuGaO2 dimethyl disulfide gas sensor.
[0018] Further improvements to the preparation method of the dimethyl disulfide gas sensor:
[0019] Preferably, the dispersion concentration of the CuGaO2 nanoparticles in anhydrous ethanol is 50-300 mg / mL.
[0020] The advantages of this invention compared to the prior art are as follows:
[0021] 1) The manufacturing process of the dimethyl disulfide gas sensor of the present invention is simple and easy to operate.
[0022] 2) The copper-iron oxide CuGaO2 nanoparticles of the present invention exhibit high response sensitivity to dimethyl disulfide gas between 100-220℃. As the working temperature increases, the response sensitivity first increases and then decreases, and the response and recovery time shortens. The response sensitivity is highest when the working temperature is 140℃ under constant temperature heating mode.
[0023] 3) The sensor prepared by this invention has excellent selectivity for dimethyl disulfide and is not sensitive to other common gases (such as methanol, ethanol, acetone, toluene, O3, H2S and NH3, etc.). It can quickly and effectively detect dimethyl disulfide gas with a concentration of 0.1-100 ppm in a variety of mixed gases. Attached Figure Description
[0024] Figure 1 The image shows the X-ray diffraction pattern of the CuGaO2 nanoparticles with a copper-iron structure in Example 1.
[0025] Figure 2 This is a scanning electron microscope image of the CuGaO2 nanoparticles with a copper-iron oxide structure in Example 1.
[0026] Figure 3 This is a scanning electron microscope image of the CuGaO2 nanoparticles with a copper-iron oxide structure in Example 2;
[0027] Figure 4 This is a scanning electron microscope image of the CuGaO2 nanoparticles with a copper-iron oxide structure in Example 3;
[0028] Figure 5 The DC resistance change response of the dimethyl disulfide gas sensor prepared in Example 1 to 1 ppm dimethyl disulfide gas at a constant operating temperature of 100-220℃ is shown in the figure.
[0029] Figure 6 The resistance dynamics of the dimethyl disulfide gas sensor prepared in Example 1 in 0.1-30 ppm dimethyl disulfide gas (operating temperature constant at 140℃) are shown in the graph.
[0030] Figure 7 This is a comparison of the response of the dimethyl disulfide gas sensor prepared in Example 1 to dimethyl disulfide and various common interfering gases at a constant operating temperature of 140°C. Where R... a R represents the resistance of the sensor in air. g This indicates the resistance of the sensor in target gases of different concentrations.
[0031] Figure 8 The graph shows the dynamic resistance change of the dimethyl disulfide gas sensor prepared in Example 1 of this invention in 0.1-5 ppm dimethyl disulfide gas (the sensor operates in pulse heating mode, with the heating voltage switching between 0.1V and 6V every 5 seconds). Detailed Implementation
[0032] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0033] Example 1
[0034] This embodiment provides a method for preparing a dimethyl disulfide gas sensor using CuGaO2, a copper-iron oxide structure, as the sensing material, comprising the following steps:
[0035] Step 1: Dissolve 1.8 mmol of Cu(NO3)3·3H2O and 1.8 mmol of Ga(NO3)3·xH2O in 17 mL of deionized water and stir magnetically to obtain a transparent and clear CuGaO2 precursor solution.
[0036] Step 2: Add 9 mL of NaOH solution to the CuGaO2 precursor solution and adjust the pH to 8 to obtain a blue suspension;
[0037] Step 3: Add 9 mL of ethylene glycol (about 0.16 mol) to the blue suspension, stir thoroughly for 1 h, transfer to a 100 mL polytetrafluoroethylene-lined high-pressure reactor with a filling degree of 35%, and heat in an oven at 190 °C for 56 h to obtain crude powder.
[0038] Step 4: The crude powder is ultrasonically cleaned sequentially with dilute ammonia solution, dilute nitric acid solution, deionized water and anhydrous ethanol, and finally dried in an oven to obtain CuGaO2 nanoparticles.
[0039] Step 5: 0.2g of CuGaO2 nanoparticles are uniformly dispersed in 1mL of anhydrous ethanol to obtain a gas-sensitive material slurry. The gas-sensitive material slurry is coated onto a substrate to form a gas-sensitive film with a coating thickness of 10μm. Then, it is aged in air at 200℃ for 72h. A Pt test electrode is then set on the upper surface of the substrate, and a heating electrode is set on the lower surface to obtain the CuGaO2 dimethyl disulfide gas sensor.
[0040] The copper-iron oxide CuGaO2 nanoparticles obtained in this embodiment were characterized by X-ray diffraction and scanning electron microscopy, and the results are shown in the attached figures. Figure 1and Figure 2 .Depend on Figure 1 , 2 It can be seen that the nanoparticles obtained using this embodiment are single-phase copper-iron ore structure CuGaO2 plate-like particles with a thickness of less than 100 nm.
[0041] Example 2
[0042] This embodiment provides a method for preparing a dimethyl disulfide gas sensor using CuGaO2, a copper-iron oxide structure, as the sensing material, comprising the following steps:
[0043] Step 1: Dissolve 1.0 mmol of Cu(NO3)3·3H2O and 1.0 mmol of Ga(NO3)3·xH2O in 12 mL of deionized water and stir magnetically to obtain a transparent and clear CuGaO2 precursor solution.
[0044] Step 2: Add 4 mL of NaOH solution to the CuGaO2 precursor solution to adjust the pH to 4.5, and a blue suspension is obtained.
[0045] Step 3: Add 5 mL of ethylene glycol (approximately 0.089 mol) to the blue suspension, stir thoroughly for 1 hour, transfer to a high-pressure reactor with a polytetrafluoroethylene liner, fill the reactor to 70%, and heat in an oven at 190°C for 56 hours to obtain crude powder.
[0046] Step 4: The crude powder is ultrasonically cleaned sequentially with dilute ammonia solution, dilute nitric acid solution, deionized water and anhydrous ethanol, and finally dried in an oven to obtain CuGaO2 nanoparticles.
[0047] Step 5: 0.2g of CuGaO2 nanoparticles are uniformly dispersed in 2mL of anhydrous ethanol to obtain a gas-sensitive material slurry. The gas-sensitive material slurry is coated onto a substrate to form a gas-sensitive film with a coating thickness of 5μm. Then, it is aged in air at 150℃ for 168h. Then, an Au test electrode is set on the upper surface of the substrate and a heating electrode is set on the lower surface to obtain the CuGaO2 dimethyl disulfide gas sensor.
[0048] The CuGaO2 nanoparticles with a copper-iron oxide structure obtained in this embodiment, as shown in the attached figure, were characterized by scanning electron microscopy. Figure 3 These are nanoflowers assembled from single-phase copper-iron ore structure CuGaO2 sheet-like particles.
[0049] Example 3
[0050] This embodiment provides a method for preparing a dimethyl disulfide gas sensor using CuGaO2, a copper-iron oxide structure, as the sensing material, comprising the following steps:
[0051] Step 1: Dissolve 1.0 mmol of Cu(NO3)3·3H2O and 1.0 mmol of Ga(NO3)3·xH2O in 10 mL of deionized water and stir magnetically to obtain a transparent and clear CuGaO2 precursor solution.
[0052] Step 2: Add 6 mL of NaOH solution to the CuGaO2 precursor solution and adjust the pH to 8 to obtain a blue suspension;
[0053] Step 3: Add 5 mL of ethylene glycol (approximately 0.089 mol) to the blue suspension, stir thoroughly for 1 hour, transfer to a high-pressure reactor with a polytetrafluoroethylene liner, fill the reactor to 70%, and heat in an oven at 190°C for 56 hours to obtain crude powder.
[0054] Step 4: The crude powder is ultrasonically cleaned sequentially with dilute ammonia solution, dilute nitric acid solution, deionized water and anhydrous ethanol, and finally dried in an oven to obtain CuGaO2 nanoparticles.
[0055] Step 5: Disperse 0.3g of CuGaO2 nanoparticles uniformly in 1mL of anhydrous ethanol to obtain a gas-sensitive material slurry. Coat the gas-sensitive material slurry onto a substrate to form a gas-sensitive film with a coating thickness of 20μm. Then, age the film in air at 350℃ for 12h. Finally, set a Pt test electrode on the upper surface of the substrate and a heating electrode on the lower surface to obtain the CuGaO2 dimethyl disulfide gas sensor.
[0056] The CuGaO2 nanoparticles with a copper-iron oxide structure obtained in this embodiment, as shown in the attached figure, were characterized by scanning electron microscopy. Figure 4 It consists of dispersed, single-phase copper-iron ore structure CuGaO2 hexagonal plate-like particles, with a thickness of about several hundred nanometers.
[0057] Performance testing:
[0058] The sensors prepared in Examples 1-3 were placed in an air environment, and then dimethyl disulfide gas molecules were introduced. The resistance changes of the sensors in air and in different concentrations of dimethyl disulfide with an air background were measured using a multimeter, and these changes were taken as the sensor signal. Taking the dimethyl disulfide gas sensor prepared in Example 1 as an example, the resistance response curve of this sensor at a constant operating temperature of 100-220℃ is shown below. Figure 5 As shown, it can be found that the sensor has the highest response to dimethyl disulfide at an operating temperature of 140℃.
[0059] Figure 6The graph shows the response of the dimethyl disulfide sensor prepared in Example 1 to 0.1-30 ppm dimethyl disulfide at a constant operating temperature of 140℃. The results show that the sensor has a response of 1.5 to 0.1 ppm dimethyl disulfide, which meets the requirements for dimethyl disulfide sensors in routine environmental monitoring.
[0060] Figure 7 The graph shows the response of the dimethyl disulfide sensor prepared in Example 1 to 10 ppm dimethyl disulfide and other common interfering gases (such as methanol, ethanol, acetone, toluene, O3, H2S, NH3, etc.) at a constant operating temperature of 140°C. This confirms that the dimethyl disulfide gas sensor of the present invention has excellent selectivity.
[0061] Figure 8 The graph shows the dynamic resistance change of the dimethyl disulfide sensor prepared in Example 1 in 0.1-5 ppm dimethyl disulfide gas (the sensor operates in pulse heating mode, with the heating voltage switching between 0.1V and 6V every 5 seconds). Figure 6 It can be seen that the sensor’s response to dimethyl disulfide is significantly improved under pulse heating mode.
[0062] The response performance of the dimethyl disulfide sensor prepared in Example 2 to 0.1-30 ppm dimethyl disulfide was tested at a constant operating temperature of 140°C. The sensor's response to 0.1 ppm dimethyl disulfide was 1.6, which can meet the requirements of dimethyl disulfide sensors for daily environmental detection.
[0063] The response performance of the dimethyl disulfide sensor prepared in Example 3 to 0.1-30 ppm dimethyl disulfide was tested at a constant operating temperature of 140℃. The sensor's response to 0.1 ppm dimethyl disulfide was 1.3, which can meet the requirements of dimethyl disulfide sensors for daily environmental detection.
[0064] Those skilled in the art should understand that the above descriptions are merely several specific embodiments of the present invention, and not all embodiments. It should be noted that many modifications and improvements can be made by those skilled in the art, and all modifications or improvements not exceeding the scope of the claims should be considered within the protection scope of the present invention.
Claims
1. A dimethyl disulfide gas sensor, characterized in that, The device includes a substrate, a gas-sensitive material uniformly coated on the surface of the substrate, a Pt or Au test electrode disposed on the surface of the substrate, and a heating electrode. The substrate is an Al2O3 substrate, and the gas-sensitive material is CuGaO2 nanoparticles with a copper-iron oxide structure.
2. The dimethyl disulfide gas sensor according to claim 1, characterized in that, The thickness of the gas-sensitive material is 500 nm-20 μm.
3. The dimethyl disulfide gas sensor according to claim 1, characterized in that, The CuGaO2 nanoparticles have a particle size of 10 nm-10 μm.
4. The dimethyl disulfide gas sensor according to claim 1, 2, or 3, characterized in that, The preparation method of the CuGaO2 nanoparticles is as follows: S1. Weigh out copper nitrate trihydrate Cu(NO3)2 with a molar ratio of (0.7-1.5):
1. 3H2O and gallium nitrate Ga(NO3)2 xH2O was dissolved in deionized water to obtain a transparent and clear CuGaO2 precursor solution; S2. Adjust the pH of the CuGaO2 precursor solution to 3-8 to obtain a blue suspension; S3. Slowly add ethylene glycol to the blue suspension, wherein the molar ratio of ethylene glycol to the sum of the molar amounts of metal ions Cu and Ga in the blue suspension is (18-54):
1. After thorough stirring, transfer the mixture to a high-pressure reactor with a polytetrafluoroethylene liner. The reactor is filled to 35%-70% and heated in an oven at 180-200 ℃ for 42-64 h to obtain a crude powder. S4. The crude powder was ultrasonically cleaned and dried sequentially with dilute ammonia solution, dilute nitric acid solution, deionized water and anhydrous ethanol to obtain CuGaO2 nanoparticles.
5. The dimethyl disulfide gas sensor according to claim 4, characterized in that, In step S2, NaOH or KOH solution is added to adjust the pH value of the CuGaO2 precursor solution.
6. The dimethyl disulfide gas sensor according to claim 4, characterized in that, The total concentration of metal ions Cu and Ga in the blue suspension of step S2 is 0.05-0.2 mol / L.
7. The dimethyl disulfide gas sensor according to claim 1, characterized in that, When used to monitor dimethyl disulfide gas, the gas-sensitive material is heated to 20-320 °C by heating electrodes.
8. A method for preparing a dimethyl disulfide gas sensor according to any one of claims 1-7, characterized in that, The process includes the following steps: uniformly dispersing CuGaO2 nanoparticles in anhydrous ethanol at a concentration of 0.05 g-0.3 g / ml to obtain a gas-sensitive material slurry; coating the gas-sensitive material slurry onto a substrate with a coating thickness of 0.5 μm-20 μm, and then aging it in air at 150-450℃ for 12-168 h; and then setting Pt or Au test electrodes and heating electrodes on the substrate to obtain a CuGaO2 dimethyl disulfide gas sensor.
Citation Information
Patent Citations
Dimethyldisulfide gas sensor based on porous Cr2O3 nano material and preparation method thereof