A sulfide electrolyte suitable for the negative electrode side of an all-solid-state battery and its preparation method
By coating polymer pyrolysis products containing C and F elements onto a sulfide electrolyte precursor to form a uniform coating layer, the problem of instability of sulfide electrolytes at low voltage is solved, the stability and conductivity of the electrolyte are improved, and high-efficiency battery performance and industrial production are achieved.
Patent Information
- Application Number
- CN202311491082.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-09
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-11-09
AI Technical Summary
Existing sulfide electrolytes are unstable at low voltages and are prone to decomposition upon contact with lithium metal, leading to decreased conductivity and lithium plating. Furthermore, high-energy ball milling is difficult to scale up for industrial production.
A polymer-coated sulfide electrolyte precursor is used to form a uniform coating layer containing C and F elements through pyrolysis products. This provides an electronic conductivity channel and generates an inert LiF layer during lithium plating. Combined with simple mixing and sintering, P2S5 loss is reduced.
It improves the stability and ionic conductivity of sulfide electrolytes, reduces electronic conductivity, enhances the electrochemical window, and reduces the energy consumption and time of high-energy ball milling, making it suitable for industrial production.
Smart Images

Figure CN117477009B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of all-solid-state battery technology, and particularly relates to a sulfide electrolyte suitable for the negative electrode side of an all-solid-state battery and its preparation method. Background Technology
[0002] In liquid lithium-ion batteries, liquid esters are typically used as electrolytes. This makes traditional liquid electrolytes and corresponding lithium-ion batteries prone to combustion and explosion upon exposure to external thermal or mechanical shocks. Furthermore, due to the narrow electrochemical window of the electrolyte, CEI or SEI formation occurs upon contact with high-nickel cathode and low-potential anode materials (such as Si and Li), continuously consuming the electrolyte. This also limits further improvements in the energy density of liquid batteries.
[0003] All-solid-state batteries offer improved safety compared to liquid lithium-ion batteries by using a non-volatile, non-flowing, and non-flammable solid electrolyte instead of the electrolyte found in traditional liquid batteries. However, sulfide electrolytes suffer from instability at low potentials. For example, Li6PS5Cl electrolyte decomposes into LiCl, Li3P, and Li2S upon contact with lithium metal, leading to a continuous decrease in electrolyte conductivity and interfacial degradation. Even without lithium metal as the negative electrode, slight lithium plating occurs on the surface of the negative electrode active material during high-rate charging or low-temperature charging. This deposited lithium metal can still cause surface degradation of the sulfide electrolyte in contact with it at the corresponding potential.
[0004] In order to improve the stability of sulfide electrolytes at low voltages, especially when they are used on the negative electrode side of all-solid-state batteries and in direct contact with the negative electrode active material, intrinsic modification or interface modification is generally carried out by means of element doping or coating of sulfides.
[0005] Chinese patent application CN202310206178.0 discloses a method for preparing a core-shell structured sulfide solid electrolyte. The core-shell sulfide solid electrolyte has a sulfide solid electrolyte as its core, with a lithium halide compound coating the surface of the sulfide solid electrolyte to form a shell. For example, a LiF-coated core-shell Li... 10 GeP2S 12Sulfide solid electrolytes. Chinese patent CN114524416A describes a ball milling method for coating lithium sulfide onto the surface of a sulfide electrolyte. However, these methods all employ ball milling and sintering to coat inorganic materials (LiCl, LiS, LiF, etc.) onto the sulfide electrolyte. These inorganic materials generally have low ionic and electronic conductivity, and the coating process inevitably results in uneven coating and defects. During high-rate charging, lithium metal tends to deposit at the interface where high electronic and ionic conductivity are mixed (this is because the two necessary conditions for lithium deposition are the simultaneous presence of lithium ions and electrons). Therefore, lithium deposition often occurs at conductive carbon (sites providing electrons) and coating defects (sites providing ions), leading to lithium deposition at coating defects in the electrolyte and causing degradation of the incompletely coated areas where lithium metal comes into contact.
[0006] Chinese patent CN113782824A describes coating a sulfide electrolyte surface with an ionicly conductive polymer. However, polymers generally only exhibit high conductivity at high temperatures, leading to a decrease in the overall conductivity of the electrolyte after coating. Furthermore, organic coatings also suffer from the drawbacks of inorganic coatings, namely, lithium plating is more likely to occur at coating defects and uncoated areas.
[0007] Meanwhile, the sulfide electrolyte uses P2S5 as a synthesis raw material, which has a boiling point of 514℃ and sublimates at temperatures not exceeding 360℃. Therefore, during the sintering process of the electrolyte precursor, P2S5, due to its low sublimation temperature, will... 7-a PS 6-a Before the crystal phase of electrolyte X is formed, some of it is sublimated and lost, which in turn changes the electrolyte composition ratio, resulting in defects in the synthesized electrolyte.
[0008] Typically, to reduce the loss of P2S5 during the sintering process of sulfide electrolytes, raw materials Li2S, LiCl, and P2S5 are pretreated using a high-energy ball mill in general electrolyte synthesis. This pretreatment forms the electrolyte precursor (i.e., P2S5 has already participated in the reaction and, together with other substances, has been transformed into the electrolyte precursor) before sintering. However, the high-energy ball milling step is energy-intensive and time-consuming (typically, the high-energy ball milling speed is >600 rpm and the milling time is >20 hours); furthermore, due to the high cost of high-energy ball mills and the small batch size, the high-energy ball milling method is difficult to scale up for industrial production. Summary of the Invention
[0009] In view of this, the technical problem to be solved by the present invention is to provide a sulfide electrolyte with strong stability suitable for the negative electrode side of an all-solid-state battery and a method for preparing the same.
[0010] This invention provides a sulfide electrolyte suitable for the negative electrode side of an all-solid-state battery, comprising a matrix and a coating layer covering the matrix; the matrix is a sulfide solid electrolyte; the coating layer contains pyrolysis products of a polymer; the polymer is selected from polymers with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide or polymers containing the element F.
[0011] Preferably, the polymer with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide is selected from one or more of polytetrafluoroethylene, polyetheretherketone, polyvinylidene fluoride, polyimide, polyethylene, polyvinyl chloride, polystyrene, and polypropylene. The mass of the polymer whose pyrolysis temperature is greater than the sublimation temperature of phosphorus pentasulfide is 0.2% to 3% of the mass of the sulfide electrolyte.
[0012] Preferably, the polymer containing element F is composed of elements C, F and H, or of elements C, F, H and A; the element A is selected from one or more of elements Cl, Br and I.
[0013] Preferably, the mass ratio of the F element to the matrix in the F-containing polymer is 0.0005 to 0.01:1.
[0014] Preferably, the polymer containing the F element is selected from one or more of polychlorotrifluoroethylene, polyvinylidene fluoride, ethylene-vinylidene fluoride copolymer, ethylene-chlorotrifluoroethylene copolymer, polyvinylidene fluoride and polyhexafluoroisobutylene; The sulfide solid electrolyte is Li with X replaced by F on its surface. 7-a PS 6-a X a , where 1≤a≤2, and X is Cl, Br or I.
[0015] The present invention also provides a method for preparing the above-mentioned sulfide electrolyte, comprising the following steps: S1) The sulfide solid electrolyte precursor is mixed with the coating solution and dried to obtain a polymer-coated precursor; the coating solution includes a polymer; the polymer is selected from polymers with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide or polymers containing the element F. S2) The polymer-coated precursor is sintered to obtain a sulfide electrolyte; the sintering temperature is higher than the polymer pyrolysis temperature and the crystallization temperature of the sulfide solid electrolyte precursor.
[0016] Preferably, the precursor of the sulfide solid electrolyte is prepared according to the following steps: LiX, Li2S and P2S5 were mixed and ball-milled to obtain a sulfide solid electrolyte precursor; wherein X is Cl, Br or I. When the polymer is a polymer with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide, the rotation speed of the mixing ball mill is 100~200 rpm; the mixing ball milling time is 10~60 min. When the polymer is a polymer containing the element F, the rotation speed of the mixing ball mill is 300~600 rpm; the mixing ball milling time is 6~24 h.
[0017] Preferably, the polymer concentration in the coating solution is 0.1% to 2% by mass. The solvent in the coating solution is selected from one or more of benzene-based solvents, nitrile solvents, and ketone solvents.
[0018] Preferably, the sintering temperature is 380℃~600℃; the sintering time is 3~10 h.
[0019] The present invention also provides an all-solid-state battery comprising the above-described sulfide electrolyte.
[0020] This invention provides a sulfide electrolyte suitable for the negative electrode side of an all-solid-state battery, comprising a substrate and a coating layer covering the substrate; the substrate is a sulfide solid electrolyte; the coating layer contains pyrolysis products of a polymer; the polymer is selected from polymers containing the element F. Compared with the prior art, the coating layer of the sulfide electrolyte provided by this invention is a uniformly mixed mixture at the atomic level, comprising C and F elements. C provides an electron conduction channel, inducing lithium plating at the C element locations; simultaneously, F is a highly electronegative anionic element. Addressing the potential lithium plating phenomenon at the negative electrode under special operating conditions (low temperature, high-rate charging), the sulfide electrolyte coating layer decomposes upon contact with lithium metal, rapidly forming LiF with the lithium metal produced by lithium plating. This consumes the deposited lithium while protecting the sulfide electrolyte substrate from lithium metal attack. Furthermore, the generated LiF remains an inert layer for lithium metal, thus preventing lithium metal from tending to form at uncoated sites, thereby enhancing the stability of the sulfide electrolyte when used on the negative electrode side.
[0021] This invention provides a sulfide electrolyte suitable for the negative electrode side of an all-solid-state battery, comprising a matrix and a coating layer covering the matrix; the matrix is a sulfide solid electrolyte; the coating layer contains pyrolysis products of a polymer; the polymer is selected from polymers with pyrolysis temperatures higher than the sublimation temperature of phosphorus pentasulfide. Compared with the prior art, this invention uses a polymer to coat the precursor of the sulfide electrolyte before sintering. The presence of the polymer protects the electrolyte precursor by covering its surface with polymer, thus effectively reducing the loss of P2S5 during the heating process, ultimately making the actual synthesis ratio closer to the theoretical calculation value; ultimately, it has beneficial effects on improving the ionic conductivity of the electrolyte, reducing the electronic conductivity, and improving the electrochemical window. Therefore, using a polymer to coat the precursor or a simple mixture of raw materials before sintering can effectively improve the electrical performance of the electrolyte. Furthermore, in order to increase the synthesis amount of electrolyte per batch while reducing the loss of P2S5 during the sintering process, this invention further proposes a method for synthesizing the electrolyte. That is, the raw materials for electrolyte synthesis, Li2S, LiCl, and P2S5, are simply mixed, and then the surface of the mixture is coated with a polymer. The presence of the polymer increases the saturated vapor pressure of P2S5 in the gas phase, thus helping to suppress the sublimation and vaporization escape of P2S5. This allows P2S5 to reach the reaction temperature and transform into an intermediate product for electrolyte formation before volatilization loss, reducing its loss during the synthesis process. This achieves the beneficial effect of making the synthesis stoichiometric ratio as close as possible to the theoretical design value. Therefore, the method for preparing sulfide electrolytes provided by this invention can avoid high-energy ball milling, simply mixing the electrolyte raw materials, coating them with a polymer, and then sintering. This reduces the loss of P2S5 during high-temperature sintering and suppresses the volatilization of sulfur and phosphorus components, thereby achieving the goal of controlling the component ratio during electrolyte synthesis. Compared with the commonly used high-energy ball milling followed by sintering method, the synthesis efficiency is greatly improved. Attached Figure Description
[0022] Figure 1 This is a schematic diagram of the preparation process of the sulfide electrolyte provided by the present invention; Figure 2 The SEM scan image and local EDS elemental analysis characterization results of the sulfide electrolyte provided in Example 1 of this invention; Figure 3 The XPS characterization results are for the electrolytes prepared in Example 1 and Comparative Example 1 of this invention. Detailed Implementation
[0023] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0024] This invention provides a sulfide electrolyte suitable for the negative electrode side of an all-solid-state battery, comprising a matrix and a coating layer covering the matrix; the matrix is a sulfide solid electrolyte; the coating layer contains pyrolysis products of a polymer; the polymer is selected from polymers with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide or polymers containing the element F.
[0025] According to the present invention, the matrix is a sulfide solid electrolyte, preferably a sulfide solid electrolyte containing Li, S and halide anions; the halide anions preferably include Cl, Br or I; more specifically, the sulfide solid electrolyte is Li 7-a PS 6-a X a Where 1≤a≤2, preferably 1≤a≤1.6, and X is Cl, Br, or I; more specifically, the sulfide solid electrolyte can be Li6PS5Cl, Li 5.6 PS 4.6 Br 1.4 With Li 5.4 PS 4.4 I 1.6 One or more of the following; or, when the polymer contains F, the halide anion element in the sulfide solid electrolyte includes one of Cl, Br, and I, and F. Specifically, the sulfide solid electrolyte is Li₂ with surface X element replaced by F. 7- a PS 6-a X a More specifically, the sulfide solid electrolyte includes, but is not limited to: Li6PS5Cl 0.9929 F 0.0071 Li6PS5Cl 0.99 F 0.01 Li 5.6 PS 4.6 Br 1.397 9F 0.0021 Li 5.6 PS 4.6 Br 1.3588 F 0.0412 1.6Li 5.4 PS 4.4 I 1.5984 F 0.0016 Li5.4 PS 4.4 I1.5 675 F0.03 25 Li with surface X replaced by F 7-a PS 6-a X a Upon contact with deposited lithium metal, a reaction occurs to form lithium fluoride, thus consuming the deposited lithium while continuing to protect the electrolyte. For example, Li6PS5Cl... 0.9929 F 0.0071 Upon contact with precipitated lithium metal, it decomposes to form Li3P, Li2S, LiCl, and LiF, and Li6PS5Cl. 0.9929 F 0.0071 + 8Li = Li3P + 5Li2S + 0.9929LiCl + 0.0071LiF While consuming the deposited lithium, the generated LiF continues to protect the sulfide electrolyte matrix from lithium metal attack.
[0026] The matrix is covered with a coating layer; the coating layer contains the pyrolysis products of the polymer; the thermal decomposition temperature of the polymer is preferably lower than the maximum temperature required for sintering the sulfide electrolyte, so that the polymer will not remain in the final electrolyte; the polymer is selected from polymers with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide or polymers containing the element F.
[0027] According to this invention, the presence of a polymer with a pyrolysis temperature higher than the sublimation temperature of phosphorus pentasulfide protects the electrolyte precursor by coating it with the polymer, thus effectively reducing the loss of P2S5 during the heating process. This results in the actual synthesis ratio being closer to the theoretical calculation value. Ultimately, this has beneficial effects on improving the ionic conductivity of the electrolyte, reducing the electronic conductivity, and expanding the electrochemical window. Therefore, using polymer coatings on the precursor or a simple mixture of raw materials before sintering can effectively improve the electrical properties of the electrolyte. Further preferably, the polymer with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide, or the polymer containing the element F, is composed only of elements C and H, or of elements C, H, and M; the element M is preferably one or more of elements O, N, and A; the element A is preferably one or more of elements Cl, Br, and I; to avoid introducing other elements into the coating layer, the element A is preferably the same as the halide anion element in the sulfide solid electrolyte; even more preferably, the polymer with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide includes, but is not limited to, one or more of polytetrafluoroethylene, polyetheretherketone, polyvinylidene fluoride, polyimide, polyethylene, polyvinyl chloride, polystyrene, and polypropylene; since some polymers leave solid carbon residue on the surface of the electrolyte after thermal decomposition, excessive carbon residue will lead to a decrease in ionic conductivity, but too little polymer coating will result in an excessively thin polymer layer, thus failing to effectively suppress the volatilization of P2S5. Therefore, the mass of the polymer with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide is preferably 0.2% to 3% of the mass of the sulfide electrolyte, more preferably 0.5% to 3%, even more preferably 1% to 3%, even more preferably 1.5% to 3%, and most preferably 1.8% to 3%.
[0028] According to this invention, when the polymer is a polymer containing the element F, the coating layer contains the pyrolysis product of the polymer, i.e., carbides, and also includes the reactants of the polymer pyrolysis product and the sulfide solid electrolyte. In this case, the coating layer is a uniformly mixed mixture at the atomic level, consisting of a mixture of C and F elements. The C element provides an electron conduction channel, inducing lithium plating at the C element locations. Simultaneously, the F element is a highly electronegative anionic element. To address the potential lithium plating at the negative electrode under special operating conditions (low temperature, high-rate charging), the sulfide electrolyte coating layer decomposes upon contact with lithium metal, rapidly forming LiF with the lithium metal produced by lithium plating. This consumes the deposited lithium while protecting the sulfide electrolyte matrix from lithium metal attack. Furthermore, the generated LiF remains an inert layer for lithium metal, thus preventing lithium metal from tending to form at uncoated sites, thereby enhancing the stability of the sulfide electrolyte when used on the negative electrode side. Further preferably, the polymer containing element F is composed of elements C, F, and H, or elements C, F, H, and A; the element A is preferably one or more of elements Cl, Br, and I; to avoid introducing other elements into the coating layer, the element A is preferably the same as the halide anion element in the sulfide solid electrolyte; even more preferably, the polymer is one or more of polychlorotrifluoroethylene, polyvinylidene fluoride, ethylene-vinylidene fluoride copolymer, ethylene-chlorotrifluoroethylene copolymer, polyvinylidene fluoride, and polyhexafluoroisobutylene; the mass ratio of element F to matrix in the polymer is preferably 0.0005:1 to 0.01:1, more preferably 0.0008:1 to 0.005:1, and even more preferably 0.001:1 to 0.002:1. Because element F has strong electronegativity, after replacing element X in the original electrolyte, the migration activation energy of Li ions will increase, which will adversely affect the conductivity. Meanwhile, the content of C and F elements is positively correlated. C is a poor conductor of lithium ions, so an increase in the carbon content coating the electrolyte surface also has an adverse effect on conductivity; therefore, the content of F element is preferably the value mentioned above.
[0029] More preferably, the polymer is one or more of polyetheretherketone, polyimide, polyethylene, polyvinyl chloride, polystyrene, and polypropylene.
[0030] This invention also provides a method for preparing the above-mentioned sulfide electrolyte, wherein a polymer is coated onto a sulfide solid electrolyte precursor and then sintered to obtain the sulfide electrolyte; the coating method can be any coating method known to those skilled in the art and is not particularly limited; in this invention, to improve the uniformity of coating, it is preferred to proceed according to the following steps: S1) The sulfide solid electrolyte precursor is mixed with a coating solution and dried to obtain a polymer-coated precursor; the coating solution includes a polymer; the polymer is selected from polymers with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide or polymers containing the element F; S2) The polymer-coated precursor is sintered to obtain the sulfide electrolyte; the sintering temperature is higher than the pyrolysis temperature of the polymer and the crystallization temperature of the sulfide solid electrolyte precursor.
[0031] See Figure 1 , Figure 1 This is a schematic diagram of the preparation process of the sulfide electrolyte provided by the present invention, wherein 1 is the sulfide solid electrolyte precursor, 2 is the coating solution, 3 is the precursor of the coated polymer, 4 is the molecular structure of the polymer, 5 is the crystallized sulfide solid electrolyte, and 6 is the coating layer.
[0032] In this invention, there are no special restrictions on the source of any raw materials; they can be commercially available.
[0033] In this invention, the sulfide solid electrolyte precursor is preferably prepared according to the following steps: mixing LiX, Li2S, and P2S5 to obtain the sulfide solid electrolyte precursor; where X is Cl, Br, or I; the mixing method can be any method well known to those skilled in the art and is not particularly limited, including but not limited to ball milling, mechanical stirring, three-dimensional mixing, etc.; ball milling is preferred in this invention; when the polymer pyrolysis temperature is greater than the sublimation temperature of phosphorus pentasulfide, the ball milling speed is preferably 100-200 rpm; the ball milling time is preferably 10-60 min, more preferably 20-40 min, and even more preferably 30 min; the sulfide electrolyte preparation method provided by this invention can avoid high-energy ball milling, simply mixing the electrolyte raw materials, coating them with polymer, and then sintering, thereby reducing the loss of P2S5 during high-temperature sintering, inhibiting the volatilization of sulfur and phosphorus components, and thus achieving the purpose of controlling the component ratio during electrolyte synthesis, and greatly improving the synthesis efficiency compared with the generally used high-energy ball milling followed by sintering method. When the polymer is a polymer containing element F, the rotation speed of the mixing ball mill is preferably 300~600 rpm, more preferably 400~500 rpm; the mixing ball milling time is preferably 6~24 h, more preferably 10~20 h, and even more preferably 12~15 h; the molar ratio of elements Li, P, S and X in the obtained sulfide solid electrolyte precursor is (7-a):1:(6-a):a; where 1≤a≤2, preferably 1≤a≤1.6.
[0034] A sulfide solid electrolyte precursor is mixed with a coating solution and dried to obtain a polymer-coated precursor. The coating solution includes a polymer. The molecular weight of the polymer is preferably 100,000 to 500,000. The polymer is the same as described above and will not be repeated here. The mass concentration of the polymer in the coating solution is preferably 0.1% to 2%, more preferably 0.3% to 1.5%, and even more preferably 0.5% to 1%. The solvent in the coating solution is preferably one or more of benzene solvents, nitrile solvents, and ketone solvents. The benzene solvent can be any benzene solvent well known to those skilled in the art and is not particularly limited, but preferably includes, but is not limited to, one or more of benzene, toluene, xylene, trimethylbenzene, and biphenyl. The nitrile solvent can be any nitrile solvent well known to those skilled in the art and is not particularly limited, but preferably includes, but is not limited to, one or more of acetonitrile, butadiene nitrile, and adiponitrile. The ketone solvent is any solvent well known to those skilled in the art. Ketone solvents familiar to those skilled in the art are acceptable and are not particularly limited. In this invention, cyclohexanone, methyl ethyl ketone, and methyl isobutyl ketone are preferred, but not limited to, one or more of these. When the polymer is a polymer containing phosphorus (F), the mass ratio of F in the polymer to the sulfide solid electrolyte precursor is preferably 0.0005~0.01:1, more preferably 0.0008~0.005:1, and even more preferably 0.001~0.002:1. When the polymer has a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide, the mass ratio of the polymer to the sulfide solid electrolyte precursor is 0.0001~0.02:1, more preferably 0.0005~0.016:1. After uniform mixing, the mixture is dried. The drying method is familiar to those skilled in the art and is not particularly limited. In this invention, evaporation is preferred to obtain the polymer-coated precursor. Because the polymer is dissolved and precipitated, compared to traditional solid-solid mixing methods, the method of this invention enables the coating precursor (polymer) to be uniformly mixed with the sulfide solid electrolyte precursor, and densely coated on the precursor material. Simultaneously, because the polymer contains sulfur (F), it is tightly bonded to the sulfide solid electrolyte precursor via hydrogen bonds. Furthermore, by varying the mass ratio of polymer to sulfide solid electrolyte precursor, precursors with different coating amounts of polymer can be obtained.
[0035] The polymer-coated precursor is sintered to obtain a sulfide electrolyte. The sintering temperature is higher than the polymer pyrolysis temperature and the crystallization temperature of the sulfide solid electrolyte precursor, thus allowing the polymer to thermally decompose while the precursor crystallizes. The presence of the polymer increases the vapor pressure of P2S5 in the gas phase, thereby further suppressing the sublimation and vaporization escape of P2S5, making the synthesized value as close as possible to the theoretical calculation value. More specifically, the thermal decomposition products of the fluorinated polymer contain HF and C, wherein the F element in HF replaces the halogens (Cl, Br, I) in the sulfide solid electrolyte. A sulfide solid electrolyte with F-type surface is formed, and simultaneously, carbon elements generated by polymer thermal decomposition are deposited in situ on the surface of the sulfide solid electrolyte. Since the F and C elements in the polymer are mixed at the atomic level, they can still exhibit atomic-level mixing of C and F after thermal decomposition on the electrolyte surface. The sintering temperature is preferably 380℃~600℃, more preferably 400℃~600℃, even more preferably 450℃~600℃, and most preferably 500℃~550℃. In the embodiments provided by the present invention, the sintering temperature is specifically 530℃. The sintering time is preferably 3~10 h, more preferably 5~8 h, and even more preferably 6~7 h.
[0036] This invention aims to enhance the stability of sulfide electrolytes when used on the negative electrode side by mixing electronic conductors (sites where C element is located, inducing lithium metal precipitation) with lithium metal inert sites (sites where F element is located, consuming or protecting the induced lithium metal) at the atomic level, thereby preventing lithium metal from being generated more tending to be generated at uncoated sites.
[0037] The present invention also provides an all-solid-state battery comprising the above-mentioned sulfide electrolyte.
[0038] To further illustrate the present invention, the following describes in detail, with reference to embodiments, a sulfide electrolyte suitable for the negative electrode side of an all-solid-state battery and its preparation method.
[0039] All reagents used in the following examples are commercially available.
[0040] Example 1
[0041] 1.1 Synthesis of sulfide electrolyte precursor: LiCl, Li2S, and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form the precursor of sulfide electrolyte Li6PS5Cl.
[0042] 1.2 Construction of the coating layer precursor: Preparation of the coating solvent: Polyvinylidene fluoride (molecular weight 160,000) was dissolved in p-toluene, and a clear solution was formed after stirring. The mass content of polyvinylidene fluoride in the solvent was 0.5%.
[0043] Construction of the electrolyte precursor coating: The Li6PS5Cl precursor was added to a toluene solution of polyvinylidene fluoride (PVDF) under continuous stirring. After uniform mixing, the solvent was evaporated to dryness at 110°C, yielding a PVDF-coated Li6PS5Cl precursor, thus obtaining the polymer-coated precursor. The mass ratio of sulfur (F) in the PVDF to the sulfide electrolyte precursor was 0.001:1.
[0044] 1.3 Crystallization of electrolyte precursor and in-situ formation of coating: The Li6PS5Cl precursor coated with polyvinylidene fluoride was sealed and sintered at 530°C for 6 h to obtain a sulfide electrolyte with F element surface substitution and C element surface coating, labeled as SSE-F / C.
[0045] See Figure 2 The SSE-F / C obtained in this embodiment was characterized by SEM and EDS elemental analysis of the local area at the frame line. Figure 2 It can be seen that the electrolyte surface is covered by C and F elements, and the positions of the two elements highly overlap, achieving a high degree of mixing.
[0046] Simultaneously, the composition of the obtained electrolyte was quantitatively analyzed. The proportion of phosphorus (P) in the electrolyte was set to 1:1. P and sulfur (S) were determined using an ICP-AES instrument, specifically an Agilent 5900. Li (Li) content was determined using atomic absorption spectrometry (AAS), specifically a Thermo iCE 3500 AAS. Cl (Cl) and phosphorus (F) contents were jointly determined using an ion chromatograph, specifically a Thermo Aquion RFIC.
[0047] The theoretical composition of the electrolyte in this embodiment is: Li6PS5Cl 0.9859 F 0.0141 After actual measurement using the above method, the actual composition of the electrolyte is Li. 5.904 PS 4.96 Cl 0.9708 F 0.0132 It can be seen that the loss of P2S5 during sintering caused the S element ratio to deviate from the theoretical value, with a deviation of 0.04.
[0048] Example 2
[0049] 2.1 Synthesis of sulfide electrolyte precursor: LiCl, Li2S, and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form the precursor of sulfide electrolyte Li6PS5Cl.
[0050] 2.2 Construction of the coating layer precursor: Preparation of the coating solvent: Polyvinylidene fluoride (molecular weight 100,000) was dissolved in p-toluene, and a clear solution was formed after stirring. The mass content of polyvinylidene fluoride in the solvent was 0.5%.
[0051] Construction of the electrolyte precursor coating: A Li6PS5Cl precursor was added to a toluene solution of polyvinylidene fluoride (PVDF) under continuous stirring. After homogeneous mixing, the solvent was evaporated to dryness at 110°C, yielding a PVDF-coated Li6PS5Cl precursor, thus obtaining the polymer-coated precursor. The mass ratio of sulfur (F) in the PVDF to the sulfide electrolyte precursor was 0.0005:1.
[0052] 2.3 Crystallization of electrolyte precursor and in-situ formation of coating: The Li6PS5Cl precursor coated with polyvinylidene fluoride was sealed and sintered at 530℃ for 6 h to obtain a sulfide electrolyte with F element surface substitution and C element surface coating, labeled as SSE-F / C.
[0053] Example 3
[0054] 3.1 Synthesis of sulfide electrolyte precursor: LiCl, Li2S, and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form the precursor of sulfide electrolyte Li6PS5Cl.
[0055] 3.2 Construction of the coating layer precursor: Preparation of the coating solvent: Polyvinylidene fluoride (molecular weight 400,000) was dissolved in p-toluene, and a clear solution was formed after stirring. The mass content of polyvinylidene fluoride in the solvent was 0.5%.
[0056] Construction of the electrolyte precursor coating: A Li6PS5Cl precursor was added to a toluene solution of polyvinylidene fluoride (PVDF) under continuous stirring. After homogeneous mixing, the solvent was evaporated to dryness at 110°C, yielding a PVDF-coated Li6PS5Cl precursor, thus obtaining the polymer-coated precursor. The mass ratio of sulfur (F) in the PVDF to the sulfide electrolyte precursor was 0.01:1.
[0057] 3.3 Crystallization of electrolyte precursor and in-situ formation of coating: The Li6PS5Cl precursor coated with polyvinylidene fluoride was sealed and sintered at 530℃ for 6 h to obtain a sulfide electrolyte with F element surface substitution and C element surface coating, labeled as SSE-F / C.
[0058] Example 4
[0059] 4.1 Synthesis of sulfide electrolyte precursor: LiCl, Li2S, and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 600 rpm for 6 h using a high-energy ball mill to form the precursor of sulfide electrolyte Li6PS5Cl.
[0060] 4.2 Construction of the coating layer precursor: Preparation of the coating solvent: Polyvinylidene fluoride (molecular weight 100,000) was dissolved in p-toluene, and a clear solution was formed after stirring. The mass content of polyvinylidene fluoride in the solvent was 2%.
[0061] Construction of the electrolyte precursor coating: A Li6PS5Cl precursor was added to a toluene solution of polyvinylidene fluoride (PVDF) under continuous stirring. After homogeneous mixing, the solvent was evaporated to dryness at 110°C, yielding a PVDF-coated Li6PS5Cl precursor, thus obtaining the polymer-coated precursor. The mass ratio of sulfur (F) in the PVDF to the sulfide electrolyte precursor was 0.01:1.
[0062] 4.3 Crystallization of electrolyte precursor and in-situ formation of coating: The above-mentioned polyvinylidene fluoride coated Li6PS5Cl precursor was sealed and sintered at 380℃ for 10 h to obtain a sulfide electrolyte with F element surface substitution and C element surface coating, labeled as SSE-F / C.
[0063] Example 5
[0064] 5.1 Synthesis of sulfide electrolyte precursor: LiCl, Li2S, and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 300 rpm for 24 h using a high-energy ball mill to form the precursor of sulfide electrolyte Li6PS5Cl.
[0065] 5.2 Construction of the coating layer precursor: Preparation of the coating solvent: Polyvinylidene fluoride (molecular weight 500,000) was dissolved in p-toluene, and a clear solution was formed after stirring. The mass content of polyvinylidene fluoride in the solvent was 0.1%.
[0066] Construction of the electrolyte precursor coating: A Li6PS5Cl precursor was added to a toluene solution of polyvinylidene fluoride (PVDF) under continuous stirring. After homogeneous mixing, the solvent was evaporated to dryness at 110°C, yielding a PVDF-coated Li6PS5Cl precursor, thus obtaining the polymer-coated precursor. The mass ratio of sulfur (F) in the PVDF to the sulfide electrolyte precursor was 0.005:1.
[0067] 5.3 Crystallization of electrolyte precursor and in-situ formation of coating: The above-mentioned polyvinylidene fluoride coated Li6PS5Cl precursor was sealed and sintered at 600℃ for 3h to obtain a sulfide electrolyte with F element surface substitution and C element surface coating, denoted as SSE-F / C.
[0068] Example 6
[0069] 6.1 Synthesis of sulfide electrolyte precursor: LiBr, Li2S, and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 500 rpm for 16 h using a high-energy ball mill to form the precursor of sulfide electrolyte Li6PS5Br.
[0070] 6.2 Construction of the coating layer precursor: Preparation of the coating solvent: Polyvinylidene fluoride (molecular weight 160,000) was dissolved in p-toluene, and a clear solution was formed after stirring. The mass content of polyvinylidene fluoride in the solvent was 0.1%.
[0071] Construction of the electrolyte precursor coating: The Li6PS5Br precursor was added to a toluene solution of polyvinylidene fluoride (PVDF) under continuous stirring. After homogeneous mixing, the solvent was evaporated to dryness at 110°C, yielding a PVDF-coated Li6PS5Br precursor, thus obtaining the polymer-coated precursor. The mass ratio of sulfur (F) in the PVDF to the sulfide electrolyte precursor was 0.005:1.
[0072] 6.3 Crystallization of electrolyte precursor and in-situ formation of coating: The above-mentioned polyvinylidene fluoride coated Li6PS5Br precursor was sealed and sintered at 600℃ for 3h to obtain a sulfide electrolyte with F element surface substitution and C element surface coating, labeled as SSE-F / C.
[0073] Example 7
[0074] 7.1 Synthesis of sulfide electrolyte precursor: LiI, Li2S, and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form the precursor of sulfide electrolyte Li6PS5I.
[0075] 7.2 Construction of the coating layer precursor: Preparation of the coating solvent: Polyvinylidene fluoride (molecular weight 400,000) was dissolved in p-toluene, and a clear solution was formed after stirring. The mass content of polyvinylidene fluoride in the solvent was 0.5%.
[0076] Construction of the electrolyte precursor coating: The Li6PS5I precursor was added to a toluene solution of polyvinylidene fluoride (PVDF) under continuous stirring. After uniform mixing, the solvent was evaporated to dryness at 110°C, yielding a PVDF-coated Li6PS5I precursor, thus obtaining the polymer-coated precursor. The mass ratio of sulfur (F) in the PVDF to the sulfide electrolyte precursor was 0.01:1.
[0077] 7.3 Crystallization of electrolyte precursor and in-situ formation of coating: The above-mentioned polyvinylidene fluoride coated Li6PS5I precursor was sealed and sintered at 530℃ for 6 h to obtain a sulfide electrolyte with F element surface substitution and C element surface coating, labeled as SSE-F / C.
[0078] Example 8
[0079] 8.1 Synthesis of sulfide electrolyte raw materials: LiCl, Li2S and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 100 rpm for 30 min to form a mixture of raw materials.
[0080] 8.2 Construction of the cladding layer: Preparation of the coating solvent: Polyvinylidene fluoride (molecular weight 160,000) was dissolved in p-toluene, and a clear solution was formed after stirring. The mass content of polyvinylidene fluoride in the solvent was 0.5%.
[0081] Construction of the electrolyte precursor coating: A mixture of raw materials was added to a toluene solution of polyvinylidene fluoride (PVDF) under continuous stirring. After homogeneous mixing, the solvent was evaporated to dryness at 110°C, yielding a substance with PVDF coated on the raw material mixture, thus obtaining the polymer-coated precursor. The mass ratio of sulfur (F) in the PVDF to the mass of the electrolyte raw material mixture was 0.001:1.
[0082] 8.3 Sintering of electrolyte and in-situ formation of coating: The raw material mixture coated with polyvinylidene fluoride was sealed and sintered at 530°C for 6 h to obtain a sulfide electrolyte with F element surface substitution and C element surface coating, labeled as SSE-F / C.
[0083] Simultaneously, the composition of the obtained electrolyte was quantitatively analyzed. The proportion of phosphorus (P) in the electrolyte was set to 1:1. P and sulfur (S) were determined using an ICP-AES instrument, specifically an Agilent 5900. Li (Li) content was determined using atomic absorption spectrometry (AAS), specifically a Thermo iCE 3500 AAS. Cl (Cl) and phosphorus (F) contents were jointly determined using an ion chromatograph, specifically a Thermo Aquion RFIC.
[0084] The theoretical composition of the electrolyte in this embodiment is: Li6PS5Cl 0.9859 F 0.0141 After actual measurement using the above method, the actual composition of the electrolyte is Li. 5.78 PS 4.91 Cl 0.95 F 0.013 It can be seen that the loss of P2S5 during sintering caused the S element ratio to deviate from the theoretical value, with a deviation of 0.13.
[0085] Example 9
[0086] 9.1 Synthesis of sulfide electrolyte raw materials: LiCl, Li2S and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 100 rpm for 30 min to form a mixture of raw materials.
[0087] 9.2 Construction of the cladding layer: Preparation of the coating solvent: Polypropylene is dissolved in toluene, and after stirring, a clear solution is formed. Polyetheretherketone (PEEK) powder is then dispersed in the solution. The mass content of polypropylene in the solvent is 0.5%, and the mass ratio of PEEK to polypropylene is 1:1.
[0088] Construction of the electrolyte precursor coating: A mixture of electrolyte raw materials was added to the above coating mixture under continuous stirring. After uniform mixing, the solvent was evaporated at 110°C to obtain a polypropylene coating on the mixture of raw materials and polyetheretherketone, i.e., the precursor of the coated polymer. The sum of the masses of polypropylene and polyimide accounted for 3% of the total mass.
[0089] 9.3 Sintering of electrolyte: The above-coated raw material mixture was sealed and sintered at 530°C for 6 h to obtain sulfide electrolyte, labeled as SSE-F / C.
[0090] Simultaneously, the composition of the obtained electrolyte was quantitatively analyzed. The proportion of phosphorus (P) in the electrolyte was set to 1:1. P and sulfur (S) were determined using an ICP-AES instrument, specifically an Agilent 5900. Li (Li) content was determined using atomic absorption spectrometry (AAS) using a Thermo iCE 3500 AAS. Cl (Cl) content was determined using an ion chromatograph, specifically a Thermo Aquion RFIC.
[0091] The theoretical composition of the electrolyte in this embodiment is Li6PS5Cl. After actual measurement using the above method, the actual composition of the electrolyte is Li. 5.904 PS 4.96 Cl 0.984 It can be seen that the loss of P2S5 during sintering caused the S element ratio to deviate from the theoretical value, with a deviation of 0.04.
[0092] Example 10
[0093] 10.1 Synthesis of sulfide electrolyte raw materials: LiCl, Li2S, and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 100 rpm for 30 min to form a mixture of raw materials.
[0094] 10.2 Construction of the cladding layer: Preparation of the coating solvent: The fully aromatic polyimide was dissolved in tetrahydrofuran and stirred to form a solution. The mass content of the fully aromatic polyimide in the solvent was 0.3%.
[0095] Construction of the electrolyte precursor coating: The mixture of raw materials was added to the above solution under continuous stirring. After uniform mixing, the solvent was evaporated at 70°C to obtain a substance in which a fully aromatic polyimide was coated on the raw material mixture, thus obtaining the precursor of the coated polymer. The fully aromatic polyimide accounted for 1.8% of the total mass.
[0096] 10.3 Sintering of electrolyte: The raw material mixture coated with the above-mentioned all-aromatic polyimide was sealed and sintered at 530°C for 6 h to obtain sulfide electrolyte.
[0097] Simultaneously, the composition of the obtained electrolyte was quantitatively analyzed. The proportion of phosphorus (P) in the electrolyte was set to 1:1. P and sulfur (S) were determined using an ICP-AES instrument, specifically an Agilent 5900. Li (Li) content was determined using atomic absorption spectrometry (AAS) using a Thermo iCE 3500 AAS. Cl (Cl) content was determined using an ion chromatograph, specifically a Thermo Aquion RFIC.
[0098] The theoretical composition of the electrolyte in this embodiment is Li6PS5Cl. After actual measurement using the above method, the actual composition of the electrolyte is Li. 5.78 PS 4.91 Cl 0.963 It can be seen that the loss of P2S5 during sintering caused the S element ratio to deviate from the theoretical value, with a deviation of 0.06.
[0099] Comparative Example 1
[0100] LiCl, Li₂S, and P₂S₅ were mixed in a molar ratio of 1:2.5:0.5, and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form a precursor for the sulfide electrolyte Li₆PS₅Cl. The Li₆PS₅Cl precursor was then sintered in a sealed container at 530 °C for 6 h to obtain a substance with a theoretical composition of Li₆PS₅Cl₆. Simultaneously, the composition of the electrolyte obtained in Comparative Example 1 was characterized according to the method described in Example 1. The actual composition of the electrolyte was Li₂S₅. 5.64 PS 4.85 Cl 0.94 It can be seen that the loss of P2S5 during sintering caused the S element ratio to deviate from the theoretical value by 0.15.
[0101] The electrolytes obtained in Example 1 and Comparative Example 1 were analyzed using XPS to characterize the distribution of chemical bonds on the electrolyte surface. The results are as follows: Figure 3 As shown in the figure. In Example 1, the presence of a characteristic peak of F- at 685 eV indicates that F has undergone elemental substitution on the surface of the electrolyte particles.
[0102] Comparative Example 2
[0103] LiCl, Li₂S, and P₂S₅ were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 100 rpm for 30 min to form a raw material mixture. This mixture was then sealed and sintered at 530°C for 6 h to obtain a substance with a theoretical composition of Li₆PS₅Cl₆. Simultaneously, the electrolyte composition obtained in Comparative Example 1 was characterized according to the method described in Example 1. The actual composition of the electrolyte was Li₂S₅Cl₆. 5.16 PS 4.65 Cl 0.86 It can be seen that the loss of P2S5 during sintering caused the S element ratio to deviate from the theoretical value by 0.35.
[0104] Table 1. Composition of electrolytes in Examples 8-10 and Comparative Examples 1-2
[0105] As can be seen from the S content deviation values in Comparative Example 2 in Table 1, if the electrolyte is not pre-formed as a precursor through high-energy ball milling and the polymer coating method of this invention is not used, the S content in the final electrolyte product deviates significantly from the theoretical value. A comparison of the S content deviation values between Comparative Example 1 and the examples shows that, while achieving approximately the same S content deviation value, the coating method of this invention can significantly reduce the time required for high-energy ball milling and improve preparation efficiency.
[0106] Comparative Example 3
[0107] LiCl, Li₂S, and P₂S₅ were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form a precursor for the sulfide electrolyte Li₆PS₅Cl. The Li₆PS₅Cl precursor was then sintered in a sealed container at 530 °C for 6 h to obtain Li₆PS₅Cl₆. Li₆PS₅Cl₆ was then mixed with NH₄F, wherein the mass ratio of F to the sulfide electrolyte precursor was 0.001:1, and sintered in a sealed container at 200 °C to obtain a sulfide electrolyte with F surface substitution.
[0108] Comparative Example 4
[0109] LiCl, Li₂S, and P₂S₅ were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form a precursor for the sulfide electrolyte Li₆PS₅Cl. The Li₆PS₅Cl precursor was then sealed and sintered at 530 °C for 6 h to obtain Li₆PS₅Cl₆. Li₆PS₅Cl₆ was then ball-milled with graphene at a mass ratio of 0.001:1, yielding a carbon-coated sulfide electrolyte.
[0110] Comparative Example 5
[0111] LiCl, Li₂S, and P₂S₅ were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form a precursor for the sulfide electrolyte Li₆PS₅Cl. The Li₆PS₅Cl precursor was then sintered in a sealed container at 530 °C for 6 h to obtain Li₆PS₅Cl₆. Li₆PS₅Cl₆ was then ball-milled with polyvinylidene fluoride (PVDF) and sintered in a sealed container at 530 °C for 6 h to obtain a sulfide electrolyte with F-substituted and C-coated surfaces.
[0112] Comparative Example 6
[0113] LiCl, Li₂S, and P₂S₅ were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form a precursor for the sulfide electrolyte Li₆PS₅Cl. The Li₆PS₅Cl precursor was then sealed and sintered at 530 °C for 6 h to obtain Li₆PS₅Cl₆. Li₆PS₅Cl₆ was then ball-milled and mixed with polyvinylidene fluoride (PVDF) and sealed and sintered at 530 °C for 6 h to obtain a sulfide electrolyte with F-substituted and C-coated surfaces.
[0114] Comparative Example 7
[0115] Synthesis of sulfide electrolyte precursor: LiBr, Li2S, and P2S5 were mixed in a molar ratio of 1:2.5:0.5, and then ball-milled at 500 rpm for 16 h using a high-energy ball mill to form the precursor of sulfide electrolyte Li6PS5Br.
[0116] The Li6PS5Br precursor was sealed and sintered at 600℃ for 3 hours to obtain Li6PS5Br6.
[0117] Comparative Example 8
[0118] Synthesis of sulfide electrolyte precursor: LiI, Li₂S, and P₂S₅ were mixed in a molar ratio of 1:2.5:0.5, and then ball-milled at 400 rpm for 12 h using a high-energy ball mill to form the precursor of the sulfide electrolyte Li₆PS₅I. The Li₆PS₅I precursor was then sintered in a sealed container at 530 °C for 6 h to obtain Li₆PS₅I₆. Comparative Example 9
[0119] 9.1 Synthesis of sulfide electrolyte raw materials: LiCl, Li2S and P2S5 were mixed in a molar ratio of 1:2.5:0.5 and then ball-milled at 100 rpm for 30 min to form a mixture of raw materials.
[0120] 9.2 Electrolyte sintering: The above raw material mixture was sealed and sintered at 530°C for 6 h to obtain sulfide electrolyte.
[0121] Simultaneously, the composition of the obtained electrolyte was quantitatively analyzed. In the composition analysis, the proportion of phosphorus (P) in the electrolyte was set to 1.
[0122] The theoretical composition of the electrolyte in this comparative example is Li6PS5Cl. After actual measurement using the above method, the actual composition of the electrolyte is Li. 5.256 PS 4.69 Cl 0.876It can be seen that due to the loss of P2S5 during sintering, the S element ratio deviates from the theoretical value by 0.31, which is much higher than the deviation in Example 8.
[0123] The samples obtained in Examples 1-7 and Comparative Examples 1, 3-8 were tested according to the following method: Weigh 0.1 g of the above electrolyte powder and press it into a cylindrical block with a diameter of 10 mm under a pressure of 200 MPa. Attach 10 mm diameter lithium metal discs to both sides. Use a charge-discharge tester to test the charge at 0.1 mA / cm². 2 Deposited at a current density of -0.1 mA / cm for 0.5 h, then at -0.1 mA / cm 2 The electrolyte was deposited at a current density of 0.5 h for 0.5 h, and this process was repeated to test the stability of the electrolyte to lithium metal, and to simulate the stability of the electrolyte under lithium plating conditions of the negative electrode active material. Because the sulfide electrolyte decomposes upon contact with lithium metal to produce a transition layer with low ionic conductivity, the ionic conductivity decreases, which manifests as an increase in polarization voltage during the test. Therefore, the test was terminated when the polarization voltage exhibited by the battery structure was 120% of the initial polarization voltage, and the time was recorded. The results are shown in Table 2.
[0124] Table 2 Electrolyte performance test results
[0125] As shown in Table 1, the time it took for the polarization voltage to reach 120% of the initial polarization voltage in the comparative examples was shorter than that in the examples, indicating that the electrolyte obtained in the examples has higher stability on the negative electrode side.
[0126] This is caused by the following reasons: Comparative Example 1 is the original Li6PS5Cl6 electrolyte, without any modification or protection. When the Li6PS5Cl electrolyte comes into contact with lithium metal, it decomposes into LiCl, Li3P, and Li2S, which in turn causes the electrolyte conductivity to decrease continuously and the interface to deteriorate continuously.
[0127] Combination Figure 3 The characterization results of the XPS surface chemical bonds of Example 1 and Comparative Example 1 show that Example 1 has a characteristic peak of F- at 685 eV, while Comparative Example 1 does not have this characteristic peak, indicating that the F element in Example 1 has undergone elemental substitution on the surface of the electrolyte particles.
[0128] Comparative Example 3 shows an electrolyte coated only with F. Compared to the electrolyte in Example 1, which was coated with a mixture of C and F, lithium metal more readily attacks coating defects, resulting in lower performance than Example 1. (Lithium metal tends to attack interfaces with a mixture of high electronic and ionic conductivity (this is because the two necessary conditions for the formation of elemental lithium are the simultaneous presence of lithium ions and electrons). Therefore, lithium deposition often occurs at coating defects (providing ion sites), leading to lithium deposition at coating defects in the electrolyte and causing degradation of the incompletely coated areas in contact with lithium metal.)
[0129] Comparative Example 4 shows an electrolyte coated only with carbon (C). Compared to an electrolyte coated with a mixture of C and sulfur (F), its resistance to lithium is even worse. This is because sulfur (F) is a highly electronegative anionic element that can quickly react with deposited lithium metal to form LiF. This process consumes the deposited lithium while protecting the sulfide electrolyte from lithium metal attack, and the resulting LiF layer remains an inert layer for lithium metal.
[0130] Comparative Example 5 involved mechanically mixing polyvinylidene fluoride (PVDF) with a sulfide electrolyte, rather than dissolving and re-precipitating the organic compound. This resulted in point-to-point contact between the organic compound and the electrolyte, rather than the surface-to-surface contact observed in Example 1. Consequently, the coating in Comparative Example 5 was a dotted coating, and its coating effect was inferior to that in Example 1.
[0131] Comparative Example 6 involves coating an organic compound onto a sintered sulfide electrolyte and then sintering it to degrade it, rather than degrading the organic compound while sintering the electrolyte precursor as in Example 1. As a result, the bonding ability between the coating layer and the sulfide electrolyte in Comparative Example 6 is lower than that in Example 1, which is reflected in the resistance to the stability of the negative electrode.
[0132] In summary, the present invention achieves a more uniform coating of the electrolyte precursor by liquid phase coating (compared to ball milling, the method of the present invention makes the coating more uniform and completely coats the electrolyte as much as possible); and can coat the electrolyte surface in situ during the electrolyte synthesis process, making the coating layer more firmly bonded to the electrolyte itself (instead of conventional coating methods, which use external mechanical force such as ball milling, resulting in a loose bond between the coating layer and the sulfide electrolyte).
[0133] Compared to conventional solid-phase coating methods such as ball milling and ALD, the coating method of the present invention has a larger single-batch processing capacity, fewer equipment limitations, and is easier to achieve large-scale production.
[0134] Compared to traditional methods of coating sulfide electrolytes with phosphorus (F), such as mixing LiF or fluoride salts with the sulfide electrolyte to construct the coating layer, this invention addresses the challenge of F being the most electronegative member of the halogens. F anions have a strong binding energy with metal cations, making them difficult to react with the sulfide electrolyte. Furthermore, traditional methods of mixing fluoride salts with sulfide electrolytes often involve simply mixing the two together, rather than generating F on the surface of the sulfide electrolyte through an in-situ reaction, as in this invention. In this invention, the coating layer bonds more tightly to the substrate, forming a continuous whole.
Claims
1. A sulfide electrolyte suitable for the negative electrode side of an all-solid-state battery, characterized in that, The system includes a matrix and a coating layer covering the matrix; the matrix is a sulfide solid electrolyte; the coating layer contains pyrolysis products of a polymer; the polymer is selected from polymers containing the element F; the polymer containing the element F is composed of elements C, F and H or elements C, F, H and A; the element A is selected from one or more of elements Cl, Br and I. The method for preparing the sulfide electrolyte includes the following steps: S1) The sulfide solid electrolyte precursor is mixed with the coating solution and dried to obtain a polymer-coated precursor; the coating solution includes a polymer; the polymer is selected from polymers with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide or polymers containing the element F. S2) The polymer-coated precursor is sintered to obtain a sulfide electrolyte; the sintering temperature is higher than the polymer pyrolysis temperature and the crystallization temperature of the sulfide solid electrolyte precursor.
2. The sulfide electrolyte according to claim 1, characterized in that, The mass ratio of the F element to the matrix in the polymer containing the F element is 0.0005~0.01:
1.
3. The sulfide electrolyte according to claim 1, characterized in that, The polymer containing the F element is selected from one or more of polychlorotrifluoroethylene, polyvinylidene fluoride, ethylene-vinylidene fluoride copolymer, ethylene-chlorotrifluoroethylene copolymer, polyvinylidene fluoride and polyhexafluoroisobutylene; The sulfide solid electrolyte is Li with X replaced by F on its surface. 7-a PS 6-a X a , where 1≤a≤2, and X is Cl, Br or I.
4. The sulfide electrolyte according to claim 1, characterized in that, The precursor of the sulfide solid electrolyte is prepared according to the following steps: LiX, Li2S and P2S5 were mixed and ball-milled to obtain a sulfide solid electrolyte precursor; wherein X is Cl, Br or I. When the polymer is a polymer with a pyrolysis temperature greater than the sublimation temperature of phosphorus pentasulfide, the rotation speed of the mixing ball mill is 100~200 rpm; the mixing ball milling time is 10~60 min. When the polymer is a polymer containing the element F, the rotation speed of the mixing ball mill is 300~600 rpm; the mixing ball milling time is 6~24 h.
5. The sulfide electrolyte according to claim 1, characterized in that, The polymer concentration in the coating solution is 0.1% to 2% by mass. The solvent in the coating solution is selected from one or more of benzene-based solvents, nitrile solvents, and ketone solvents.
6. The sulfide electrolyte according to claim 1, characterized in that, The sintering temperature is 380℃~600℃; the sintering time is 3~10 h.
7. An all-solid-state battery, characterized in that, Includes the sulfide electrolyte according to any one of claims 1 to 6.
Citation Information
Patent Citations
Sulfide electrolyte membrane as well as preparation method and application thereof
CN113782824A
Lithium sulfide coated sulfide solid electrolyte as well as preparation method and application thereof
CN114524416A
Core-shell sulfide solid electrolyte, preparation method and all-solid-state battery
CN116072961A
Composite electrolyte film for all-solid-state lithium metal negative electrode battery, preparation method of composite electrolyte film and all-solid-state sulfide lithium ion battery comprising composite electrolyte film
CN112599846A
Element-doped sulfide solid electrolyte with coating layer and preparation method thereof
CN115995600A