Atomically dispersed nickel-based catalyst and its preparation method and application
By using atomic dispersed nickel-based catalysts in lithium oxygen batteries, the problem of insufficient electrochemical performance is solved. By distributing nickel single atoms and nickel clusters on graphene oxide and introducing nitrogen elements, catalytic performance and cell stability are improved. The performance improvement of lithium oxygen batteries has been achieved.
Patent Information
- Application Number
- CN202311386641.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-10-24
AI Technical Summary
The electrochemical performance of existing lithium oxygen batteries has not reached a satisfactory level on the positive and negative electrode sides, especially the problems of slow oxygen reduction/oxygen precipitation reaction kinetics, accumulation of discharge products lead to passivation, and lithium metal corrosion. The existing catalysts cannot be effective. Improve battery performance.
Using atomic-scale dispersed nickel-based catalyst, the catalytic properties and affinity for lithium are improved by uniformly distributing metal nickel single atoms and nickel clusters on reduced graphene oxide and introducing nitrogen elements. , at the same time, the contact area between the electrode and the electrolyte is increased, and the transmission path of ions and electrons is shortened.
Significantly reduce the charging overpotential, increase the discharge capacity, improve the cycle life and cycle stability of the battery, delay the corrosion of lithium metal, and improve battery safety. It is suitable for the positive and negative electrode materials of lithium oxygen batteries.
Smart Images

Figure CN117638329B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of energy storage materials, and in particular to an atomic-level dispersed nickel-based catalyst and a preparation method and application thereof. Background Art
[0002] As traditional fossil energy is gradually depleted, lithium-oxygen batteries have become popular due to their high theoretical specific energy density (3500Wh kg -1 ) has attracted increasing attention from researchers. With an energy density 10 times higher than that of the most advanced lithium-ion batteries, it is considered to be the most promising new generation energy storage system and can be widely used in large-scale or long-term power consumption equipment such as electric vehicles.
[0003] A typical non-aqueous lithium-oxygen battery consists of a metallic lithium negative electrode, a porous oxygen positive electrode including a gas diffusion layer and a catalyst, and an electrolyte containing lithium ions. During the battery discharge process, the system undergoes an oxygen reduction reaction, that is, lithium ions are stripped from the lithium metal negative electrode and diffused to the positive electrode side, and react chemically with oxygen passing through the gas diffusion layer to produce an intermediate product LiO2 and a final discharge product Li2O2; and as a secondary battery, during the subsequent charging process of the lithium-oxygen battery, an oxygen evolution reaction occurs, that is, the discharge product Li2O2 is reversibly converted into lithium ions and oxygen.
[0004] As a unique semi-open battery system, the development of lithium-oxygen actually faces huge obstacles, such as on the negative electrode: the formation of lithium dendrites, the generation of dead lithium, and the serious corrosion of lithium metal by electrolyte / air; on the electrolyte: the nucleophilic attack of the intermediate super radical ions on the electrolyte; on the positive electrode: the slow oxygen reduction / oxygen evolution reaction kinetics, passivation caused by the accumulation of discharge products, etc.
[0005] In order to solve the above problems, in terms of positive electrode, researchers are committed to exploring efficient electrocatalysts with good oxygen reduction / oxygen evolution reaction kinetics. The current achievements are mainly concentrated in carbon materials, precious metals, transition metal oxides, metal nitrides, metal sulfides and metal carbides. At the same time, in terms of negative electrode, various stabilization strategies have been proposed, such as constructing a new type of replaceable lithium-containing negative electrode, applying electrolyte additives / modification and constructing a protective layer. In recent years, single-atom catalysts with characteristics including high atomic utilization and unsaturated coordination structure have attracted great attention in the field of catalysis and have been widely used in batteries, electrocatalysis, biomedicine and other fields. As a system determined by catalytic reactions, the application of single-atom catalysts in lithium-oxygen batteries has begun, and the results show that the electrochemical performance of the battery system has been significantly improved. For example, Chinese patent document CN111224087A discloses a carbon composite material loaded with transition metal single atoms and its preparation method and application, which is used as a positive electrode material for lithium-oxygen batteries, which can reduce the charge and discharge overpotential, improve the battery energy conversion efficiency, inhibit side reactions, and improve the battery cycle stability. For another example, Chinese patent document CN116230973A discloses a Co-Pd diatomic cathode catalyst for lithium-air batteries, a preparation method and an application thereof. The lithium-oxygen battery constructed using the cathode material exhibits a low charging platform (3.2V) and a low overpotential (0.6V), solving the high overpotential problem (1.5V) commonly found in lithium-oxygen batteries; and has a high discharge platform (2.8V) and a good discharge capacity (15000mAh g -1 ). At the same time, single-atom catalysts are also applied to the negative electrode side of the battery. For example, Chinese patent document CN116374997A discloses a carbon-based composite negative electrode material and its preparation method and application. The invention coats an artificial SEI film on the surface of a carbon nano-substrate deposited with fluorine, and uses magnetron sputtering, electrostatic spinning or in-situ growth technology to add a single-atom catalyst on the surface of the artificial SEI film, so that the negative electrode can stably and effectively exert its capacity while also extending the battery life.
[0006] However, the electrochemical performance of lithium-oxygen batteries reported on this basis is still unsatisfactory and there is still a large gap from practical application. At the same time, the negative electrode of lithium-oxygen batteries also faces various problems due to their complex system.
[0007] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0008] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide an atomically dispersed nickel-based catalyst and a preparation method and application thereof, aiming to solve the problem that the existing electrocatalysts cannot effectively improve the electrochemical performance of the positive and negative electrode sides of lithium-oxygen batteries.
[0009] The technical solution of the present invention is as follows:
[0010] An atomically dispersed nickel-based catalyst comprises: a substrate, and metal nickel single atoms and / or nickel clusters supported on the substrate; the substrate is reduced graphene oxide; and the reduced graphene oxide is doped with nitrogen.
[0011] The atomically dispersed nickel-based catalyst, wherein the reduced graphene oxide is in granular form; the particle size of the reduced graphene oxide is 0.2 μm-10 μm.
[0012] The atomically dispersed nickel-based catalyst, wherein the total size of the nickel clusters and the size of the metal nickel single atom are both less than 1 nm.
[0013] The atomically dispersed nickel-based catalyst, wherein the total mass of the nickel single atoms and the nickel clusters is 0.038wt%-0.811wt% of the atomically dispersed nickel-based catalyst.
[0014] The atomically dispersed nickel-based catalyst, wherein the mass percentage of nitrogen element doped in the reduced graphene oxide is 1.37wt%-3.20wt%.
[0015] A method for preparing an atomically dispersed nickel-based catalyst comprises the following steps:
[0016] Mixing a nickel salt solution, water, and an aqueous solution of graphene oxide to obtain a precursor solution;
[0017] The precursor solution is transferred to a reactor for hydrothermal reaction to obtain a black gel;
[0018] The black gel is annealed in an atmosphere containing nitrogen to obtain the atomic-level dispersed nickel-based catalyst.
[0019] The method for preparing the atomic-level dispersed nickel-based catalyst, wherein the temperature of the hydrothermal reaction is 170° C.-190° C., and the time of the hydrothermal reaction is 5 h-7 h.
[0020] The method for preparing the atomically dispersed nickel-based catalyst, wherein the annealing temperature is 850°C-950°C, the annealing time is 0.5h-1.5h, and the heating rate of the annealing is 4°C min -1 -6℃min -1 .
[0021] Application of an atomically dispersed nickel-based catalyst in lithium-oxygen battery cathode materials.
[0022] Application of an atomically dispersed nickel-based catalyst in lithium-oxygen battery negative electrode materials.
[0023] Beneficial effects: The present invention provides an atomic-level dispersed nickel-based catalyst and a preparation method and application thereof. The atomic-level dispersed nickel-based catalyst comprises: a matrix, metal nickel single atoms and / or nickel clusters loaded on the matrix; the matrix is reduced graphene oxide; the reduced graphene oxide is doped with nitrogen. The present invention utilizes the active sites of metal nickel single atoms and / or nickel clusters to be evenly distributed between the carbon matrix, and at the same time introduces nitrogen elements to increase the degree of internal defects of the material, form a coordination structure with the metal nickel sites, generate regional activity, and enhance the catalytic performance of the material and its affinity for lithium. In addition, the atomic-level dispersed nickel-based catalyst has a rich pore structure and specific surface area, which increases the contact area between the electrode and the electrolyte, shortens the transmission path of ions and electrons, effectively improves the three-phase interface problem, and also provides more sites for the accommodation of discharge products. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A schematic diagram of a process flow of a method for preparing an atomically dispersed nickel-based catalyst according to the present invention;
[0025] Figure 2 The spherical aberration transmission electron microscopy image of the atomically dispersed nickel-based catalyst prepared in Examples 1-4;
[0026] Figure 3 The extended X-ray absorption fine structure image of the atomically dispersed nickel-based catalyst prepared in Example 2;
[0027] Figure 4 The first cycle discharge capacity curve of the lithium oxygen battery using the atomically dispersed nickel-based catalyst as the positive electrode prepared in Example 1-4;
[0028] Figure 5 The charge and discharge performance curve of a lithium oxygen battery using an atomically dispersed nickel-based catalyst as a positive electrode prepared in Example 2;
[0029] Figure 6 The cycle stability curve of the lithium oxygen battery using the atomically dispersed nickel-based catalyst as the positive electrode prepared in Example 2;
[0030] Figure 7 This is a cycle stability curve diagram of a lithium-oxygen battery with an atomically dispersed nickel-based catalyst positive electrode and a composite lithium metal negative electrode prepared in Example 2. DETAILED DESCRIPTION
[0031] The present invention provides an atomic-level dispersed nickel-based catalyst and a preparation method and application thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0032] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as generally understood by those skilled in the art in the art to which the present invention belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined as herein.
[0033] The present invention provides an atomic-level dispersed nickel-based catalyst, comprising: a substrate, metal nickel single atoms and / or nickel clusters loaded on the substrate; the substrate is reduced graphene oxide; the reduced graphene oxide is doped with nitrogen.
[0034] In this embodiment, the active sites of nickel metal atoms and / or nickel clusters are evenly distributed between the carbon matrix, and nitrogen elements are introduced to increase the degree of internal defects of the material, so that the nickel metal and the nitrogen elements form a coordination structure, generate regional activity, and enhance the catalytic performance of the material and the affinity for lithium. In addition, the atomically dispersed nickel-based catalyst provided by the present invention has a rich pore structure and specific surface area, increases the contact area between the electrode and the electrolyte, shortens the transmission path of ions and electrons, effectively improves the three-phase interface problem, and also provides more sites for the accommodation of discharge products.
[0035] Specifically, the atomically dispersed nickel-based catalyst is used as a positive electrode material for lithium-oxygen batteries, which can significantly reduce the charge overpotential, increase the discharge capacity, and improve the cycle life of the battery; at the same time, it is applied to a composite lithium metal negative electrode prepared from lithium metal, which gives the lithium-oxygen battery good high-rate cycle stability, effectively delays the corrosion of the battery system to the lithium metal, and improves safety. Therefore, the atomically dispersed nickel-based catalyst solves or suppresses the problems of the positive electrode and welfare side of the lithium-oxygen battery at the same time, and is cost-effective, which is of extremely important practical significance for realizing its practical application.
[0036] In some embodiments, the reduced graphene oxide is in granular form; the particle size of the reduced graphene oxide is 0.2 μm-10 μm. Controlling the particle size of the reduced graphene oxide between 0.2 μm and 10 μm can effectively make the atomically dispersed nickel-based catalyst have a rich pore structure and specific surface area, thereby increasing the contact area between the electrode and the electrolyte, thereby shortening the transmission path of ions and electrons, effectively improving the three-phase interface problem, and also providing more sites for the accommodation of discharge products.
[0037] In some embodiments, the atomically dispersed nickel-based catalyst may be, but is not limited to, Ni1-N / rGO, Ni2-N / rGO, Ni3-N / rGO, and Ni4-N / rGO depending on the content difference of the catalytic active sites.
[0038] In some embodiments, the total size of the nickel clusters and the size of the single metal nickel atom are both less than 1 nm, and the smaller size gives it greater atomic utilization and higher catalytic activity.
[0039] In some embodiments, the total mass of the nickel atoms and the nickel clusters is 0.038wt%-0.811wt% of the atomically dispersed nickel-based catalyst. Different mass fractions correspond to different states of existence of the element. When extremely low content of metal nickel atoms and / or nickel clusters are loaded on the substrate, when the atomically dispersed nickel-based catalyst is used as a positive electrode material for a lithium-oxygen battery, the charging overpotential can be significantly reduced, the discharge capacity can be increased, and the cycle life of the battery can be improved; and when the atomically dispersed nickel-based catalyst is loaded on the surface of lithium metal to prepare a composite lithium metal negative electrode, the lithium-oxygen battery can be endowed with good high-rate performance and cycle stability, which effectively delays the corrosion of the battery system to the lithium metal and improves safety.
[0040] In some embodiments, the mass percentage of nitrogen doped in the reduced graphene oxide is 1.37wt%-3.20wt%. Doping the reduced graphene oxide with a nitrogen content of 1.37wt%-3.20wt% can effectively increase the internal defect level of the carbon material, form a coordination structure with the metal nickel site, thereby generating regional activity, and further enhancing the catalytic performance of the material and its affinity for lithium.
[0041] In addition, Figure 1 As shown, the present invention also provides a method for preparing an atomically dispersed nickel-based catalyst, comprising the steps of:
[0042] Step S10: mixing a nickel salt solution, water, and a graphene oxide aqueous solution to obtain a precursor solution;
[0043] Step S20: transferring the precursor solution to a reaction vessel for hydrothermal reaction to obtain a black gel;
[0044] Step S30: annealing the black gel in an atmosphere containing nitrogen to obtain the atomic-level dispersed nickel-based catalyst.
[0045] In this embodiment, nickel salt and graphene carbon material are used as raw materials, and a simple hydrothermal reaction-high temperature thermal reduction treatment method is adopted to obtain a carbon composite material of metal single atoms / clusters, that is, the atomically dispersed nickel-based catalyst. In the atomically dispersed nickel-based catalyst prepared by this method, the metal nickel sites are evenly distributed between the reduced graphene oxide, and the nitrogen element is introduced at the same time, which increases the degree of internal defects of the material, forms a coordination structure with the metal nickel sites, generates regional activity, and enhances the catalytic performance of the material and the affinity for lithium.
[0046] Furthermore, the preparation method provided by the present invention has the advantages of simple and easy-to-control preparation process, low energy consumption, wide source of raw materials, low cost, green and environmental protection, etc. The existence form of active sites in the material can be regulated according to the content of the precursor, so it also has the characteristics of flexibility and strong practicality, and realizes the batch and rapid synthesis of atomically dispersed nickel-based catalysts, which is suitable for large-scale industrial production; in addition, the atomically dispersed nickel-based catalyst is applied to the positive and negative electrode sides of lithium-oxygen batteries for the first time, and achieved good results, with obvious prospects for industrial application.
[0047] Specifically, the atomically dispersed nickel-based catalyst prepared by this preparation method has a rich pore structure and specific surface area, which increases the contact area between the electrode and the electrolyte, shortens the transmission path of ions and electrons, effectively improves the three-phase interface problem, and also provides more sites for the accommodation of discharge products.
[0048] In some embodiments, before step S10, the method further includes: pre-treating the graphene oxide aqueous solution by ultrasonic treatment for 3 hours.
[0049] In some embodiments, the temperature of the hydrothermal reaction is 170° C.-190° C., and the time of the hydrothermal reaction is 5 h-7 h.
[0050] In a preferred embodiment, the temperature of the hydrothermal reaction is 180° C., and the time of the hydrothermal reaction is 6 hours.
[0051] In some embodiments, the annealing temperature is 850°C-950°C, the annealing time is 0.5h-1.5h, and the heating rate of the annealing is 4°C min -1 -6℃min -1 .
[0052] In a preferred embodiment, the annealing temperature is 900°C, the annealing time is 1h, and the heating rate of the annealing is 4°C min -1 -6℃min -1 .
[0053] Under the hydrothermal reaction conditions and annealing treatment conditions, an atomically dispersed nickel-based catalyst can be obtained in which metal nickel sites are uniformly distributed among the matrix.
[0054] In some embodiments, in step S30, the annealing treatment is performed in an atmosphere of a mixed gas of Ar and NH3, and the flow rate of the mixed gas is controlled at 100 ml min -1 Preferably, the annealing treatment is carried out in an atmosphere of a mixed gas of Ar (150 sccm) and NH3 (50 sccm).
[0055] Specifically, the preparation method of the atomic-level dispersed nickel-based catalyst includes the following steps: adding a certain amount of nickel salt solution and deionized water in a certain proportion to the pretreated graphene oxide aqueous solution, and obtaining a uniform and stable precursor solution after ultrasonication and stirring; then transferring the precursor solution to a hydrothermal reactor, and obtaining a black gel after hydrothermal reaction and deionization soaking and washing three times; finally, freeze-drying the black gel for 72 hours to remove the entrained moisture, and then transferring it to a tubular furnace for high-temperature annealing treatment, and cooling it to room temperature to obtain the atomic-level dispersed nickel-based catalyst.
[0056] In addition, the present invention also provides an application of an atomic-level dispersed nickel-based catalyst in a lithium-oxygen battery positive electrode material.
[0057] And, the application of an atomically dispersed nickel-based catalyst in the negative electrode material of lithium-oxygen batteries.
[0058] In this embodiment, when the atomically dispersed nickel-based catalyst is used as a catalytic positive electrode, the oxygen reduction / oxygen evolution reaction kinetics are accelerated, the generation / decomposition efficiency of lithium peroxide is improved, and it is beneficial to improve the electrochemical performance of the lithium oxygen battery. At a current of 200mA / g, the first cycle discharge capacity of the lithium oxygen battery with a catalytic positive electrode is as high as 18000mAh / g, and the overpotential is only 1.08V, and it can be stably cycled for 225 cycles under the restriction of 500mAh / g-200mA / g. When the atomically dispersed nickel-based catalyst is applied to the surface of lithium metal to prepare a composite lithium metal as a negative electrode material, the direct contact between the lithium oxygen battery electrolyte and the lithium metal is hindered, and the corrosion of the electrolyte and intermediate products to lithium is reduced, giving the lithium oxygen battery good high-rate cycle stability, so that it can be stably cycled for more than 300 cycles under the high current restriction of 500mAh / g-500mA / g.
[0059] In some embodiments, when the atomically dispersed nickel-based catalyst is used as a positive electrode material in a lithium-oxygen battery, the steps are specifically included:
[0060] Step S1: mixing the atomically dispersed nickel-based catalyst with a conductive agent, a binder, and a solvent to obtain a slurry;
[0061] Step S2: applying the slurry on a carbon paper substrate and vacuum drying to obtain a positive electrode sheet;
[0062] Step S3: Assemble the positive electrode plate into a battery, use metallic lithium as the negative electrode, glass fiber film as the separator, and assemble it into a button battery with the electrolyte.
[0063] In this embodiment, in step S1, Ketjen black is used as a conductive agent, 6% polytetrafluoroethylene is used as a binder, and isopropyl alcohol solution is used as a solvent; the mass ratio of the atomically dispersed nickel-based catalyst to the conductive agent and the binder is 6:3:1. The mass ratio of the total mass of the atomically dispersed nickel-based catalyst and the conductive agent to the mass ratio of isopropyl alcohol is 1:140.
[0064] In some embodiments, in the positive electrode sheet, the active material loading of each positive electrode sheet is 0.15-0.2 mg / cm 2 ; A solution of lithium bis(trifluoromethanesulfonate)imide dissolved in tetraethylene glycol dimethyl ether was used as the electrolyte with a concentration of 1 mol / L; the amount of the electrolyte used was 230 μL.
[0065] In some embodiments, when the atomically dispersed nickel-based catalyst is used as a negative electrode material in a lithium oxygen battery, the method specifically includes the following steps: mixing the atomically dispersed nickel-based catalyst with a conductive agent and a solvent to obtain a mixed solution; applying the mixed solution on the surface of a lithium sheet, and drying to obtain a composite lithium metal with a protective layer; using the composite lithium metal as the negative electrode, the positive electrode sheet prepared in the above step S3 as the positive electrode, and a glass fiber film as a diaphragm, and assembling them with an electrolyte into a button battery.
[0066] Furthermore, when preparing composite lithium metal, the conductive agent is Ketjen black, and the solvent is tetraethylene glycol dimethyl ether; the mass ratio of the atomically dispersed nickel-based catalyst to the conductive agent is 2:1, and the mass ratio of the total mass of the atomically dispersed nickel-based catalyst and Ketjen black to tetraethylene glycol dimethyl ether is 1:140; a solution of lithium bis(trifluoromethylsulfonic acid) imide dissolved in tetraethylene glycol dimethyl ether is used as the electrolyte, and the concentration is 1 mol / L; the amount of the electrolyte used is 230 μL.
[0067] The following examples are further given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention.
[0068] Example 1
[0069] Unless otherwise specified, all raw materials in the examples are conventional raw materials and can be obtained commercially; the methods used in the examples are all prior art unless otherwise specified.
[0070] Among them, nickel chloride hexahydrate was purchased from Aladdin; graphene oxide was purchased from Suzhou Carbonfeng Graphene Technology Co., Ltd.
[0071] Examples 1-4
[0072] Examples 1-4 respectively provide an atomically dispersed nickel-based catalyst. The difference between Examples 1-4 is that the amount of nickel salt solution added is different. The specific preparation method thereof comprises the following steps:
[0073] 1. Dissolve 50 mg NiCl2·6H2O in 50 mL deionized water and stir magnetically for 1 h until completely dissolved to obtain a nickel salt solution; as shown in the following table, add a certain amount of the above nickel salt solution and deionized water in a certain proportion to 50 mL of graphene oxide aqueous solution that had been ultrasonically treated for 3 h, and then stir magnetically for 0.5 h and ultrasonically for 0.5 h to obtain four uniform and stable precursor solutions for standby use.
[0074] Example 1 Example 2 Example 3 Example 4 Nickel salt solution (mL) 0.16 0.32 2.76 22.13 Deionized water (mL) 29.84 29.68 27.24 7.87
[0075] 2. The above four precursor solutions were transferred to the hydrothermal reactor respectively, sealed and placed in a forced air drying oven, and hydrothermally reacted at 180°C for 6 hours to obtain black cylindrical regular gel samples. The above samples were soaked and washed with deionized water three times, each time for 30 minutes, and set aside.
[0076] 3. The cleaned black gel sample was freeze-dried for 72 h to remove the impurities, and then transferred to a tube furnace for high temperature annealing treatment at 5 °C min in an Ar (150 sccm) / NH3 (50 sccm) atmosphere. -1 The temperature was raised to 900°C at a heating rate and calcined at high temperature for 1 hour. The flow rate of the mixed gas was 100 ml min -1 , cooled to room temperature, and obtained Ni1-N / rGO of Example 1, Ni2-N / rGO of Example 2, Ni3-N / rGO of Example 3, and Ni4-N / rGO of Example 4, respectively.
[0077] The spherical aberration transmission electron microscopy images of the atomically dispersed nickel-based catalysts prepared in Examples 1-4 are as follows: Figure 2As shown, a is the spherical aberration transmission electron micrograph of the atomically dispersed nickel-based catalyst Ni1-N / rGO prepared in Example 1. It can be seen from the figure that Ni is uniformly dispersed in the entire graphene carbon material matrix in the form of single atoms; b is the spherical aberration transmission electron micrograph of the atomically dispersed nickel-based catalyst Ni2-N / rGO prepared in Example 2. It can be seen from the figure that Ni is uniformly dispersed in the entire graphene carbon material matrix in the form of coexistence of single atoms and clusters, but the single atomic form is the majority; c is the spherical aberration transmission electron micrograph of the atomically dispersed nickel-based catalyst Ni3-N / rGO prepared in Example 3. It can be seen from the figure that Ni is uniformly dispersed in the entire graphene carbon material matrix in the form of coexistence of single atoms and clusters, but the cluster form increases; d is the spherical aberration transmission electron micrograph of the atomically dispersed nickel-based catalyst Ni4-N / rGO prepared in Example 4. It can be seen from the figure that Ni is uniformly dispersed in the entire graphene carbon material matrix in the form of clusters.
[0078] The extended X-ray absorption fine structure of the atomically dispersed nickel-based catalyst Ni2-N / rGO prepared in Example 2 is shown in FIG. Figure 3 As shown, from Figure 3 It can be seen that the bonding in the atomically dispersed nickel-based catalyst is mostly Ni-N coordination, with a small amount of Ni-Ni coordination and no Ni-O coordination, which further confirms that Ni exists in the form of coexistence of single atoms and clusters.
[0079] The atomically dispersed nickel-based catalyst prepared in Examples 1-4 is used as a catalytic positive electrode material in a lithium-oxygen battery, and the specific steps are as follows:
[0080] Preparation of positive electrode sheets for lithium oxygen batteries: The atomically dispersed nickel-based catalyst prepared in Example 1-4, the conductive agent Ketjen black, and the 6% polytetrafluoroethylene binder are independently dispersed in an isopropanol solution in a mass ratio of 6:3:1, wherein the mass ratio of the atomically dispersed nickel-based catalyst to Ketjen black and to isopropanol is 1:140, and magnetic stirring is performed for 0.5 h and ultrasonication is performed for 3 h to obtain a uniform slurry; 50 μL of the above slurry is evenly applied on a carbon paper substrate, and vacuum dried at 90 ° C for 12 h to obtain a positive electrode sheet, and the active material loading of each positive electrode sheet is 0.15-0.2 mg / cm 2 .
[0081] Lithium oxygen battery assembly and testing: The obtained positive electrode plates were assembled in a glove box filled with high-purity argon gas, with H2O and O2 contents less than 0.1ppm. Metal lithium (purity>99.9%) was used as the negative electrode, glass fiber film (GF / D) was used as the diaphragm, and a solution of lithium bis(trifluoromethylsulfonyl)imide dissolved in tetraethylene glycol dimethyl ether was used as the electrolyte (concentration of 1 mol / L). The amount of electrolyte was 230μL, and CR2032 button cells were assembled. The assembled battery was transferred to the lithium oxygen battery test box, and after standing at room temperature for 3 hours, 1 atmosphere of oxygen was introduced, and then it was allowed to stand for 6 hours in an oxygen atmosphere, and then oxygen was introduced for the second time. The electrochemical performance of the lithium oxygen battery after the above treatment was tested. The test equipment was the Land battery test system (5V, 1mA), and the test voltage range was 2.0-4.5 / 5.0V.
[0082] The first cycle discharge capacity curve of the battery at a current density of 200 mA / g is as follows: Figure 4 As shown by Figure 4 It can be seen that the first-cycle discharge capacities of the lithium-oxygen batteries using the catalytic positive electrodes prepared in Examples 1-4 are 7000, 18000, 9500 and 2200 mAh / g, respectively.
[0083] The charge and discharge performance curve of the battery at a limited capacity of 500mAh / g and a current density of 100mA / g is as follows: Figure 5 As shown by Figure 5 It can be seen that the overpotential of the lithium-oxygen battery with the catalytic positive electrode prepared in Example 2 is only 1.08V.
[0084] The cycle stability curve of the battery at a limited capacity of 500mAh / g and a current density of 200mA / g is as follows Figure 6 As shown by Figure 6 It can be seen that the lithium-oxygen battery with the catalytic positive electrode prepared in Example 2 can be stably cycled for 225 times.
[0085] The atomically dispersed nickel-based catalyst prepared in Example 2 is used as a negative electrode material in a lithium-oxygen battery, and the specific steps are as follows:
[0086] Preparation of a composite lithium metal negative electrode for a lithium-oxygen battery: The atomically dispersed nickel-based catalyst prepared in Example 2 and the conductive agent Ketjen black are uniformly dispersed in tetraethylene glycol dimethyl ether in a mass ratio of 2:1, wherein the mass ratio of the atomically dispersed nickel-based catalyst to Ketjen black and to tetraethylene glycol dimethyl ether is 1:140, and magnetic stirring is performed for 0.5 h and ultrasound is performed for 3 h to obtain a uniform mixed solution; in a glove box filled with high-purity argon, 70 μL of the above mixed solution is evenly applied to the surface of the lithium sheet, and dried at 60°C for 12 h to obtain a composite lithium metal with a protective layer.
[0087] Lithium oxygen battery assembly and testing: The obtained composite lithium metal was assembled into a battery in a glove box filled with high-purity argon gas with H2O and O2 contents less than 0.1 ppm, with the composite lithium metal as the negative electrode. The rest of the assembly method and test conditions were the same as above.
[0088] The cycle stability curve of the battery at a limited capacity of 500mAh / g and a current density of 500mA / g is as follows: Figure 7 As shown by Figure 7 It can be seen that the lithium oxygen battery with a catalytic positive electrode and a composite lithium metal negative electrode prepared in Example 2 can be stably cycled for more than 300 times.
[0089] In summary, the present invention provides an atomic-level dispersed nickel-based catalyst and its preparation method and application. The atomic-level dispersed nickel-based catalyst includes: a matrix, metal nickel atoms and / or nickel clusters loaded on the matrix; the matrix is reduced graphene oxide; the reduced graphene oxide is doped with nitrogen. The present invention utilizes the active sites of metal nickel atoms and / or nickel clusters to be evenly distributed between the carbon matrix, and at the same time introduces nitrogen elements to increase the degree of internal defects of the material, form a coordination structure with the metal nickel sites, generate regional activity, and enhance the catalytic performance of the material and its affinity for lithium. In addition, the atomic-level dispersed nickel-based catalyst has a rich pore structure and specific surface area, which increases the contact area between the electrode and the electrolyte, shortens the transmission path of ions and electrons, effectively improves the three-phase interface problem, and also provides more sites for the accommodation of discharge products.
[0090] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing an atomically dispersed nickel-based catalyst, characterized in that: Includes steps: Mixing a nickel salt solution, water, and an aqueous solution of graphene oxide to obtain a precursor solution; The precursor solution is transferred to a reactor for hydrothermal reaction to obtain a black gel; Annealing the black gel in an atmosphere of a mixed gas of Ar and NH3 to obtain the atomically dispersed nickel-based catalyst; The temperature of the hydrothermal reaction is 170°C-190°C, and the time of the hydrothermal reaction is 5h-7h; the temperature of the annealing treatment is 850°C-950°C, and the time of the annealing treatment is 0.5h-1.5h, and the heating rate of the annealing treatment is 4°C min -1 -6℃min -1 ; The flow rate of the mixed gas is 100min -1 ; The atomically dispersed nickel-based catalyst includes a substrate, nickel single atoms and / or nickel clusters supported on the substrate; the substrate is reduced graphene oxide; the reduced graphene oxide is doped with nitrogen; the reduced graphene oxide is granular; the particle size of the reduced graphene oxide is 0.2μm-10μm; the total size of the nickel clusters and the size of the nickel single atoms are both less than 1nm; the total mass of the nickel single atoms and the nickel clusters is 0.038wt%-0.811wt% of the atomically dispersed nickel-based catalyst; the mass percentage of the nitrogen element doped in the reduced graphene oxide is 1.37wt%-3.20wt%.
2. An application of the atomically dispersed nickel-based catalyst prepared by the method for preparing the atomically dispersed nickel-based catalyst as claimed in claim 1 in a positive electrode material for a lithium-oxygen battery.
3. Use of the atomically dispersed nickel-based catalyst prepared by the method for preparing the atomically dispersed nickel-based catalyst as claimed in claim 1 in negative electrode materials for lithium-oxygen batteries.