A metal reflector and a method for electroless plating of nickel-phosphorus alloy on its surface.
By using C18150 chromium zirconium copper alloy and electroless nickel-phosphorus alloy plating process, the problems of uneven modified layer thickness, surface defects and poor polishability of metal mirrors were solved, achieving a high gloss and stable mirror surface, and improving optical performance and processing accuracy.
Patent Information
- Application Number
- CN202311642336.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-04
AI Technical Summary
In the existing technology, the modified layer of metal mirrors has uneven thickness, fine defects on the surface, poor polishability, and the nickel-phosphorus plating layer is easy to strip, which leads to unstable mechanical dimensions of the substrate, affecting optical performance and processing accuracy.
The mirror body is made of C18150 chromium zirconium copper alloy. Through adhesive protection, multiple cleaning and chemical nickel-phosphorus alloy plating process, including first cleaning, water washing, second cleaning, neutralization and hot water washing, the modified layer thickness is uniform and polishable, and poor coating adhesion and unstable substrate size are avoided.
The mirror surface has achieved a high gloss finish, with good coating thickness uniformity, strong polishability, stable substrate mechanical dimensions, and sub-nanometer processing precision, thereby improving the optical performance and service life of the mirror.
Smart Images

Figure BDA0004584810370000051 
Figure BDA0004584810370000061
Abstract
Description
Technical Field
[0001] This invention belongs to the field of reflector technology and relates to a metal reflector and a method for electroless plating of nickel-phosphorus alloy on its surface. Background Technology
[0002] With the development of technology and the emergence of new fields, the materials used for reflectors have become increasingly diverse, with pure metal reflectors beginning to emerge. Compared to traditional glass reflectors, metal reflectors are cheaper to manufacture. Furthermore, due to the excellent processing characteristics of metals, and relying on modern ultra-precision machining technology, they can be used as both structural and optical components. By comprehensively optimizing the entire process chain—design, manufacturing, testing, and assembly—and effectively integrating optical and structural elements into optomechanical components, true optomechanical integrated manufacturing can be achieved. This results in more compact system structures, shorter development and production cycles, and higher product cost-effectiveness and technological advantages, offering broad market prospects in numerous military and civilian applications such as laser communication, laser manufacturing and weaponry, optical remote sensing, navigation and guidance, and reconnaissance and early warning.
[0003] Currently, the main materials for metal reflectors are aluminum alloys and beryllium alloys. However, as the application fields of metal reflectors gradually increase, the related technical requirements are becoming more and more difficult, and it is necessary to select a new metal or alloy to meet the relevant requirements.
[0004] To meet the optical performance requirements of a reflector, the reflector surface is often required to be sufficiently smooth. While a super-smooth surface can be achieved using normal machining methods, this places extremely high demands on the equipment. The residual stress generated during turning can also have a certain impact on the surface accuracy of the reflector.
[0005] Existing technologies for modifying alloy surfaces using chemical plating are mostly aimed at solving problems such as corrosion. There is limited documentation on surface modification techniques for optical applications, and these techniques suffer from the following drawbacks:
[0006] 1) Poor uniformity of the thickness of the chemical plating modified layer: The existing technology does not control the thickness of the modified layer precisely enough, resulting in uneven thickness and affecting the optical performance of the reflector;
[0007] 2) Minor surface defects: The current technology does not process the surface of the mirror meticulously enough, which easily produces minor defects and reduces the optical quality of the mirror;
[0008] 3) Poor polishability: Existing technologies for chemical plating of mirror surfaces cannot effectively improve their polishability, which limits the fine processing of mirrors.
[0009] 4) Processing is required after nickel stripping: The nickel-phosphorus plating layer used in the prior art is easy to strip, which leads to unstable mechanical dimensions of the substrate and requires additional processing. Summary of the Invention
[0010] The technical problem to be solved by the present invention is to provide a metal reflector and a method for electroless plating of nickel-phosphorus alloy on its surface. The reflector has a low cost and can achieve a reflector with extremely high surface smoothness through surface modification treatment.
[0011] To solve the above-mentioned technical problems, the metal reflector of the present invention has a mirror body material of chromium zirconium copper alloy and a mirror body surface plated with nickel phosphorus alloy.
[0012] Furthermore, the mirror body material is a C18150 chromium-zirconium-copper alloy.
[0013] Furthermore, the method for electroless nickel-phosphorus alloy plating on the surface of the aforementioned metal reflector is as follows: Apply a protective adhesive to the parts of the mirror body other than the surface to be nickel-plated; wipe the mirror body surface with an organic solvent; perform a first cleaning of the mirror body using solution A; rinse with water; perform a second cleaning of the mirror body using solution B; rinse with water; neutralize; clean; after hot water rinsing, immerse in an electroless nickel-phosphorus plating solution for nickel-phosphorus alloy plating; Solution A is composed of an acidic solution with added chromium trioxide, copper sulfate, and a surfactant, wherein the concentration of chromium trioxide is 30–80 g / L, the concentration of copper sulfate is 1–3 g / L, and the concentration of surfactant OP-10 is 0.01–0.03 ml / L; Solution B is composed of an acidic solution with added chromium trioxide, nickel nitrate, sodium nitrate, and sodium nitrite, wherein the concentration of chromium trioxide is 25–35 g / L, the concentration of nickel nitrate is 5–7 g / L, the concentration of sodium nitrate is 1–3 g / L, and the concentration of sodium nitrite is 1–3 g / L.
[0014] Next, apply protective adhesive 3-5 times to the parts of the mirror body except for the areas to be nickel plated. After the protective adhesive has solidified, use a sharp knife to trim the shape and expose the areas to be nickel-phosphorus plated. First wipe the surface of the mirror body with acetone, then wipe the surface of the mirror body with petroleum ether, and repeat the wiping process.
[0015] Preferably, the concentration of chromium trioxide in solution A is 50 g / L, the concentration of copper sulfate is 2 g / L, and the concentration of surfactant OP-10 is 0.02 ml / L.
[0016] Furthermore, the surface of the wiped mirror is cleaned once with solution A at a temperature of 30°C. The concentration of sulfuric acid in solution A is 16-24 ml / L, the concentration of nitric acid is 18-22 ml / L, the concentration of copper sulfate is 0-3 g / L, the concentration of copper nitrate is 2-2.5 g / L, the concentration of nickel nitrate is 9-12 g / L, and the cleaning time is 5-8 seconds.
[0017] Preferably, the concentration of nickel nitrate in solution B is 5 g / L, the concentration of sodium nitrate is 1 g / L, and the concentration of sodium nitrite is 1 g / L.
[0018] Furthermore, the mirror surface is cleaned a second time using solution B at a temperature of 40–45°C. The concentration of chromium trioxide in solution B is 25–35 g / L, the concentration of sulfuric acid is 95–110 ml / L, the concentration of phosphoric acid is 18–22 ml / L, the concentration of acetic acid is 19–23 ml / L, and the cleaning time is 4–6 seconds.
[0019] Furthermore, the acidic solution is neutralized using an aqueous solution of sodium carbonate, a sodium hydroxide solution, or ammonia water, with a neutralization time of 10 seconds.
[0020] Next, the microscope body is placed in preheated deionized water at a temperature of 70-80°C for 2 minutes.
[0021] Next, immerse the mirror body in the nickel-phosphorus plating solution and let it stand until the temperature is consistent with that of the nickel-phosphorus plating solution. Then, bring a cleaned thin iron wire into contact with the surface of the mirror body for 5 to 10 seconds until a reaction occurs on the surface of the mirror body and bubbles are generated. Remove the iron wire.
[0022] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0023] 1. Using chromium-zirconium-copper alloy as the mirror body material has the characteristics of high thermal conductivity, low coefficient of expansion, high elongation, high tensile strength, good mechanical dimensional stability, long service life, good weldability, and low cost.
[0024] 2. By employing steps such as applying adhesive for protection, wiping the surface, and cleaning multiple times, minor surface imperfections can be effectively reduced.
[0025] 3. It can ensure the uniformity of the modified layer thickness.
[0026] 4. By enhancing the polishability of the coating, the surface deviation of the metal mirror in the mid-to-high frequency band can be processed to the sub-nanometer level with high precision, easily achieving a roughness better than 1nm, which improves the optical performance of the mirror and thus improves the surface finish of the mirror.
[0027] 5. By selecting optimized primary cleaning solution components and secondary cleaning processes, the mechanical dimensional characteristics of the mirror surface can be kept stable, and problems such as substrate passivation and poor adhesion of the nickel-phosphorus layer after plating can be avoided.
[0028] 6. The nickel-phosphorus plating method used is easy to remove nickel from the substrate. After nickel removal, the substrate has stable mechanical dimensions and can be directly re-plated with nickel without further processing. Detailed Implementation
[0029] The present invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely for explaining the present invention and are not intended to limit the present invention.
[0030] The metal reflector of the present invention has a mirror body material of C18150 chromium-zirconium-copper alloy or other chromium-zirconium-copper alloy, and the surface of the mirror body is plated with nickel-phosphorus alloy.
[0031] The complete process for electroless nickel-phosphorus alloy plating on the surface of a metal reflector according to the present invention includes processes such as adhesive protection, surface wiping, primary cleaning, water washing, secondary cleaning, water washing, neutralization, cleaning, hot water washing, and electroless nickel plating. Taking C18150 chromium-zirconium-copper alloy as an example, the specific steps are as follows:
[0032] Step 1: Apply protective adhesive to the parts of the mirror body that need protection, 3-5 times. After the protective adhesive has solidified, use a sharp knife to trim the shape and expose the parts that need to be plated with nickel and phosphorus.
[0033] Step 2: Wipe the surface to remove oil, dust and other impurities: Use degreased cotton soaked in organic solvent to wipe the surface. First wipe the lens surface with acetone, then wipe the lens surface with petroleum ether, and repeatedly wipe with fresh degreased cotton.
[0034] Step 3, First Cleaning: Use Solution A at 30℃ to perform a first cleaning on the wiped mirror surface to remove the surface oxide layer and activate the surface. Solution A consists of an acidic solution with added chromium trioxide, copper sulfate, and surfactant. The concentrations of chromium trioxide in Solution A are: 0–80 g / L, sulfuric acid: 16–24 ml / L, nitric acid: 8–22 ml / L, copper sulfate: 1–3 g / L, copper nitrate: 2–2.5 g / L, nickel nitrate: 9–12 g / L, and surfactant OP-10: 0.01–0.03 ml / L. The cleaning time is 5–8 seconds. Sulfuric acid can be replaced with hydrofluoric acid, and nickel nitrate can be replaced with nickel sulfate.
[0035] Step 4, Water washing: Use flowing pure water at 25℃ to wash for 1 minute to remove the residual primary cleaning solution in the micropores on the surface of the lens.
[0036] Step 5, Secondary Cleaning: Perform a secondary cleaning using Solution B at a temperature of 40–45℃. Solution B consists of an acidic solution with added chromium trioxide, nickel nitrate, sodium nitrate, and sodium nitrite. The concentrations in Solution B are: chromium trioxide 25–35 g / L, sulfuric acid 95–110 ml / L, phosphoric acid 18–22 ml / L, acetic acid 19–23 ml / L, nickel nitrate 5–7 g / L, sodium nitrate 1–3 g / L, and sodium nitrite 1–3 g / L. The cleaning time is 4–6 seconds. Sodium nitrate can be replaced with sodium phosphate, and acetic acid can be replaced with lactic acid.
[0037] Step 6, Water washing: Use flowing pure water at 25℃ to wash for 1 minute to remove residual secondary cleaning solution in the micropores on the surface of the lens.
[0038] Step 7, Neutralization: Use a neutralization solution at 25°C to neutralize any acidic solution that may still be present in the pores of the mirror surface during the second cleaning, for 10 seconds; the neutralization solution can be an aqueous solution of sodium carbonate, a sodium hydroxide solution, or ammonia, etc.
[0039] Step 8, Water washing: Rinse with running water at 25°C for 1 minute to remove residual neutralization solution from the micropores on the surface of the microscope.
[0040] Step 9, Preheating: Place the cleaned microscope body into preheated deionized water at a temperature of 55-95℃ for 1-5 minutes.
[0041] Step 10, Electroless Nickel-Phosphorus Alloy Plating: Immerse the mirror body in the electroless nickel plating solution and let it stand for 1 minute. During this time, the mirror body and the nickel-phosphorus plating solution maintain the same temperature. Contact a clean, fine iron wire (0.5 mm in diameter) with the surface of the mirror body for 5-15 seconds until a reaction occurs and bubbles are generated. Remove the iron wire. At the beginning of the electroless nickel-phosphorus alloy plating process, a vigorous chemical reaction occurs in the plating area on the mirror body surface. This reaction produces gases such as hydrogen, which may adhere to the mirror body surface as dense bubbles, affecting subsequent reactions and resulting in poor adhesion between the plating layer and the mirror body, as well as pinholes on the plating surface. This invention uses clean, fine iron wire to eliminate bubbles on the mirror body surface, ensuring a uniform reaction.
[0042] The different concentrations of chromium trioxide and copper sulfate in a single cleaning process determine the porosity of the coating surface. The concentration of surfactant determines the plating speed in the subsequent electroless plating process. The specific effects are shown in Table 1. However, the components in the acidic solution have little effect on the plating speed and porosity within a given concentration range, so they are not listed in Table 1.
[0043] Table 1
[0044]
[0045] During the secondary cleaning, the concentration of nickel nitrate affects the uniformity of the coating, the concentration of sodium nitrate affects the surface cracking of the coating, and the concentration of sodium nitrite affects the hardness of the coating, as detailed in Table 2. The components in the acidic solution and chromium trioxide have little effect on the coating effect within the given concentration range, so they are not listed in Table 2.
[0046] Table 2
[0047]
[0048] Electroless plating of nickel-phosphorus alloy on the surface of a reflector differs from plating on other surfaces, requiring a certain level of hardness. To achieve an ultra-smooth surface and improve reflector performance, polishing is necessary after the electroless plating process, making polishability a crucial indicator of coating quality. The nickel-phosphorus alloy coating prepared in this invention exhibits extremely high polishability, enabling the machining of surface deviations in the mid-to-high frequency bands of metal reflectors to sub-nanometer precision, easily achieving a roughness better than 1 nm. This reduces costs while simultaneously improving the optical performance of the reflector and expanding its application range.
[0049] The effects of preheating and exhaust treatment on the coating performance of metal mirrors are shown in Table 3.
[0050] Table 3
[0051] Preheating time (min) Preheating temperature (°C) Exhaust time (s) Coating adhesion Polishing efficiency Number of pinholes Example 1 0 0 0 Difference Low many Example 2 0 55 5 Difference Low many Example 3 0 75 8 middle middle few Example 4 1 95 15 middle Low few Example 5 1 0 0 Difference Low many Example 6 1 55 5 middle middle many Example 7 2 75 8 excellent high none Example 8 2 95 15 excellent high few Example 9 2 0 0 Difference Low many Example 10 5 55 5 Difference Low few Example 11 5 75 8 middle high none Example 12 5 95 15 middle middle few
[0052] This invention uses a primary cleaning and a secondary cleaning process to replace conventional acid washing, alkali washing, activation, and other steps. The primary cleaning removes oil and dirt adhering to the mirror surface and activates the mirror surface, allowing subsequent reactions to proceed fully. The secondary cleaning further eliminates impurities on the mirror surface and etches a certain amount of corrosion on the mirror surface. Under the action of reagents such as phosphoric acid and nickel nitrate, a transition layer is generated on the mirror surface, improving the properties of the coating.
[0053] The present invention is not limited to the above embodiments. It is reasonable to foresee that those skilled in the art can make many simple alternatives based on the basic concept of the present invention, such as changing the acid solution components or adjusting the concentration of each component in the first and second cleaning without affecting the cleaning effect.
Claims
1. A method for electroless plating of nickel-phosphorus alloy onto the surface of a metal reflector, characterized in that, The method is as follows: Apply a protective adhesive to the parts of the mirror body except for the surface to be plated with nickel-phosphorus alloy; wipe the mirror body surface with an organic solvent; perform a first cleaning with solution A; rinse with water; perform a second cleaning with solution B at a temperature of 40-45℃; rinse with water; neutralize; clean; after hot water rinsing, immerse in a chemical nickel-phosphorus plating solution for nickel-phosphorus alloy plating; wherein solution A contains 50 g / L chromium trioxide, 2 g / L copper sulfate, 0.02 ml / L surfactant OP-10, 16-24 ml / L sulfuric acid, and 18-22 ml / L nitric acid. The solution has the following components:
1. Sulfuric acid concentration of 2-2.5 g / L, 2.5 g / L copper nitrate concentration of 9-12 g / L, and a cleaning time of 5-8 seconds; 2. Solution B is composed of an acidic solution with added chromium trioxide, nickel nitrate, sodium nitrate, and sodium nitrite; wherein the concentration of chromium trioxide is 25-35 g / L, the concentration of nickel nitrate is 5 g / L, the concentration of sodium nitrate is 1 g / L, the concentration of sodium nitrite is 1 g / L, the concentration of sulfuric acid is 95-110 ml / L, the concentration of phosphoric acid is 18-22 ml / L, the concentration of acetic acid is 19-23 ml / L, and the cleaning time is 4-6 seconds; the mirror body material is a chromium-zirconium-copper alloy.
2. The method for electroless plating of nickel-phosphorus alloy onto the surface of a metal reflector according to claim 1, characterized in that, Apply protective adhesive 3-5 times to the parts of the mirror body except for the parts that need to be plated with nickel-phosphorus alloy. After the protective adhesive has solidified, use a sharp knife to trim the shape to expose the parts that need to be plated with nickel-phosphorus alloy. First wipe the surface of the mirror body with acetone, then wipe the surface of the mirror body with petroleum ether, and wipe repeatedly.
3. The method for electroless plating of nickel-phosphorus alloy onto the surface of a metal reflector according to claim 1, characterized in that, Use solution A at 30°C to clean the wiped mirror surface once.
4. The method for electroless plating of nickel-phosphorus alloy onto the surface of a metal reflector according to claim 1, characterized in that, Preheat the microscope body by immersing it in preheated deionized water at a temperature of 70-80°C for 2 minutes.
5. The method for electroless plating of nickel-phosphorus alloy onto the surface of a metal reflector according to claim 1, characterized in that, Place the mirror body into the nickel-phosphorus plating solution and let it stand until the temperature is consistent with that of the nickel-phosphorus plating solution. Then, bring a clean thin iron wire into contact with the surface of the mirror body for 5 to 10 seconds until a reaction occurs on the surface of the mirror body and bubbles are generated. Remove the iron wire.
Citation Information
Patent Citations
Mirror Support for a Composite Optical Mirror and Method for Its Production
US20210231912A1