A negative electrode slurry and its preparation method, electrode sheet and lithium-ion battery
By introducing hydroxypropyl distarch phosphate into the negative electrode slurry and cross-linking it with a binder to form a network, the volume expansion problem of silicon-based negative electrode materials is solved, the adhesion and cycle performance of the electrode are improved, and the electrical performance of the battery is ensured to be stable.
Patent Information
- Application Number
- CN202311793784.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-22
AI Technical Summary
Existing silicon-based anode materials exhibit severe volume expansion during cyclic lithium intercalation, leading to continuous formation of the SEI film and damage to the electrode structure, resulting in significant capacity decay. Furthermore, existing anode slurries cannot effectively limit expansion and do not significantly improve electrical performance.
A negative electrode slurry containing hydroxypropyl distarch phosphate as an additive restricts the expansion of silicon-based materials and improves adhesion and cycle performance by forming a cross-linked network with binder monomers.
It effectively limits the expansion of silicon-based anode materials, improves the adhesion and cycle performance of the electrode sheets, and maintains the stability of the battery's electrical performance.
Smart Images

Figure CN117747836B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion batteries, specifically to a negative electrode slurry and its preparation method, an electrode sheet, and a lithium-ion battery. Background Technology
[0002] Currently, silicon-based anode materials possess extremely high theoretical specific capacity (3579 mAh / g, Li). 15 The advantages of Si4, such as its low voltage platform and abundant sources, have led to extensive exploration of its potential as a next-generation high-performance lithium-ion battery anode material, and the application of silicon-carbon systems in consumer and power batteries has begun.
[0003] However, silicon-based anode materials can expand by up to 300% during cyclic lithium intercalation. After prolonged cycling, the severe volume effect of silicon particles leads to the continuous formation of the SEI film and damage to the electrode structure, ultimately resulting in significant battery capacity decay. Silicon-based anodes often use linear polymers as binders and require the use of thickeners and dispersants, such as sodium carboxymethyl cellulose and sodium alginate. Increasing the amount of auxiliary materials used is detrimental to improving the proportion of active material in the electrode sheet and only promotes the processing performance of the anode slurry, without significantly improving the electrical performance of the silicon-based anode.
[0004] Therefore, it is indeed necessary to develop a negative electrode slurry that can limit the expansion of silicon-based materials and has good cycle performance, as well as a corresponding preparation method. Summary of the Invention
[0005] The purpose of this invention is to provide a negative electrode paste that addresses the shortcomings of existing technologies, thereby solving the problems that existing negative electrode pastes cannot limit the expansion of silicon-based materials, result in severe battery capacity decay, and do not significantly improve electrical performance.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A negative electrode slurry includes a negative electrode active material, a binder, and an additive; the binder includes binder monomer A, which includes one or more of acrylic acid, methacrylic acid, 2-acetamidoacrylic acid, maleic acid, 2-ethylacrylic acid, 2-propylacrylic acid, and methylene succinic acid; the additive is hydroxypropyl distarch phosphate, with the following structural formula:
[0008]
[0009] Preferably, the adhesive further includes adhesive monomer B, which includes one or more of acrylonitrile, acrylamide, methacrylamide, N-ethylacrylamide, N-hydroxymethylacrylamide, and N-isopropylacrylamide.
[0010] Preferably, the adhesive further includes adhesive monomer C, which includes one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, tert-butyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and 2-methoxyethyl acrylate.
[0011] Preferably, the weight ratio of the binder monomer A, binder monomer B and binder monomer C is (30-60):(20-50):(0-20).
[0012] Preferably, the adhesive further includes adhesive D, which includes one or more of styrene-butadiene rubber, styrene-acrylic rubber, and acrylate rubber.
[0013] Preferably, the negative electrode slurry comprises, by weight, 12-195 parts of the negative electrode active material, 1.005-9 parts of the binder, and 0.01-0.5 parts of the additive.
[0014] Preferably, the negative electrode slurry further includes a conductive agent and a solvent, wherein the conductive agent is 0.1-4 parts by weight and the solvent is 1-400 parts by weight.
[0015] Preferably, the weight-average molecular weight of the adhesive is 20w-100w.
[0016] Furthermore, the present invention also provides a method for preparing an adhesive, comprising the following steps:
[0017] S1. Mix binder monomer A, binder monomer B and binder monomer C with deionized water to obtain solution A, and then wash solution A by passing inert gas through it.
[0018] S2. Place solution A from step S1 in an inert gas atmosphere, add an initiator and stir to react, then cool to room temperature to obtain an aqueous solution of the composite adhesive.
[0019] S3. Mix the active material with the conductive agent, add some additives, some composite binders and some solvents, and stir evenly to obtain solution B;
[0020] S4. Add the remaining additives, composite binder and solvent to solution B, then add binder D, and stir evenly to obtain the negative electrode slurry.
[0021] Preferably, the initiator is ammonium persulfate and / or potassium persulfate, and the amount of the initiator is 0.1-1% of the mass of the composite binder.
[0022] In addition, the present invention also provides a negative electrode sheet, including a current collector and a negative electrode slurry coating coated on at least one side of the current collector, wherein the negative electrode slurry coating is the aforementioned negative electrode slurry.
[0023] In addition, the present invention also provides a lithium-ion battery, comprising a cell wound with a negative electrode, a positive electrode and a separator, an electrolyte, and a casing for encapsulating the cell and the electrolyte, wherein the negative electrode is the aforementioned negative electrode.
[0024] Compared to existing technologies, the advantages of this invention are as follows: The negative electrode slurry provided by this invention, by adding the additive hydroxypropyl distarch phosphate, allows for more precise control of the slurry's viscosity, facilitating coating under different processing conditions. Furthermore, without altering the processing performance of the negative electrode slurry, the additive participates in the construction of the binder coating network, improving adhesion and the cycle performance of the negative electrode. During subsequent baking, the abundant hydroxyl groups in hydroxypropyl distarch phosphate can form hydrogen bonds with the carboxyl groups in binder monomer A, resulting in esterification and cross-linking reactions to form a cross-linked coating network, which better restricts the expansion of the silicon-based negative electrode material. In addition, compared to traditional thickeners, this additive allows for viscosity control and cross-linked network formation with a smaller addition amount. Attached Figure Description
[0025] Figure 1 This is a schematic diagram of the cross-linked coating layer formed by the cross-linking of the additive and binder monomer A of the present invention. Detailed Implementation
[0026] To make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0027] According to a first aspect of this application, this application provides a negative electrode slurry, comprising a negative electrode active material, a binder, and an additive; the binder comprises binder monomer A, which includes one or more of acrylic acid, methacrylic acid, 2-acetamidoacrylic acid, maleic acid, 2-ethylacrylic acid, 2-propylacrylic acid, and methylene succinic acid; the additive is hydroxypropyl distarch phosphate, the structural formula of which is as follows:
[0028]
[0029] The additive hydroxypropyl distarch phosphate acts as a thickener and in-situ crosslinker in the slurry. Binder monomer A in the binder acts as a dispersant and binder, and during the subsequent baking process, binder monomer A will crosslink with the additive to form a crosslinked coating layer. The additive, as a thickener and in-situ crosslinker in the linear binder, and the binder used in conjunction with it, allow the thickener to participate in the construction of the binder coating network without altering the processing performance of the negative electrode slurry, thereby improving adhesion and the cycle performance of the negative electrode.
[0030] In some embodiments, the adhesive further includes adhesive monomer B, which includes one or more of acrylonitrile, acrylamide, methacrylamide, N-ethylacrylamide, N-hydroxymethylacrylamide, and N-isopropylacrylamide.
[0031] In some embodiments, the adhesive further includes adhesive monomer C, which includes one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, tert-butyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and 2-methoxyethyl acrylate.
[0032] In some embodiments, the weight ratio of adhesive monomer A, adhesive monomer B and adhesive monomer C is (30-60):(20-50):(0-20).
[0033] In some embodiments, the adhesive further includes adhesive D, which includes one or more of styrene-butadiene rubber, styrene-acrylic rubber, and acrylate rubber.
[0034] In some embodiments, the negative electrode slurry comprises, by weight, 12-195 parts of negative electrode active material, 1.005-9 parts of binder, and 0.01-0.5 parts of additives.
[0035] In some embodiments, the negative electrode slurry further includes a conductive agent and a solvent, wherein the conductive agent is 0.1-4 parts by weight and the solvent is 1-400 parts by weight.
[0036] In some embodiments, the weight-average molecular weight of the adhesive is 20w-100w.
[0037] According to a second aspect of this application, this application provides a method for preparing a negative electrode slurry, comprising the following steps:
[0038] S1. Mix binder monomer A, binder monomer B and binder monomer C with deionized water to obtain solution A, and then wash solution A by passing inert gas through it.
[0039] S2. Place solution A from step S1 in an inert gas atmosphere, add an initiator and stir to react, then cool to room temperature to obtain an aqueous solution of the composite adhesive.
[0040] S3. Mix the active material with the conductive agent, add some additives, some composite binders and some solvents, and stir evenly to obtain solution B;
[0041] S4. Add the remaining additives, composite binder and solvent to solution B, then add binder D, and stir evenly to obtain the negative electrode slurry.
[0042] In some embodiments, the initiator is ammonium persulfate and / or potassium persulfate, and the amount of initiator is 0.1-1% of the mass of the composite binder.
[0043] In some embodiments, the active material is one or more of artificial graphite, natural graphite, nano-silicon, silicon-carbon materials, silicon-oxygen materials, hard carbon, and mesophase carbon microspheres.
[0044] In some embodiments, the conductive agent is one or more of carbon black, acetylene black, Ketjen black, carbon nanotubes, carbon fibers, and graphene.
[0045] According to a third aspect of this application, this application provides a negative electrode sheet, including a current collector and an active layer coated on at least one surface of the current collector, the active layer including the aforementioned negative electrode slurry.
[0046] In some embodiments, the negative electrode sheet is prepared by coating the above-mentioned negative electrode slurry onto copper foil and baking it at a high temperature of 70-100°C to obtain the negative electrode sheet. During the baking process, the abundant hydroxyl groups in hydroxypropyl distarch phosphate can crosslink with the carboxyl groups in the composite binder to form a crosslinked coating network, which can better limit the expansion of the silicon-based negative electrode material. Compared with traditional thickeners, this additive can control the viscosity and form a crosslinked network with a smaller amount added.
[0047] According to a fourth aspect of this application, this application provides a lithium-ion battery, including a cell wound with a negative electrode, a positive electrode and a separator, an electrolyte, and a casing for encapsulating the cell and the electrolyte, wherein the negative electrode is the aforementioned electrode sheet.
[0048] In some embodiments, the negative electrode sheet is rolled and slit, then wound with conventionally used lithium cobalt oxide positive electrode sheet and separator to prepare a bare cell, and then manufactured into a battery through subsequent assembly, molding and testing processes.
[0049] The positive electrode includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. The positive active material layer includes a positive active material, which may be, but is not limited to, a chemical formula such as Li. a Ni x Co y M z O2-b N b (where 0.95≤a≤1.2, x>0, y≥0, z≥0, and x+y+z=1, 0≤b≤1, M is selected from one or more combinations of Mn and Al, and N is selected from one or more combinations of F, P, and S) The positive electrode active material may also be, but is not limited to, LiCoO2, LiNiO2, LiVO2, LiCrO2, LiMn2O4, LiCoMnO4, Li2NiMn3O8, LiNi 0.5 Mn 1.5 The positive electrode active material can be one or more combinations of O4, LiCoPO4, LiMnPO4, LiFePO4, LiNiPO4, LiCoFSO4, CuS2, FeS2, MoS2, NiS, and TiS2. The positive electrode active material can also be modified. Methods for modifying the positive electrode active material are known to those skilled in the art. For example, coating, doping, and other methods can be used to modify the positive electrode active material. The materials used for modification can be one or more combinations of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce, and W, including but not limited to. The positive electrode current collector is typically a structure or component that collects current. The positive electrode current collector can be any material suitable for use as a positive electrode current collector in lithium-ion batteries. For example, the positive electrode current collector can be, but is not limited to, metal foil, and more specifically, aluminum foil, among others.
[0050] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the surface of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, which may be one or more of the following: graphite, soft carbon, hard carbon fiber, mesophase carbon microspheres, silicon-based materials, tin-based materials, lithium titanate, or other metals that can form alloys with lithium. Specifically, the graphite may be selected from one or more of artificial graphite, natural graphite, and modified graphite; the silicon-based material may be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, and silicon alloys; and the tin-based material may be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. The negative electrode current collector is typically a structure or component that collects current. The negative electrode current collector may be any material suitable for use as a negative electrode current collector in lithium-ion batteries, for example, it may be, but is not limited to, metal foil, and more specifically, copper foil.
[0051] The lithium-ion battery also includes an electrolyte, which comprises an organic solvent, an electrolyte lithium salt, and additives. The electrolyte lithium salt can be LiPF6 and / or LiBOB used in high-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, and LiPF6 used in low-temperature electrolytes; it can also be at least one of LiBF4, LiBOB, LiPF6, and LiTFSI used in overcharge-resistant electrolytes; or it can be at least one of LiClO4, LiAsF6, LiCF3SO3, and LiN(CF3SO2)2. The organic solvent can be a cyclic carbonate, including PC and EC; it can also be a chain carbonate, including DFC, DMC, or EMC; or it can be a carboxylic acid ester, including MF, MA, EA, MP, etc. The additives include, but are not limited to, at least one of film-forming additives, conductive additives, flame-retardant additives, overcharge-resistant additives, additives for controlling the H2O and HF content in the electrolyte, additives for improving low-temperature performance, and multifunctional additives.
[0052] In some embodiments, the housing is made of stainless steel or aluminum-plastic film, preferably aluminum-plastic film.
[0053] Example 1
[0054] Preparation of composite adhesive:
[0055] 50 parts acrylic acid, 40 parts methacrylamide, 10 parts ethyl acrylate, and 900 parts deionized water were mixed and stirred uniformly at 350 rpm to obtain solution A. The monomer solution was rinsed with argon gas to remove oxygen from the system. After purging, the solution was placed in a closed environment protected by argon circulation, and 0.5 parts ammonium persulfate were added. The mixture was stirred at 350 rpm under a constant temperature of 50°C for 10 hours. After the reaction was completed, the solution was allowed to cool to room temperature to obtain an aqueous solution of the composite adhesive.
[0056] Preparation of negative electrode slurry:
[0057] The preparation method of this negative electrode slurry includes the following steps:
[0058] Solution B is prepared by mixing 90 parts of artificial graphite, 5 parts of nano-silicon, 1 part of carbon nanotubes, 1.6 parts of composite binder (i.e., 16 parts of 10% composite binder aqueous solution), 0.02 parts of hydroxypropyl distarch phosphate, and 36 parts of deionized water and stirring at 500 r / min.
[0059] Add 0.8 parts of styrene-acrylic rubber, 1.6 parts of composite binder, 0.02 parts of hydroxypropyl distarch phosphate, and 36 parts of deionized water to solution B, and stir evenly at a speed of 1000 r / min to obtain the negative electrode slurry.
[0060] Preparation of negative electrode:
[0061] The above-mentioned negative electrode slurry is coated onto copper foil and baked at 80°C to obtain a negative electrode sheet.
[0062] The fabrication of lithium-ion batteries:
[0063] After being rolled and slit, the aforementioned negative electrode sheet is wound together with conventionally used lithium cobalt oxide positive electrode sheet and separator to prepare a bare cell. The cell is then assembled, formed and tested to produce a battery for subsequent performance testing.
[0064] Example 2
[0065] Unlike Example 1, the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry in this example is 0.08 parts.
[0066] The rest is the same as in Example 1, and will not be repeated here.
[0067] Example 3
[0068] Unlike Example 1, the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry in this example is 0.12 parts.
[0069] The rest is the same as in Example 1, and will not be repeated here.
[0070] Example 4
[0071] Unlike Example 1, the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry in this example is 0.16 parts.
[0072] The rest is the same as in Example 1, and will not be repeated here.
[0073] Example 5
[0074] Unlike Example 1, the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry in this example is 0.20 parts.
[0075] The rest is the same as in Example 1, and will not be repeated here.
[0076] Example 6
[0077] Unlike Example 1, the composite binder in this example contains 40 parts of acrylic acid and 50 parts of methacrylamide, and the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry is 0.12 parts.
[0078] The rest is the same as in Example 1, and will not be repeated here.
[0079] Example 7
[0080] Unlike Example 1, the composite binder in this example contains 60 parts of acrylic acid and 30 parts of methacrylamide, and the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry is 0.12 parts.
[0081] The rest is the same as in Example 1, and will not be repeated here.
[0082] Example 8
[0083] Unlike Example 1, in this example, the composite binder contains 60 parts of acrylic acid, 20 parts of methacrylamide, and 20 parts of ethyl acrylate, and the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry is 0.12 parts.
[0084] The rest is the same as in Example 1, and will not be repeated here.
[0085] Example 9
[0086] Unlike Example 1, in this example, the composite binder contains 45 parts acrylic acid, 40 parts methacrylamide, and 15 parts ethyl acrylate, and the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry is 0.12 parts.
[0087] The rest is the same as in Example 1, and will not be repeated here.
[0088] Example 10
[0089] Unlike Example 1, in this example, the composite binder contains 55 parts acrylic acid, 40 parts methacrylamide, and 5 parts ethyl acrylate, and the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry is 0.12 parts.
[0090] The rest is the same as in Example 1, and will not be repeated here.
[0091] Example 11
[0092] Unlike Example 1, the composite binder in this example contains 60 parts of acrylic acid and 40 parts of methacrylamide, and the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry is 0.20 parts.
[0093] The rest is the same as in Example 1, and will not be repeated here.
[0094] Comparative Example 1
[0095] Unlike Example 1, the total amount of hydroxypropyl distarch phosphate added to the negative electrode slurry in this comparative example is 0 parts.
[0096] The rest is the same as in Example 1, and will not be repeated here.
[0097] Comparative Example 2
[0098] Unlike Example 1, the composite binder in this comparative example contains 0 parts of acrylic acid, 90 parts of methacrylamide, and 0.12 parts of hydroxypropyl distarch phosphate in the negative electrode slurry.
[0099] The rest is the same as in Example 1, and will not be repeated here.
[0100] Comparative Example 3
[0101] Unlike Example 1, the hydroxypropyl distarch phosphate in the negative electrode slurry of this comparative example is replaced with sodium carboxymethyl cellulose, the feeding process remains unchanged, and the total addition amount is 0.12 parts.
[0102] The rest is the same as in Example 1, and will not be repeated here.
[0103] The following performance tests were performed on the negative electrode slurry, negative electrode sheet, and battery prepared in the examples and comparative examples, respectively:
[0104] (1) Slurry viscosity test
[0105] The viscosity of the negative electrode slurry prepared according to the above method was tested using a rotational viscometer. The test rotation speed was set to 15 rpm, and the viscosity unit was cps.
[0106] (2) Electrode peel strength test
[0107] Cut the negative electrode sheet prepared according to the above method into strips 20mm wide and 180mm long. Prepare a clean, dust-free, and uneven glass plate, and attach a 24mm wide strip of 3M Scotch double-sided tape to the glass plate. Attach one end of the strip electrode sheet to the double-sided tape, with a 100mm adhesive length. Roll the section where the electrode sheet and glass plate are joined 3-4 times to ensure a tight bond. Perform an electrode sheet peel test using an electronic universal testing machine to measure the electrode sheet adhesion strength. With one end of the electrode sheet fixed to the glass plate facing upwards, and the other end of the glass plate fixed with a lower clamp, fold the free end of the electrode sheet upwards 180° and fix it with an upper clamp. At room temperature, keeping the lower clamp stationary, stretch the upper clamp upwards at a stretching rate of 100mm / min. Take the average peel force of the 25mm-100mm section as the adhesion strength obtained from a single test, in gf.
[0108] (3) Cycle retention test
[0109] ① Charge the battery at 0.5C to 4.5V at 25℃, with a cutoff current of 0.05C, and let it rest for 5 minutes; ② Measure the battery's discharge capacity at this point and record it as Dbefore; ③ Discharge the battery at 0.8C to 3V and let it rest for 5 minutes; ④ Charge the battery at 1.5C to 4.5V, with a cutoff current of 0.05C, and let it rest for 5 minutes; ⑤ Repeat steps ③ and ④ above 300 times, and then measure the battery's discharge capacity at this point and record it as Dafter. The cycle retention rate is calculated as Dafter / Dbefore * 100%.
[0110] (4) Cyclic thickness change rate test
[0111] ① Charge the battery at 0.5C to 4.5V at 25℃, with a cutoff current of 0.05C, and let it rest for 5 minutes; ② Measure the battery thickness at this point and record it as dbefore; ③ Discharge the battery at 0.8C to 3V and let it rest for 5 minutes; ④ Charge the battery at 1.5C to 4.5V, with a cutoff current of 0.05C, and let it rest for 5 minutes; ⑤ Repeat steps ③ and ④ above 300 times, and then measure the battery thickness at this point and record it as dafter. The cycle thickness retention rate is calculated as (dafter - dbefore) / dbefore * 100%.
[0112] The performance test results are shown in Table 1 below.
[0113] Table 1
[0114]
[0115] Comparing Examples 1-5 with Comparative Example 1, it was found that as the amount of hydroxypropyl distarch phosphate additive increased, the viscosity of the negative electrode slurry also increased, and the viscosity of the slurry remained within a range conducive to coating and processing. This resulted in improved adhesion of the negative electrode sheet and better cycle performance. In contrast, Comparative Example 1, which did not contain the additive hydroxypropyl distarch phosphate, had poor viscosity and poor electrode adhesion. Furthermore, in the above examples, when the amount of hydroxypropyl distarch phosphate added was greater than 0.12%, the cycle retention rate and cycle thickness change rate of the negative electrode were at comparable levels. Based on the design principle that the less auxiliary material used in the electrode formulation, the better, Example 3 is the preferred embodiment without sacrificing cycle performance.
[0116] Comparative studies of Examples 3 and 8-11 revealed that the higher the proportion of binder monomers A and B in the binder, the greater the electrode adhesion. This is because binder monomers A, B, and hydroxypropyl distarch phosphate all contain polar functional groups, and the higher their proportion, the stronger the electrode adhesion.
[0117] Comparing Examples 3, 6-8 with Comparative Example 2, it was found that the higher the proportion of binder monomer B in the binder, the greater the electrode adhesion. This indicates that binder monomer B plays a major role in improving the electrode adhesion.
[0118] Comparing Example 3 with Comparative Example 3, it was found that when using the same amount of CMC as a thickener, the viscosity of the negative electrode slurry was lower, and the cycle performance of the electrode decreased. This is because CMC has a relatively small binding effect in the electrode and does not participate in the construction of the cross-linked network during the electrode baking process. In contrast, the addition of hydroxypropyl distarch phosphate, while acting as a thickener, allows its hydroxyl groups to undergo esterification with the carboxyl groups in the binder during the subsequent electrode baking process, forming covalent bonds. These co-existing hydrogen bonds help build a cross-linked network, thereby limiting the rebound during negative electrode cycling and slowing down capacity decay.
[0119] In summary, the present invention provides a negative electrode slurry comprising a negative electrode active material, a binder, and an additive. The binder includes binder monomer A, and the additive is hydroxypropyl distarch phosphate. This additive, used in conjunction with the binder, participates in the construction of the binder coating network without altering the processing performance of the negative electrode slurry, thereby improving adhesion and the cycle performance of the negative electrode. Furthermore, the abundant hydroxyl groups in the additive can crosslink with the carboxyl groups in binder monomer A, forming a crosslinked coating network through synergistic hydrogen bonding, which can better limit the expansion of the silicon-based negative electrode material.
[0120] Based on the disclosure and teachings of the foregoing specification, those skilled in the art can make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments described above, and any obvious improvements, substitutions, or modifications made by those skilled in the art based on the present invention are within the scope of protection of the present invention. Furthermore, although some specific terms are used in this specification, these terms are only for convenience of explanation and do not constitute any limitation on the present invention.
Claims
1. A negative electrode slurry, characterized in that: Includes negative electrode active material, binder and additives; The adhesive includes adhesive monomer A, which includes one or more of acrylic acid, methacrylic acid, 2-acetamidoacrylic acid, maleic acid, 2-ethylacrylic acid, 2-propylacrylic acid, and methylene succinic acid. The additive is hydroxypropyl distarch phosphate, and its structural formula is: 。 2. The negative electrode slurry according to claim 1, characterized in that: The negative electrode active material is 12-195 parts by weight, the binder is 1.005-9 parts, and the additive is 0.01-0.5 parts.
3. The negative electrode slurry according to claim 1, characterized in that: The adhesive further includes adhesive monomer B, which includes one or more of acrylonitrile, acrylamide, methacrylamide, N-ethylacrylamide, N-hydroxymethylacrylamide, and N-isopropylacrylamide.
4. The negative electrode slurry according to claim 2, characterized in that: The adhesive further includes adhesive monomer C, which includes one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, tert-butyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and 2-methoxyethyl acrylate.
5. The negative electrode slurry according to claim 3, characterized in that: The weight ratio of the binder monomer A, binder monomer B and binder monomer C is (30-60):(20-50):(0-20).
6. The negative electrode slurry according to claim 1 or 3, characterized in that: The adhesive further includes adhesive D, which includes one or more of styrene-butadiene rubber, styrene-acrylic rubber, and acrylate rubber.
7. The negative electrode slurry according to claim 1, characterized in that: The negative electrode slurry also includes a conductive agent and a solvent, wherein the conductive agent is 0.1-4 parts by weight and the solvent is 1-400 parts by weight.
8. The negative electrode slurry according to claim 1, characterized in that: The weight-average molecular weight of the adhesive is 20w-100w.
9. A method for preparing the negative electrode slurry according to claim 1, characterized in that, Includes the following steps: S1. Mix binder monomer A, binder monomer B and binder monomer C with deionized water to obtain solution A, and then wash solution A by passing inert gas through it. S2. Place solution A from step S1 in an inert gas atmosphere, add an initiator and stir to react, then cool to room temperature to obtain an aqueous solution of the composite adhesive. S3. Mix the active material with the conductive agent, add some additives, some composite binders and some solvents, and stir evenly to obtain solution B; S4. Add the remaining additives, composite binder and solvent to solution B, then add binder D, and stir evenly to obtain the negative electrode slurry. Wherein, the binder monomer B includes one or more of acrylonitrile, acrylamide, methacrylamide, N-ethylacrylamide, N-hydroxymethylacrylamide, and N-isopropylacrylamide; The binder monomer C includes one or more of methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, tert-butyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and 2-methoxyethyl acrylate. The adhesive D includes one or more of styrene-butadiene rubber, styrene-acrylic rubber, and acrylate rubber.
10. The method for preparing the negative electrode slurry according to claim 9, characterized in that, The initiator is ammonium persulfate and / or potassium persulfate, and the amount of the initiator is 0.1-1% of the mass of the composite adhesive.
11. A negative electrode sheet, characterized in that: It includes a current collector and a negative electrode slurry coating coated on at least one side of the current collector, wherein the negative electrode slurry coating is the negative electrode slurry according to any one of claims 1 to 8.
12. A lithium-ion battery, characterized in that: Includes the negative electrode sheet as described in claim 11.
Citation Information
Patent Citations
Composition for electric storage device, slurry for electric storage device, electric storage device electrode, and electric storage device
JP2018152276A
Starch-Based Hot Melt Adhesive
US20150045480A1