Positive electrode lithium supplement material and preparation method thereof, positive electrode sheet and secondary battery
By using lithium-rich particles as the core in the positive electrode lithium supplement material, covering the catalytic layer and protective layer, combined with porous carbon mesh and hydrophobic materials, the problem of the generation of harmful substances in the positive electrode lithium supplement material during the discharge process is solved, and the lithium ion efficiency is improved. the extraction efficiency and the electrochemical performance of the battery.
Patent Information
- Application Number
- CN202311485323.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-11-08
AI Technical Summary
Existing cathode lithium supplement materials produce harmful substances during the discharge process, resulting in reduced battery performance and limited commercialization. They also easily react with water to generate strong alkalis and harmful gases.
It uses lithium-rich particles as the core, covering the catalytic layer and the protective layer. The catalytic layer contains the metal element M1, and the protective layer contains the metal oxide M2. The porous carbon network is used to improve the conductivity and the extraction efficiency of lithium ions, and through hydrophobic materials and conductive The carbon layer further protects the material.
It effectively reduces the accumulation of harmful substances in the electrolyte, improves the extraction efficiency of lithium ions, reduces the deterioration and water absorption rate of materials in humid air, and improves the electrochemical performance and safety of batteries.
Smart Images

Figure CN117766763B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode lithium supplement material and a preparation method thereof, a positive electrode plate and a secondary battery. Background Art
[0002] During the first charging process of a lithium-ion battery, a large amount of solid electrolyte interface film will be generated on the surface of the negative electrode of the battery, which consumes the limited lithium ions and electrolyte in the battery, causing irreversible capacity loss, reducing the energy density of the lithium-ion secondary battery, and limiting the application of lithium-ion batteries. In the prior art, adding positive electrode lithium supplement material to the positive electrode material can effectively compensate for the first irreversible capacity loss of the lithium battery.
[0003] However, in actual industrial applications, some positive electrode lithium supplement materials will produce some harmful substances during the discharge and lithium supplement process, which will cause harm to the battery. In addition, such lithium supplement materials are also prone to react with water in the air to produce strong alkali LiOH and H2S. This limits the commercialization of such lithium supplement materials. Therefore, how to solve the above problems has become the key. Summary of the invention
[0004] The purpose of the present application is to provide a positive electrode lithium supplement material and a preparation method thereof, a positive electrode plate and a secondary battery.
[0005] This application provides the following technical solutions:
[0006] In the first aspect, the present application provides a positive electrode lithium supplement material, including a core, a catalytic layer and a protective layer; wherein the core includes lithium-rich particles; the catalytic layer is coated on the outer surface of the core, the catalytic layer contains a catalyst, and the catalyst contains a metal element M1; the protective layer is coated on the outer surface of the catalytic layer, the protective layer includes a metal oxide, the metal oxide contains a metal element M2, and the metal elements M1 are different from M2.
[0007] The present invention coats a catalytic layer on the outer surface of the lithium-rich particles as the inner core, and the catalytic layer includes a catalyst. The catalyst can catalyze the conversion of harmful substances in the positive electrode lithium supplement material during the discharge process, thereby reducing the accumulated concentration of harmful materials in the electrolyte; and the present invention also coats a protective layer on the outer surface of the catalytic layer, and the protective layer includes a stable metal oxide, so that the protective layer can reduce the erosion of the inner core by external water vapor, thereby effectively improving the problem of material deterioration in humid air to generate residual alkali and harmful odorous gases, thereby avoiding problems such as mixed material gelation and loss of active components.
[0008] In one embodiment, the catalytic layer includes a first porous carbon mesh, and the catalyst is distributed in the first porous carbon mesh; and / or, the protective layer includes a second porous carbon mesh, and the metal oxide is distributed in the second porous carbon mesh. The porous carbon mesh in the catalytic layer and the protective layer can improve the electrical conductivity of the layer, thereby improving the efficiency of lithium ion escape. Moreover, the porous carbon mesh retained by the carbon framework is more likely to form a continuous carbon structure. The advantage of this structure is that a fast ion channel can be formed using a continuous porous carbon mesh, thereby further improving the efficiency of lithium ion escape.
[0009] In one embodiment, the positive electrode lithium supplement material further includes a porous carbon framework, the lithium-rich particles are contained in the inner cavity of the porous carbon framework and / or attached to its skeleton, and the catalyst is embedded in the skeleton inside the porous carbon framework to form the catalytic layer. The advantage of retaining a porous carbon framework in the catalytic layer and the protective layer is that the porous carbon framework is a three-dimensional skeleton structure, which can provide a larger specific surface area, which is conducive to increasing the attachment sites of lithium-rich particles, thereby increasing the mass proportion of lithium-rich particles in the positive electrode lithium supplement material to improve the capacity of the material; and the porous carbon framework provides a reaction space for catalyzing lithium polysulfide, and lithium polysulfide can fully combine with metal compounds, thereby improving the catalytic efficiency; and the porous carbon framework also provides a channel for the escape of lithium ions, thereby improving the escape efficiency of lithium ions.
[0010] In one embodiment, in the catalytic layer, the content of the catalyst gradually increases from the outer side away from the core to the inner side close to the core. The advantage of this arrangement is that after the core is discharged, the formation of harmful substances (such as lithium polysulfide) is mainly concentrated in the core close to the core, so more harmful substances (such as lithium polysulfide) can be converted by the catalyst, thereby improving the conversion efficiency.
[0011] In one embodiment, the positive electrode lithium supplement material further includes a hydrophobic material, and the hydrophobic material is located in the catalyst layer and / or the protective layer. The hydrophobic material can be used to lock moisture during the material preparation process to prevent the loss of lithium source, and the hydrophobic material retained in the material can also form a doping enhancement protective layer or catalyst layer conductivity, thereby improving the lithium ion extraction efficiency.
[0012] In one embodiment, the positive electrode lithium supplement material further includes a hydrophobic material layer, and the hydrophobic material layer is coated on the outer surface of the protective layer. The hydrophobic material layer can further improve the hydrophobic properties of the material, and when the carbon skeleton is still retained in the catalytic layer or the protective layer, the lithium-rich particles on the carbon skeleton are encapsulated to prevent the lithium-rich particles from being exposed.
[0013] In one embodiment, the positive electrode lithium supplement material further includes a conductive carbon layer, and the conductive carbon layer is coated on the outer surface of the protective layer. The purpose of providing the conductive carbon layer is to improve the ionic conductivity of the positive electrode lithium supplement material and further protect the inner core to prevent external water vapor from corroding the material.
[0014] In one embodiment, the lithium-rich particles include a binary lithium-rich compound having a structural formula of Li x K y , M is selected from any one of S, P, N, Br, I, F, O, B, Se, 1≤x≤5, 0<y.
[0015] In one embodiment, the metal element M1 is selected from at least one of Fe, Cu, Zn, In, Cd, Co, and Ni.
[0016] In one embodiment, the metal element M2 is selected from at least one of Al, Zr, Mg, Cr, Mn, Ca, and Ti.
[0017] In one embodiment, the particle size D50 of the lithium-rich particles is 50 nm to 20 μm.
[0018] In one embodiment, the catalytic layer has a thickness of 2 nm to 10 nm.
[0019] In one embodiment, the protective layer has a thickness of 3 nm to 15 nm.
[0020] In one embodiment, the mass ratio of the core, the catalytic layer, and the protective layer is 100:(0.01-50):(0.01-50).
[0021] In a second aspect, the present application also provides a method for preparing a positive electrode lithium replenishing material, comprising: providing a metal organic framework with a core-shell structure, wherein the metal organic framework comprises an inner layer framework and an outer layer framework; mixing and sintering a lithium source and the metal organic framework to obtain the positive electrode lithium replenishing material, wherein the lithium source forms a core, the inner layer framework forms a catalytic layer, and the outer layer framework forms a protective layer.
[0022] In a third aspect, the present application also provides a positive electrode plate, which includes a current collector and an active material layer arranged on the current collector, the active material layer includes a positive electrode material and the positive electrode lithium replenishing material described in any one of the embodiments of the first aspect, or the active material layer includes a positive electrode material and a positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material described in any one of the embodiments of the second aspect.
[0023] In a fourth aspect, the present application also provides a secondary battery, comprising the positive electrode plate described in the third aspect, or the battery comprises the positive electrode lithium replenishing material described in any one of the embodiments of the first aspect, or the battery comprises the positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material described in any one of the embodiments of the second aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0025] Figure 1 A schematic diagram of the cross-sectional structure of a positive electrode lithium supplement material in one embodiment;
[0026] Figure 2 A schematic diagram of the preparation process of a positive electrode lithium supplement material in one embodiment;
[0027] Figure 3 A schematic diagram of the cross-sectional structure of a positive electrode lithium supplement material in another embodiment;
[0028] Figure 4 A schematic diagram of the cross-sectional structure of a first porous carbon mesh in one embodiment
[0029] Figure 5 A schematic diagram of the cross-sectional structure of a positive electrode lithium supplement material in another embodiment;
[0030] Figure 6 A schematic diagram of the preparation process of a positive electrode lithium supplement material in another embodiment;
[0031] Figure 7 A schematic diagram of the cross-sectional structure of a positive electrode lithium supplement material in another embodiment;
[0032] Figure 8 A flow chart of the preparation of a positive electrode lithium supplement material in one embodiment;
[0033] Fig. 9 This is a SEM image of the framework structure obtained after step 1 in Example 1;
[0034] Fig.10 This is a SEM image of the framework structure obtained after step 2 in Example 1. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0036] It should be noted that when an object is said to be "fixed to" another object, it can be directly on the other object or there can be an intermediate object. When an object is said to be "connected to" another object, it can be directly connected to the other object or there can be an intermediate object at the same time.
[0037] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more related listed items.
[0038] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0039] In the first aspect, the present application provides a positive electrode lithium supplement material, please refer to Figure 1 , including a core 10, a catalytic layer 20 and a protective layer 30; wherein the core 10 includes lithium-rich particles; the catalytic layer 20 is coated on the outer surface of the core 10, the catalytic layer 20 contains a catalyst, and the catalyst contains a metal element M1; the protective layer 30 is coated on the outer surface of the catalytic layer 20, the protective layer 30 includes a metal oxide, the metal oxide contains a metal element M2, and the metal elements M1 are different from M2.
[0040] Specifically, the inner core 10 includes lithium-rich particles (which may be nanometer-sized) smaller than the inner core particle size, and the inner core may include one or more lithium-rich particles.
[0041] The lithium-rich particles are lithium source nuclei for lithium replenishment. The positive electrode lithium replenishment material with the lithium-rich particles constituting the core 10 is added to the electrode so that during the first cycle of charging, it acts as a "sacrificial agent" to release all the lithium ions contained in it at once as much as possible to replenish the irreversible lithium ions consumed by the formation of the SEI film at the negative electrode, thereby maintaining the abundance of lithium ions in the battery system and improving the first efficiency and overall electrochemical performance of the battery.
[0042] Optionally, the lithium-rich particles include binary lithium-rich compounds (particles), the chemical formula of which includes Li x Ky , wherein K is one or more elements selected from S, P, N, I, Br, F, O, B, and Se, 1≤x≤5, and 0<y. Specifically, the lithium-rich particles may be one or more selected from lithium sulfide (Li2S), lithium selenide (Li2Se), lithium phosphide (Li3P), lithium iodide (LiI), and lithium bromide (LiBr).
[0043] Compared with other positive electrode lithium replenishment materials, positive electrode lithium replenishment materials made of binary lithium-rich compounds have weaker binding forces between lithium ions and anions, smaller polarization of binary lithium-rich compounds, and lower voltage platform required for charging, which can effectively reduce the activation barrier of binary lithium-rich compounds, thereby significantly improving the efficiency of lithium ion deintercalation, so that positive electrode lithium replenishment materials can have higher lithium replenishment specific capacity. In addition, binary lithium-rich compounds do not produce oxygen during the lithium replenishment process, which can reduce the risk of flatulence in lithium batteries.
[0044] In other embodiments, the lithium-rich particles further include ternary lithium-rich compounds (particles), the chemical formula of which includes Li a K b O c , wherein K is at least one element selected from Fe, Ni, Mn, Cu, Zn, Co, Cr, Zr, Sb, Ti, V, Mo, and Sn, 1≤a≤8, 0<b, 0<c<7. In a specific embodiment, the lithium-rich oxide may be Li5FeO4, Li6MnO4, Li6CoO4, Li6ZnO4, Li2NiO2, Li2CuO2, Li2CoO2, Li2MnO2, Li2Ni 0.5 Mn 1.5 O4、Li2Ni d Cu (1-d) At least one of O2 (0<d<1), etc.
[0045] In one embodiment, the catalytic layer 20 is obtained by carbonizing a metal organic material (hereinafter referred to as a precursor) and reacting it with non-metallic elements (such as sulfur, selenium and other elements) in lithium-rich particles. The catalytic layer 20 is coated on the outer surface of the inner core 10, and the catalytic layer 20 contains a catalyst (metal compound or metal particles). The catalyst in the catalytic layer 20 is obtained by reacting the non-metallic elements in the lithium-rich particles with the metal elements in the catalytic layer precursor, or by retaining the metal compound in the catalytic layer 20 precursor. Therefore, the catalyst contains the metal element M1, which is the metal element in the precursor.
[0046] Optionally, the catalyst layer precursor has a molecular cage shape with a cage-like structure. Then a lithium source (such as lithium sulfate) is added thereto, and thus the lithium source can be accommodated in the cavity of the precursor. Under high-temperature reaction, the organic matter in the catalyst layer precursor is carbonized into a carbon material, and the carbon material reacts with the lithium source so that the non-metal in the lithium source can be reduced, thereby obtaining lithium-rich particles. Among them, some non-metal elements can also react with the metal element M1 in the catalyst layer precursor to obtain a metal compound.
[0047] It can be understood that during the preparation of the material, the lithium source will enter the space enclosed by the precursor through the cavity in the catalyst layer precursor, as Figure 2 shown. Therefore, before carbonization, the lithium source and the catalyst layer precursor will form a pseudo-coated structure, that is, the core is the lithium source and the outer periphery is the catalyst layer precursor. Then, since the carbon material (hereinafter referred to as the carbon framework) in the catalyst layer precursor after carbonization is consumed by the lithium source, the structure of the carbon framework partially collapses, while the metal compound obtained by the reaction of the metal element M1 is retained. Therefore, the originally outer catalyst layer precursor forms a catalyst layer 20 composed of a metal compound.
[0048] Optionally, the inner side of the cavity of the catalyst layer precursor has hydrophilicity, and the lithium source is a salt solution. Under the drive of concentration and the attraction of the hydrophilic cavity, as much lithium source as possible will be encapsulated into the nano-cavity of the precursor.
[0049] In actual industrial applications, some cathode lithium supplement materials will produce some harmful substances during the discharge lithium supplement process, which will cause harm to the battery. For example, for a cathode lithium supplement material based on lithium sulfide, soluble polysulfide lithium (Li2S n , 2 < n < 8) will be generated after the discharge process, that is, the "shuttle effect". This process not only consumes a large amount of electrolyte, but also results in low utilization rate of sulfur active substances and short cycle life. When other binary lithium-rich compounds are applied to lithium batteries, such as lithium selenide, the "shuttle effect" problem will also be brought.
[0050] In the embodiments of the present application, the catalyst layer 20 contains a metal compound (such as a metal sulfide) with strong catalytic performance. The catalyst (metal compound) in the catalyst layer 20 can accelerate the conversion rate of harmful materials (such as polysulfide lithium) and reduce the cumulative concentration of harmful materials (such as polysulfide lithium) in the electrolyte. For example, iron sulfide has multiple active center catalytic sites, and there is a significant charge transfer with polysulfide lithium, which can well adsorb polysulfide lithium. In addition, its d-band center has a strong interaction with the p orbit of polysulfide, reducing the activation energy barrier for the conversion of polysulfide, increasing the reaction kinetic rate of redox, and promoting its rapid conversion to discharge products.
[0051] Furthermore, the protective layer 30 is also obtained by carbonizing the metal organic material and reacting with the lithium source. The protective layer 30 is coated on the outer surface of the catalyst layer 20, and the protective layer 30 includes a metal oxide. The metal oxide in the protective layer 30 is obtained by reacting the oxygen element in the lithium-rich particles with the metal element M2 in the metal organic material. Therefore, the metal oxide contains the metal element M2, which is the metal element in the precursor.
[0052] It should be explained that the metal element M2 in the protective layer 30 is different from the metal element M1 in the catalytic layer 20 .
[0053] Optionally, the shell precursor of the core-shell structured positive electrode lithium supplement material is a MOFs material. The MOFs material includes a double-layer nested framework, an inner framework close to the core and an outer framework located outside the inner framework, and the inner framework and the outer framework contain different metal elements. Figure 2 As shown, the inner frame 20S (containing metal element M1) reacts with the non-metallic element (non-oxygen) in the lithium source 10S to form a catalytic layer 20; the outer frame 30S (metal element M2) is used to react with the oxygen element in the lithium source 10S to form a protective layer 30. In one embodiment, taking lithium-rich particles as lithium sulfide as an example, the metal element M1 constituting the inner frame 20S is a sulfur-philic metal, and the metal element M2 constituting the outer frame 30S is an oxygen-philic metal.
[0054] So, if Figure 2 As shown, before carbonization, the lithium source 10S and the precursor will form a coating-like structure, that is, the core is the lithium source 10S, and the lithium source 10S has an inner frame 20S and an outer frame 30S. After carbonization, the first carbon frame (the carbide of the inner frame 20S) and the second carbon frame (the carbide of the outer frame 30S) are consumed, resulting in the partial collapse of the structure of the carbon frame, and the metal in the precursor reacts with sulfur (taking lithium sulfide as an example) and oxygen to generate metal sulfide and metal oxide.
[0055] The advantage of using MOFs material as a precursor to make the catalytic layer 20 is that MOFs material has abundant micropores and strong adsorption capacity, and can firmly adsorb the lithium source (lithium salt solution) in its cavity, thereby improving the reaction effect during preparation; and, the lithium source adsorbed in the cavity reacts and grows lithium-rich particles under the confinement of the MOFs material, making it easier to realize nano-sizing of the lithium-rich particles, that is, to obtain lithium-rich particles (kernel 10) with smaller particle size. The small-sized lithium-rich particles can significantly improve the electrochemical properties of the positive electrode lithium supplement material and reduce the activation voltage of the lithium battery.
[0056] The advantage of using MOFs materials as precursors to make the protective layer 30 is that the formed protective layer 30 includes metal oxides with strong hydrophobic properties. In addition, the protective layer 30 made of oxygen-philic metals can react with oxygen elements in the lithium source (such as lithium sulfate), on the one hand eliminating oxygen in the lithium source, and on the other hand fixing oxygen elements in the positive electrode lithium replenishing material to prevent oxygen elements from combining to form oxygen and reacting with the electrolyte during the lithium replenishing process.
[0057] Optionally, the metal element M1 is selected from at least one of Fe, Cu, Zn, In, Cd, Co, and Ni.
[0058] Optionally, the metal element M2 is selected from at least one of Al, Zr, Mg, Cr, Mn, Ca, and Ti.
[0059] The MOFs material includes one or more of MIL-101(Fe), MIL-101(Al), MIL-53(Fe), MIL-53(Al), UiO-66(Zr), MIL-125(Ti), HKUST-1, and PCN-222(Cu).
[0060] For example, the precursor is a core-shell structured MIL-101, the inner framework includes Fe elements, the outer framework includes Al elements, and the lithium source is lithium sulfate. After the precursor and the lithium source are mixed and carbonized, the Fe element reacts with the S element to form FeS, and the Al reacts with the O element to form Al2O3. The core-shell structured MIL-101-based MOFs with a bimetallic source have a sulfur-philic metal (Fe) in the inner layer and an oxygen-philic metal (Al) in the outer layer. The core-shell structured MIL-101 has a high specific surface area and high porosity. The cavity can accommodate gases such as CO2 and biological enzymes, and can also absorb nitrates and phosphates to remove nitrogen and phosphorus.
[0061] The present invention coats the outer surface of the inner core 10 with lithium-rich particles with a catalytic layer 20, and the catalytic layer 20 includes a catalyst. The catalyst can catalyze the conversion of harmful substances in the positive electrode lithium supplement material during the discharge process, such as lithium polysulfide, thereby reducing the accumulated concentration of harmful materials in the electrolyte; and the present invention also coats the outer surface of the catalytic layer 20 with a protective layer 30, and the protective layer 30 includes a stable metal oxide, so that the protective layer 30 can reduce the erosion of the inner core 10 by external water vapor, thereby effectively improving the problem of material deterioration in humid air to generate residual alkali and harmful odorous gases, thereby This avoids the gelation of the mixture and the loss of active components. At the same time, the catalytic layer 20 and the protective layer 30 in the present invention are prepared by MOFs materials with a core-shell structure. During the preparation process, the high specific surface area, high porosity and nanopore cage effect of MOFs are utilized to effectively prepare lithium-rich particles with smaller particle size, thereby improving the electrochemical properties of the positive electrode lithium supplement material, especially improving the ion and electronic conductivity, and reducing the activation voltage of the lithium battery to adapt to the low-voltage electrolyte system (if the activation voltage of the lithium battery is too high, the electrolyte is unstable and easy to decompose), further improving the coulombic efficiency of the lithium battery.
[0062] In one embodiment, the catalyst includes a metal compound and metal particles, and the metal particles are the same as the metal element in the metal compound (i.e., both are metal elements M1). Specifically, based on the above embodiment, the metal element M1 in the inner frame is not combined with some non-metallic elements (such as sulfur) in the lithium source. Therefore, the catalyst layer 20 includes metal particles.
[0063] For example, the inner frame includes Fe element, and the catalyst layer 20 may include FeS and metal element Fe.
[0064] The metal particles in the catalyst layer 20 also have a catalytic effect and can catalyze the conversion of harmful substances (such as lithium polysulfide). In addition, compared with metal compounds, metal particles have stronger conductivity, which can reduce the internal resistance in the catalyst layer 20 and improve the efficiency of lithium ion extraction.
[0065] In one implementation, please refer to Figure 3 The catalytic layer 20 includes a first porous carbon mesh 20A, and the catalyst is distributed in the first porous carbon mesh 20A; and / or, the protective layer 30 includes a second porous carbon mesh 30A, and the metal oxide is distributed in the second porous carbon mesh 30A.
[0066] Specifically, based on the above-mentioned embodiment, in the precursor of the core-shell structure, the inner frame and the outer frame are two different single-layer metal organic frameworks, the metal elements in the inner frame and the outer frame are different, and the organic ligands used are also different. The inner frame and the outer frame independently form a nested double-layer cage structure. Therefore, the carbonized carbon frame can be a porous carbon mesh structure, that is, the inner frame in the above-mentioned is converted into the first porous carbon mesh 20A, and the outer carbon frame is converted into the second porous carbon mesh 30A. It can be understood that the porous carbon mesh can be regarded as a single-layer mesh structure.
[0067] When the first porous carbon net 20A and the second porous carbon net 30A are not completely consumed or are not consumed, at least a portion of the porous carbon net remains in the catalytic layer 20 or the protective layer 30. Figure 4 As shown, taking the first porous carbon mesh 20A as an example, it includes a carbon skeleton (first porous carbon mesh 20A) and a catalytic site 20B. Among them, the catalytic site 20B is a single catalyst molecule (or atom), such as a metal compound or metal particle, and the carbon skeleton is used to connect two adjacent catalytic sites 20B. Thereby, the position of part of the catalytic layer 20 is presented in the form of a porous carbon mesh. The second porous carbon mesh 30A is also the same, which will not be repeated here.
[0068] The porous carbon mesh in the catalyst layer 20 and the protective layer 30 can improve the conductivity of the layers, thereby improving the efficiency of lithium ion release. In addition, the porous carbon mesh retained by the carbon framework is more likely to form a continuous carbon structure. The advantage of this structure is that a fast ion channel can be formed using a continuous porous carbon mesh, thereby further improving the efficiency of lithium ion release.
[0069] In another embodiment, please refer to Figure 5 The positive electrode lithium supplement material also includes a porous carbon framework 40, lithium-rich particles are accommodated in the inner cavity of the porous carbon framework 40 and / or attached to its skeleton, the catalyst is embedded in the skeleton inside the porous carbon framework 40 to form a catalytic layer 20; and / or, the metal oxide is embedded in the skeleton outside the porous carbon framework 40 to form a protective layer 30.
[0070] Specifically, on the basis of the above-mentioned implementation mode, the precursor of the positive electrode lithium supplement material includes a bimetallic organic framework, that is, the inner layer framework and the outer layer framework are two metal organic frameworks with the same structure (using the same organic ligand), and only the metal elements in the framework distribution are different. After the bimetallic organic framework is converted into a porous carbon framework through a carbonization reaction, a catalytic layer 20 is formed on the inner side of the porous carbon framework, and a protective layer 30 is formed on the outer side.
[0071] When the porous carbon framework 40 is not completely consumed or is not consumed, at least a portion of the porous carbon framework 40 remains. The metal elements M1 and M2 in the original porous carbon framework 40 react respectively, such as Figure 5As shown, the catalyst generated by the M1 reaction is embedded in the skeleton inside the porous carbon framework 40 to form a catalytic layer 20 , and the metal oxide generated by the M2 reaction is embedded in the skeleton outside the porous carbon framework 40 to form a protective layer 30 .
[0072] The advantage of retaining the porous carbon framework 40 in the catalytic layer 20 and the protective layer 30 is that the porous carbon framework 40 is a three-dimensional skeleton structure, which can provide a larger specific surface area, which is beneficial to increase the attachment sites of lithium-rich particles, thereby increasing the mass proportion of lithium-rich particles in the positive electrode lithium supplement material to enhance the capacity of the material; and the porous carbon framework provides a reaction space for catalyzing lithium polysulfide, and lithium polysulfide can fully combine with the catalyst, thereby improving the catalytic efficiency; and the porous carbon framework also provides a channel for the escape of lithium ions, thereby improving the escape efficiency of lithium ions.
[0073] In one embodiment, in the catalyst layer 20, the content of the catalyst gradually increases from the outer side away from the core 10 to the inner side close to the core 10. It can be understood that the lithium source is mainly contained in the core position of the precursor, that is, Figure 2 As shown. Therefore, the combination of the non-metallic elements in the lithium source and the M1 element is concentrated at the connection between the lithium source and the inner frame, that is, the closer the catalyst layer 20 is to the inner core 10, the more non-metallic elements are contained, and the more catalyst is formed. The advantage of this arrangement is that after the inner core 10 is discharged, the formation of harmful substances (such as lithium polysulfide) is mainly concentrated near the core of the inner core 10, so more harmful substances (such as lithium polysulfide) can be converted via the catalyst, thereby improving the conversion efficiency.
[0074] In one implementation, please refer to Figure 6 The positive electrode lithium supplement material also includes a hydrophobic material (the shaded portion outside the lithium source 10S in the figure), and the hydrophobic material is located in the catalyst layer 20 and / or the protective layer 30, or the hydrophobic material is located between the catalyst layer 20 and the protective layer 30.
[0075] Specifically, based on the above embodiment, before the positive electrode lithium supplement material is carbonized, after the lithium source and the precursor form a coating-like structure (hereinafter referred to as a composite precursor), a certain amount of hydrophobic material (such as organosilane) can be added therein, and the hydrophobic material forms a coating on the surface of the composite precursor. The hydrophobic material is used to lock the lithium source (metal salt) to the inner frame and the outer frame in the above.
[0076] Optionally, the hydrophobic material can be formed on the outer surface of the composite precursor, and can also enter the composite precursor through the holes on the inner frame and the outer frame. The composite precursor includes an inner frame A and an outer frame A, and a lithium source A in the frame, and also includes a hydrophobic material (the shaded part located in the inner frame A and the outer frame A), and the hydrophobic material blocks the lithium source.
[0077] It can be understood that the lithium source exists on the frame in the form of a metal salt solution and can be contained in the frame due to the surface tension of the liquid. Then the coating formed by the hydrophobic material can further lock the water to prevent the loss of the lithium source, thereby preventing the lithium source content from being greatly reduced during carbonization.
[0078] Optionally, the hydrophobic material can be an organic material. The organic material can be organic silane, paraffin, ethane, etc. It can achieve water lock encapsulation, and at the same time, it can also be pyrolyzed as a carbon source to participate in the reduction of lithium source to form lithium-rich particles. Of course, when using the above materials as hydrophobic materials.
[0079] Optionally, the hydrophobic material can also be a metal organic coordination material or an inorganic material. After carbonization, part of such material can be retained in the obtained positive electrode lithium supplement material, that is, the hydrophobic material mentioned above. It can be understood that the hydrophobic material exists inside and outside the inner frame and the outer frame during preparation, so after preparation, the hydrophobic material can be located in the catalyst layer 20 or the protective layer 30, and can also be located between the catalyst layer 20 and the protective layer 30.
[0080] The above-mentioned hydrophobic material can not only enhance the hydrophobic effect of the protective layer 30 or the catalytic layer 20, but the metal elements contained therein can also enhance the conductivity of the protective layer 30 or the catalytic layer 20 and improve the extraction efficiency of lithium ions.
[0081] In one implementation, please refer to Figure 7 The positive electrode lithium supplement material further includes a hydrophobic material layer 50 , and the hydrophobic material layer 50 is coated on the outer surface of the protective layer 30 .
[0082] Specifically, based on the above-mentioned embodiment, the hydrophobic material outside the protective layer 30 can form a continuous layer, namely, the hydrophobic material layer 50. The hydrophobic material layer 50 is located on the outer surface of the protective layer 30. The hydrophobic material layer 50 can further improve the hydrophobic performance of the material, and when the carbon skeleton is still retained in the catalytic layer 20 or the protective layer 30, the lithium-rich particles on the carbon skeleton are encapsulated to prevent the lithium-rich particles from being exposed.
[0083] In one implementation, please refer to Figure 7 The positive electrode lithium supplement material further includes a conductive carbon layer 60, which is coated on the outer surface of the protective layer 30. Specifically, the conductive carbon layer 60 can be obtained by chemical vapor deposition, that is, the material having the catalytic layer 20 and the protective layer 30 is placed in a mixed atmosphere of organic carbon and inert protective gas in a tube furnace for deposition and coating.
[0084] It is understandable that the purpose of providing the conductive carbon layer 60 is to improve the ionic conductivity of the positive electrode lithium supplement material and further protect the core 10 to prevent the material from being corroded by external water vapor. Moreover, the thickness of the conductive carbon layer 60 prepared by the vapor deposition method is controllable, which can achieve complete coating while reducing the impact on the material capacity.
[0085] In one embodiment, the particle size D50 of the lithium-rich particles is 50 nm to 20 μm. Specifically, the particle size D50 of the lithium-rich particles may be, but is not limited to, 50 nm, 100 nm, 500 nm, 1 μm, 2 μm, 3 μm, 5 μm, 8 μm, 10 μm, 15 μm, or 20 μm.
[0086] The particle size of existing commercial lithium supplements is generally 10μm to 30μm. Due to the insulating properties, the internal volume of most particles hinders the conversion of sulfur, thereby showing a higher potential barrier and lower capacity. In the process of preparation, the embodiment of the present application utilizes the high specific surface area, high porosity and nanopore cage effect of MOFs to adsorb and accommodate lithium-rich particles, which can effectively prepare lithium-rich particles with smaller particle size. The particle size of the particles can be controlled at the nanometer level, thereby improving the electrochemical properties of the positive electrode lithium supplement material, especially improving the ionic and electronic conductivity, and reducing the activation voltage of the lithium battery to adapt to the low-voltage electrolyte system (if the activation voltage of the lithium battery is too high, the electrolyte is unstable and easy to decompose), further improving the coulombic efficiency of the lithium battery.
[0087] By significantly reducing the particle size, nano-scale lithium-rich particles can shorten the diffusion length and expand the active specific surface area, which is conducive to the insertion and extraction of lithium ions, thereby increasing the capacity of lithium-supplementing materials. When the particle size of lithium-rich particles is smaller than the above range, the difficulty of preparation increases, and the particles will form relatively serious agglomerations; when the particle size of lithium-rich particles is larger than the above range, the specific surface area of lithium-rich particles decreases, reducing the insertion and extraction efficiency of lithium ions, resulting in poor lithium-supplementing effect of positive electrode lithium-supplementing materials.
[0088] In one embodiment, the thickness of the catalyst layer is 2 nm to 10 nm. Specifically, the thickness of the catalyst layer can be, but is not limited to, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, and 10 nm.
[0089] Since the catalytic layer is obtained by MOFs material, the catalytic layer provided by the present application has a thinner thickness compared to the existing coating method. While providing a catalytic effect, it can also reduce the mass proportion of non-lithium compounds in the positive electrode lithium replenishing material, thereby increasing the lithium replenishing capacity of the positive electrode lithium replenishing material.
[0090] When the thickness of the catalytic layer is less than the above range, the catalytic layer does not completely cover the inner core, which is not conducive to the conversion of lithium polysulfide; when the thickness of the catalytic layer is greater than the above range, since the catalytic layer does not contribute lithium ions, the overall gram capacity of the positive electrode lithium supplement material will be reduced.
[0091] In one embodiment, the thickness of the protective layer is 3 nm to 15 nm. Specifically, the thickness of the protective layer can be, but is not limited to, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, and 15 nm.
[0092] It is understandable that the protective layer is formed in the same way as the catalytic layer, so the protective layer is also thinner than the existing encapsulation layer. While providing hydrophobicity to prevent corrosion, it can also reduce the mass proportion of non-lithium compounds in the positive electrode lithium replenishing material, thereby increasing the lithium replenishing capacity of the positive electrode lithium replenishing material.
[0093] When the thickness of the protective layer is less than the above range, the protective layer does not completely cover the core, which is not conducive to providing a hydrophobic environment for the core and the catalytic layer; when the thickness of the protective layer is greater than the above range, since the protective layer does not contribute lithium ions, the overall gram capacity of the positive electrode lithium supplement material will be reduced.
[0094] In one embodiment, the mass ratio of the core, the catalytic layer, and the protective layer is 100:(0.01-50):(0.01-50). Specifically, the mass ratio of the core, the catalytic layer, and the protective layer can be, but is not limited to, 100:0.01:0.01, 100:50:50, 100:5:0.01, 100:10:0.01, 100:30:0.01, 100:50:0.01, 100:0.01:5, 100:0.01:10, 100:0.01:30, 100:0.01:50, 100:10:30, 100:30:30, 100:20:50, 100:10:50.
[0095] By controlling the mass ratio of the inner core, the catalytic layer and the protective layer within the above range, not only can the conversion of harmful substances (such as polysulfides) in the positive electrode lithium replenishment material be ensured, but also it can be ensured that the positive electrode lithium replenishment material has a higher hydrophobic property, which can avoid the problem of the material absorbing water to produce residual alkali and harmful gases, and the positive electrode lithium replenishment material can also have a higher lithium replenishment capacity.
[0096] When the proportion of the inner core is smaller than the above range, the mass proportion of the catalytic layer or the protective layer is too high. Since the catalytic layer and the protective layer do not contribute lithium ions, the overall gram capacity of the positive lithium supplement material will be reduced. When the proportion of the inner core is larger than the above range, the mass proportion of the catalytic layer or the protective layer is too small, which may lead to incomplete coating, resulting in part of the coating being too thin, or part of the inner core being exposed to the external environment.
[0097] In one embodiment, the thickness of the conductive carbon layer is 1 nm to 5 μm. Optionally, the thickness of the conductive carbon layer can also be 1 nm to 100 nm, 1 nm to 50 nm, or 25 nm to 50 nm. When the thickness of the conductive carbon layer is less than the above range, it is difficult for the conductive carbon layer to provide sufficient stability and conductivity; when the thickness of the conductive carbon layer is greater than the above range, it will affect the transmission rate of lithium ions and the capacity of the material.
[0098] In the second aspect, the present application also provides a method for preparing a positive electrode lithium supplement material, please refer to Figure 8 , specifically used for preparing the positive electrode lithium supplement material in the first aspect. The preparation method comprises the following steps:
[0099] Step S10, providing a metal organic framework with a core-shell structure, wherein the metal organic framework comprises an inner layer framework and an outer layer framework.
[0100] Step S20, mixing the lithium source and the metal organic framework and sintering them to obtain a positive electrode lithium supplement material, wherein the lithium source forms the inner core, the inner framework forms the catalytic layer, and the outer framework forms the protective layer.
[0101] Specifically, in step S10, the method for preparing the metal organic framework of the core-shell structure is:
[0102] The sulfophilic metal salt (M1) and the organic ligand are added in a molar ratio to a flask containing a certain amount of N, N-dimethylformamide (DMF) solvent, mixed and stirred evenly, and a certain amount of stabilizer and dispersant are added. Under heating conditions, the solvent heats to form inner layer framework seeds. Then, an appropriate amount of oxophilic metal salt (M2) is ultrasonically dissolved in a mixed solution of a certain amount of DMF and a formulation agent, and slowly added to the flask with a peristaltic pump. M2 is deposited on the surface of the inner layer framework seeds and continues to self-assemble with the organic ligand to synthesize a core-shell structured metal organic framework (core-shell structure MOFs).
[0103] Optionally, the obtained sample is centrifuged and washed with methanol for multiple times to remove unreacted organic ligands, and then vacuum dried overnight at a certain temperature to obtain a metal organic framework (M1@M2) for standby use.
[0104] In step S20, the metal organic framework (M1@M2) of the core-shell structure prepared in step S20 is immersed in an appropriate amount of n-hexane solution, and then added with a lithium source solution of a certain concentration, and stirred until the metal salt aqueous solution enters the cavity in a directional manner.
[0105] Optionally, after the metal salt aqueous solution (lithium source) is introduced into the cavity, a certain amount of hydrophobic material can be added, which is dissolved in n-hexane and forms a coating on the surface of the metal organic framework (M1@M2) to lock the metal salt aqueous solution. The obtained sample is centrifuged and washed with methanol, and placed in a freeze dryer for freeze drying.
[0106] Then, the prepared metal organic framework (M1@M2) with a hydrophobic coating core-shell structure is passed through a 200-mesh sieve, placed in a porcelain boat, and placed in a tubular furnace for carbon thermal reduction under an inert atmosphere. The lithium source reacts with the carbon skeleton to generate lithium-rich particles, that is, the core is formed. Some sulfur-philic metal atoms combine with sulfur to form a catalytic layer with high catalytic conversion activity, while oxygen-philic metal atoms combine with oxygen elements in the ligand to form a protective layer, that is, the positive electrode lithium supplement material is obtained.
[0107] Optionally, after step S20, the method may further include: passing the positive electrode lithium replenishing material prepared in step S20 through a 300-mesh sieve, spreading it flat in a porcelain boat, and placing it in a tubular furnace under a mixed atmosphere of organic carbon and inert protective gas for chemical vapor deposition coating to obtain a positive electrode lithium replenishing material with a conductive carbon layer.
[0108] Optionally, in the above step S10, the thiophilic metal salt (M1) includes at least one of iron acetylacetonate, copper acetylacetonate, and chromium acetylacetonate.
[0109] Optionally, in the above step S10, the oxophilic metal salt (M2) includes at least one of aluminum chloride, aluminum nitrate, aluminum sulfate, zirconium chloride, zirconium citrate, titanium tetrachloride, and titanium bromide.
[0110] Optionally, in the above step S10, the organic ligand includes at least one of 2-methylimidazole, terephthalic acid, trimesic acid, 2,4,6-tri-(4-pyridyl)pyridine, 3,5-di(4-carboxyphenyl)pyridine, tetracarboxyphenylporphyrin, and 2,4,6-tri(2-pyridyl)triazine.
[0111] Optionally, in the above step S10, the stabilizer and dispersant include at least one of polyvinyl pyrrolidone (PVP), polyacrylic acid (PAA), polyacrylamide (PAM), polyethylene glycol (PEG), polyvinyl alcohol (PVA), cetyltrimethylammonium bromide (CTAB), and sodium dodecylbenzene sulfonate (SDBS).
[0112] Optionally, in the above step S10, the formulation agent includes at least one of formic acid, acetic acid, citric acid, hydrofluoric acid, and hydrochloric acid.
[0113] Optionally, in the above step S10, the mass ratio of M1:M2:organic ligand:stabilizer:formulating agent is 1:(0.1-20):(0.1-40):(0.1-10):(0.1-25).
[0114] Among them, when the content ratio of M1 is too low, the mass ratio of the inner framework is small, resulting in less catalyst in the catalytic layer. When the content ratio of M1 is too high, it will compete with M2 for organic ligands, and too much metal sulfide will be formed after carbon thermal reduction, which reduces the proportion of active lithium sulfide. When the content ratio of M2 is too low, it is not enough to form a uniform and effective protective layer in the later stage. When the content ratio of M2 is too high, the protective layer is too thick, which is not conducive to the migration of lithium. If the proportion of organic ligands is too low, it is difficult to coordinate the metal ions completely, the crystallinity of the material is low, and the low proportion of organic ligands is prone to insufficient ligands and M2 to grow on the surface of the metal organic framework. If the proportion of organic ligands is too high, it will increase the nucleation points in the solvent, accelerate the crystal synthesis rate, and the product structure is easy to cross, affecting the formation of the core-shell structure. The proportion of the stabilizer is too low to play a dispersing role, and the nanoparticles will still agglomerate and be uneven. If the proportion is too high, it will limit the interface reaction and affect the crystal growth. If the proportion of the regulator is too low, the solubility and deprotonation ability of the organic ligand will be insufficient. If the proportion is too high, the deprotonation of the organic ligand will be significantly affected and there is a possibility of causing the framework structure to collapse.
[0115] Optionally, in the above step S10, the solvent thermal temperature is selected to be 80° C. to 160° C., and more preferably 100° C. to 150° C. If the temperature is too low, sufficient energy cannot be obtained to overcome the energy barrier and the metal organic framework cannot be formed. If the temperature is too high, the nucleation rate is too fast, the crystal growth is uneven, and the organic solvent evaporates or even decomposes.
[0116] Optionally, in the above step S10, the solvent thermal reaction time is preferably 12 h to 18 h.
[0117] Optionally, in the above step S20, the concentration of the lithium source (metal salt solution) is 10 mg / mL to 500 mg / mL, more preferably 10 mg / mL to 100 mg / mL, further preferably 50 mg / mL to 100 mg / mL, and further preferably 75 mg / mL to 100 mg / mL. When the concentration of the lithium source (metal salt solution) is too low, the concentration difference driving force entering the metal organic framework cavity is low, affecting the packaging amount. When the concentration of the lithium source (metal salt solution) is too high, it causes a waste of raw materials, and the introduction of excessive anions or anion groups may affect the growth of crystals.
[0118] Optionally, in the above step S20, the hydrophobic material includes at least one of polydimethylsiloxane (PDMS), perfluorooctyltriethoxysilane, trichloromethylsilane, polytetrafluoroethylene (PTFE), and hexadecyltrimethoxysilane.
[0119] Optionally, in the above step S20, the content of the hydrophobic material is 0.1wt% to 10wt%. When the amount of hydrophobic material added is insufficient, the coating is not dense enough and the ability to lock water-soluble inorganic metal salts is limited. When the amount of hydrophobic material added is too large, it is easy to introduce too many impurity elements and release them after pyrolysis.
[0120] Optionally, in the above step S20, the carbon thermal reduction temperature is selected to be 400° C. to 1000° C., and more preferably 600° C. to 900° C. If the temperature is too low, the material cannot be carbonized or the carbonization is incomplete, the reduction is insufficient, and even the conditions for the start of the carbon thermal reduction reaction cannot be met. The reaction rate is low, the crystallization performance of the material is poor, and impurities are easily generated. If the temperature is too high, the metal is easy to volatilize, and it is also easy to promote secondary crystallization of the crystal, and the specific surface area becomes smaller while the material grains become larger.
[0121] Optionally, in the above step S20, the carbon thermal reduction reaction time is preferably 1 h to 5 h, and the heating rate is preferably 1° C. / min to 10° C. / min.
[0122] Optionally, in the above step S20, the inert atmosphere includes at least one of nitrogen, argon, neon and helium.
[0123] Optionally, after the above step S20, the organic carbon atmosphere includes at least one of methane, acetylene, and propylene.
[0124] The present invention prepares a catalytic layer and a protective layer through MOFs materials, and utilizes the high specific surface area, high porosity and nanopore cage effect of MOFs materials to adsorb a lithium source in a hydrophilic cavity; and in the pyrolysis process, the organic skeleton acts as a carbon source, and MOFs acts as a sacrificial template to form a catalytic layer with catalytic performance and a protective layer with hydrophobic performance. The preparation method can form a catalytic layer and a protective layer at the same time, reducing the cumbersome process steps of multiple coating processes. At the same time, the formed catalytic layer and protective layer can play the role of stabilizing the material and catalyzing the rapid conversion of polysulfides. The structure of this stable multifunctional layer can effectively improve the problem of material deterioration in humid air to generate residual alkali and produce harmful odorous gases, thereby avoiding the loss of mixed gel and active components. In addition, because the double-layer nested structure MOFs has abundant micropores and strong adsorption capacity, it can confine the growth of lithium-rich materials in the cage holes, realize the nano-sizing of materials, significantly improve the electrochemical properties of positive electrode lithium supplement materials, and reduce the activation voltage of lithium batteries. The metal sources in the catalytic layer and the protective layer have different metallic properties and affinities to different non-metallic elements, so two functional layers, protective and catalytic, are formed during the sintering process.
[0125] In a third aspect, the present application also provides a positive electrode plate, which includes a current collector and an active material layer arranged on the current collector, the active material layer includes the positive electrode lithium replenishing material of the first aspect, or the active material layer includes the positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material of the second aspect.
[0126] In one embodiment, the positive electrode sheet includes a positive current collector, and the positive current collector has a positive active layer, and the positive active layer includes components such as positive active materials, positive lithium supplement materials, conductive agents, and binders. The present application does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. The positive current collector includes but is not limited to any one of copper foil and aluminum foil. The positive electrode active material can be a phosphate positive electrode active material and a ternary positive electrode active material. In a specific embodiment, it includes one or more of lithium cobaltate, lithium manganate, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium phosphate, fluorolithium vanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide. The conductive agent includes one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60, and carbon nanotubes, and the content of the conductive agent in the positive electrode active layer is 3wt% to 5wt%. The types of binders include one or more of polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives, and the content of the binder in the positive electrode active layer is 2wt% to 4wt%.
[0127] In one possible implementation, the content of the positive electrode lithium replenishing material in the positive electrode active material can be controlled at 1% to 6% of the mass of the positive electrode active material. This ratio can just make up for the loss of active lithium in the battery during the first charging process. If the amount of positive electrode lithium replenishing material added to the positive electrode plate is too low, the active lithium lost in the positive electrode active material cannot be fully replenished, which is not conducive to improving the energy density and capacity retention rate of the battery. If the amount of positive electrode lithium replenishing material added to the positive electrode active material is too high, the negative electrode lithium plating may become serious and increase the cost. In some specific embodiments, in the positive electrode active material, the mass percentage of the positive electrode lithium replenishing material can be 1%, 2%, 4%, 6%, etc.
[0128] In a fourth aspect, the present application also provides a secondary battery, wherein the secondary battery comprises the above-mentioned positive electrode plate, the above-mentioned positive electrode lithium supplement material is added to the positive electrode plate, or the secondary battery comprises the positive electrode lithium supplement material obtained by the above-mentioned preparation method.
[0129] The technical solution of the present invention is described in detail below through specific embodiments.
[0130] Example 1
[0131] The positive electrode lithium supplement material (C@Al2O3@FeS@Li2S) provided in this embodiment includes a core (Li2S), a catalyst layer (containing FeS), a protective layer (containing Al2O3) and a conductive carbon layer (C). The particle size D50 of lithium sulfide contained in the core is 60nm, and the mass ratio of the core to the catalyst layer and the protective layer is 100:15:20.
[0132] The preparation method is as follows:
[0133] Step 1, add ferric acetylacetonate and terephthalic acid to 50mL of DMF in a mass ratio of 1:4.7 to obtain solutions A and B, add PVP twice the mass of ferric acetylacetonate to solution A, and ultrasonicate for 30min. Pour solution A into a flask, slowly add solution B to A, and stir at 110°C for 6h. Add ferric acetylacetonate and aluminum chloride hexahydrate to 100mL of DMF containing 5mL, continue stirring for 8h, and the mass ratio of ferric acetylacetonate to aluminum chloride hexahydrate is 1:2. Then centrifuge at 8000rpm for 10min, collect the solid, wash alternately with DMF and anhydrous ethanol, repeat the operation 3 times, and dry the powder at 80°C for 12h to obtain the sample MIL-101 (Al@Fe).
[0134] Step 2: Take 10g of the MIL-101 (Al@Fe) core-shell structure MOFs prepared in step 1 and immerse it in 100mL of n-hexane, add 200mL of lithium sulfate aqueous solution with a mass concentration of 80mg / mL, and stir slowly for 2h. Then add a certain amount of organosilane, which dissolves in n-hexane and forms a coating on the surface of MIL-101 (Al@Fe), locking the precursor metal salt of binary lithium supplement such as lithium sulfide. The obtained sample is centrifuged and washed with methanol, and placed in a freeze dryer for freeze drying.
[0135] Step 3, the MIL-101 (Al@Fe) with a hydrophobic coating core-shell structure prepared in step 2 is passed through a 200-mesh sieve, then placed in a porcelain boat, and placed in a tubular furnace for carbon thermal reduction under an inert atmosphere. During this period, the organic hydrophobic layer is pyrolyzed and disappears, and lithium sulfate reacts with the inner carbon skeleton of MOFs to form an inner layer of the lithium-supplemented main material. A small amount of sulfur-philic metal atoms combine with sulfur to form a catalytic layer (FeS) with high catalytic conversion activity, and oxygen-philic metal atoms combine with the oxygen element in the ligand to form a protective layer (Al2O3), thereby obtaining Al2O3@FeS@Li2S.
[0136] Step 4, the Al2O3@FeS@Li2S composite material prepared in step 3 is passed through a 300-mesh sieve, spread flat on a porcelain boat, and placed in a tubular furnace in a mixed atmosphere of organic carbon and inert protective gas for chemical vapor deposition coating to obtain C@Al2O3@FeS@Li2S.
[0137] Among them, the MOFs precursor MIL-101 (Al@Fe) used has a spindle-shaped morphology and a specific surface area of 1137m 2 / g, the porosity is 16% for micropores and 49% for mesopores.
[0138] For further information, please refer to Fig. 9 and Fig.10 . Fig. 9 The particles shown in the figure are the framework structure obtained after step 1 in Example 1. It can be clearly observed that the morphology of MIL-101 (Al@Fe) is spindle-shaped. Fig.10 The particles shown in the figure are the framework structure obtained after step 2 in the embodiment. It can be observed that the morphology of MIL-101 (Al@Fe) after the introduction of lithium sulfate still retains the original framework structure and is still spindle-shaped.
[0139] Example 2
[0140] The positive electrode lithium supplement material (C@Al2O3@FeS@Li2S) provided in this embodiment includes a core (Li2S), a catalytic layer (containing FeS), a protective layer (containing Al2O3) and a conductive carbon layer (C).
[0141] The parameters and method of making the materials are the same as those in Example 1. The difference is that the MOFs precursor MIL-53 (Al@Fe) used is octahedral in shape and has a specific surface area of 1137 m 2 / g, the porosity is 16% for micropores and 49% for mesopores. The other material parameters are the same as those in Example 1.
[0142] Example 3
[0143] The positive electrode lithium supplement material (Al2O3@FeS@Li2S) provided in this embodiment includes a core (Li2S), a catalyst layer (containing FeS) and a protective layer (containing Al2O3).
[0144] The parameters and method of making the materials are the same as those in Example 1. The difference is that the precursor MIL-101 (Al@Fe) used has a spindle-shaped morphology and a specific surface area of 968 m 2 / g, the porosity is 11% for micropores and 67% for mesopores. And, the outermost conductive carbon layer is not included.
[0145] Example 4
[0146] The positive electrode lithium supplement material (C@Al2O3@FeSe@Li2Se) provided in this embodiment includes a core (Li2Se), a catalytic layer (containing FeSe), a protective layer (containing Al2O3) and a conductive carbon layer (C).
[0147] The material used is a lithium source containing selenium, and the method is the same as that in Example 1. The difference is that the precursor MIL-101 (Al@Fe) used has a spindle-like morphology and a specific surface area of 831 m 2 / g, the porosity is 16% for micropores and 58% for mesopores.
[0148] Example 5
[0149] The positive electrode lithium supplement material (C@TiO2@CuS@Li2S) provided in this embodiment includes a core (Li2S), a catalytic layer (containing CuS), a protective layer (containing TiO2) and a conductive carbon layer (C).
[0150] The parameters and method of making the materials are the same as those in Example 1. The difference is that the precursor MIL-101 (Ti@Cu) has a spindle-like morphology and a specific surface area of 872 m 2 / g, the porosity is 13% for micropores and 54% for mesopores.
[0151] Example 6
[0152] The positive electrode lithium supplement material (C@Al2O3@FeS@Li2S) provided in this embodiment includes a core (Li2S), a catalytic layer (containing FeS), a protective layer (containing Al2O3) and a conductive carbon layer (C).
[0153] The preparation method is the same as that in Example 1. The difference is that the mass ratio of the core to the catalytic layer and the protective layer is 100:1:20; the precursor MIL-101 (Al@Fe) has a spindle shape and a specific surface area of 1028 m 2 / g, the porosity is 17% for micropores and 56% for mesopores.
[0154] Example 7
[0155] The positive electrode lithium supplement material (C@Al2O3@FeS@Li2S) provided in this embodiment includes a core (Li2S), a catalytic layer (containing FeS), a protective layer (containing Al2O3) and a conductive carbon layer (C).
[0156] The preparation method is the same as that in Example 1. The difference is that the mass ratio of the core to the catalytic layer and the protective layer is 100:15:0.6; the precursor MIL-101 (Al@Fe) has a spindle shape and a specific surface area of 916 m 2 / g, the porosity is 23% for micropores and 47% for mesopores.
[0157] Comparative Example 1
[0158] There is no need to provide a precursor of the metal-organic framework, and the positive electrode lithium supplement material directly uses commercially available micron-sized lithium sulfide.
[0159] Comparative Example 2
[0160] The difference from Example 1 is that only a protective layer and a carbon layer (C@Al2O3@Li2S) are included, and the MOFs precursor used is a single-layer metal aluminum organic framework.
[0161] Comparative Example 3
[0162] The difference from Example 1 is that only a catalytic layer and a carbon layer (C@FeS@Li2S) are included, and the MOFs precursor used is a single-layer metallic iron organic framework.
[0163] The positive electrode lithium replenishing materials provided in the above-mentioned Examples 1-7 and the positive electrode lithium replenishing materials provided in Comparative Examples 1-3 are respectively assembled into positive electrode sheets and lithium ion batteries according to the following methods:
[0164] Positive electrode: The positive electrode lithium supplement material, SP and PVDF are mixed in a mass ratio of 90:4:6 to prepare a positive electrode slurry, the positive electrode slurry is coated on the surface of an aluminum foil, vacuum dried at 110°C overnight, and rolled to obtain a positive electrode sheet;
[0165] Negative electrode: Graphite, carboxymethyl cellulose (CMC), SBR and SP were mixed in a mass ratio of 95.8:1.2:2:1, and the mixture was ball-milled and stirred to obtain a negative electrode slurry. The negative electrode slurry was coated on the surface of copper foil, and vacuum dried at 110°C overnight to obtain a negative electrode sheet.
[0166] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF6 was added to form an electrolyte, and the concentration of LiPF6 was 1 mol / L;
[0167] Diaphragm: Polypropylene microporous separator;
[0168] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of graphite negative electrode sheet - separator - electrolyte - positive electrode sheet.
[0169] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery embodiment was tested under the following test conditions:
[0170] Constant current and constant voltage charging, the first cycle charge and discharge voltage is 2.5-4.3V, the current is 0.1C, and the cut-off current is 0.01C.
[0171] Activation voltage test method:
[0172] This is observed from the voltage-gram capacity curve obtained from the lithium battery performance test of the blue battery testing system.
[0173] Test method for ionic conductivity:
[0174] Using an electrochemical workstation, a sinusoidal current is applied to the electrode system, and the signal generated by the electrode in response to the current is recorded to obtain an impedance spectrum generated by a series of sinusoidal signals of different frequencies. The internal resistance value Z is obtained from the electrochemical impedance spectroscopy (EIS), and then the ionic conductivity S = L / (Z·A) is calculated, where L is the distance between the two electrodes and A is the electrode area.
[0175] Test method for electronic conductivity:
[0176] The resistivity of the positive electrode lithium supplement material in each embodiment and comparative example was calculated and tested by a four-probe method, and the electronic conductivity was obtained by taking the inverse of the resistivity.
[0177] The water absorption rate test method is as follows:
[0178] First, control the room humidity at 25°C, 30-35% relative humidity.
[0179] Second, take out 0.3-0.5g of sample from the glove box, one sample at a time, and take out another sample from the glove box after the test.
[0180] Third, place the weighing bottle in an analytical balance with a precision of 1 part per 100,000, close the door, and reset to zero.
[0181] Fourth, weigh 0.17-0.19 grams of the sample to be tested into the container, spread the material with a spoon, close the hatch, stabilize for 3-5 seconds, turn on the timer, and record the mass of the analytical balance as the value of 0min. Then record the values of 5min, 10min, 15min, and 20min respectively, and calculate the average absorption data for 10-20 minutes.
[0182] Calculation formula:
[0183] V=(w t2 -w t1 ) / w0*(t2-t1); unit: ppm / s. Where t1 and t2 represent time, w0 represents initial mass, and w t1 represents the mass at t1, w t2 represents the mass at t2.
[0184] The test results are shown in Table 1 below:
[0185] Table 1. Test results of materials and batteries in Examples and Comparative Examples
[0186]
[0187] From the test results of Examples 1-7 and Comparative Example 1 in Table 1, it can be seen that the initial charging capacity, lithium replenishment gram capacity, ion conductivity and electronic conductivity of the battery provided by Examples 1-7 are all higher than those of Comparative Example 1, while the activation voltage and water absorption rate are both lower than those of Comparative Example 1. This indicates that the positive electrode lithium replenishment material provided by the present application has higher electrochemical properties and lower corrosion resistance than conventional lithium replenishment materials currently on the market.
[0188] Furthermore, the first charge gram capacity and lithium supplement gram capacity of Comparative Example 1 are reduced by 25.45% and 25.79% respectively compared with Example 1. Because the lithium sulfide particle size in Comparative Example 1 is relatively large, and the sulfur element and lithium sulfide have strong insulation and are not easy to conduct electricity, the sample ion transmission efficiency is low, the redox reaction is slow, the activation voltage rises to 3.78V, and the conductivity is greatly reduced, and the uncoated lithium sulfide cannot cope well with moisture in the air. After the coated lithium sulfide (Example 1), the lithium sulfide is restricted to be coated in the catalytic layer and the protective layer. The reduction in the sample particle size allows the active material to fully contact with the electrolyte, the ion transmission distance is shortened, the rate is accelerated, and the required activation voltage is significantly reduced. At the same time, the conductivity and air stability of the sample are significantly improved.
[0189] From the test results of Example 1 and Comparative Examples 2 and 3 in Table 1, it can be seen that the battery first charge capacity, lithium replenishment gram capacity, ionic conductivity and electronic conductivity provided by Example 1 are higher than those of Comparative Examples 2 and 3, while the activation voltage and water absorption rate are lower than those of Comparative Examples 2 and 3. Because Comparative Example 2 lacks the help of a catalyst, the power of the conversion of long-chain lithium polysulfide to short-chain lithium sulfide is reduced, and the utilization rate of active lithium sulfide is reduced; and Comparative Example 3 lacks a protective layer, so the material's ability to resist water absorption is weakened and the water absorption rate is increased. This shows that the double-layer coated positive electrode lithium replenishment material solution provided in this application is more superior than the single-layer coated lithium replenishment material, and the double-layer coated positive electrode lithium replenishment material has higher electrochemical properties and lower corrosion resistance.
[0190] From the test results of Example 1 and Example 2 in Table 1, it can be seen that the performance of the positive electrode lithium supplement material obtained by using different MOFs precursor structures (spindle-shaped and octahedral) is also different. Among them, the MIL-53 framework is mainly centered on the metal oxygen octahedron, which coordinates with organic matter to form a one-dimensional rhombus channel. Although there is mutual conversion between large pores and narrow pores, and the adsorption capacity is strong, it is not as affinity to water solvent as the three-dimensional cage structure of the MIL-101 framework. Therefore, less lithium sulfate is introduced, and the final lithium sulfide is also less, resulting in the first charge gram capacity and lithium supplement gram capacity of Example 2 being lower than that of Example 1.
[0191] From the test results of Example 1 and Example 3 in Table 1, it can be seen that when the outermost conductive carbon layer is not added, the first charge gram capacity and lithium replenishment gram capacity of Example 3 are relatively low, and the electronic conductivity of the material decreases. This is because the lack of the assistance of the conductive carbon layer causes the overall conductivity of the positive electrode lithium replenishment material to decrease. In addition, due to the lack of further protection provided by the conductive carbon layer, the water absorption rate of Example 3 is increased by 43.55% compared with Example 1.
[0192] It can be seen from the test results of Example 1 and Example 4 in Table 1 that the solution provided by the present application is also applicable to other lithium-rich materials, and can reduce the activation voltage and water absorption rate of the material while ensuring the initial charge gram capacity and lithium replenishment gram capacity of the material. This shows that the solution has high universality and can be applied to different lithium-rich materials for use in large-scale commercial production.
[0193] From the test results of Example 1 and Example 5 in Table 1, it can be seen that the performance of the lithium-rich material is improved differently by using different metal sources and reacting the catalytic layer and protective layer. The first charge gram capacity and lithium replenishment gram capacity of Example 5 are lower than those of Example 1, because the catalytic effect of CuS is not as good as FeS, and the inhibitory effect of titanium oxide on the shuttle effect of lithium sulfide is weaker. However, the water absorption rate of Example 5 is smaller, and it is less likely to cause the lithium replenisher to deteriorate after contact with water, because compared with the 1137m of MIL-101 (Fe@Al), the lithium replenisher has a lower water absorption rate than the 1137m of MIL-101 (Fe@Al). 2 / g specific surface area, MIL-101 (Cu@Ti) has a lower specific surface area, which is caused by lower sensitivity to contact with external water vapor.
[0194] From the test results of Example 1 and Example 6 in Table 1, it can be seen that the electrochemical performance of Example 6 is lower than that of Example 1, and the difference between the two is that the mass ratio of the catalyst layer and the protective layer in Example 7 is different (1:20). This shows that the content of sulfide in the positive electrode lithium supplement material has a greater impact on the performance of the lithium supplement material. Too little of this layer leads to insufficient catalytic activity, polysulfide is still difficult to convert, and too much insoluble lithium sulfide is deposited, resulting in loss of active lithium. On the other hand, the content of the metal oxide layer is relatively high, which helps to reduce the water absorption rate, but it will also increase the migration resistance of lithium and sulfides of different valence states, ultimately resulting in poor lithium supplement performance.
[0195] From the test results of Example 1 and Example 7 in Table 1, it can be seen that the electrochemical performance (gram capacity of the first charge and gram capacity of lithium replenishment) of Example 7 is lower than that of Example 1, and the water absorption rate is increased more. The difference between the two is that the mass ratio of the catalyst layer and the protective layer in Example 7 is different (15:0.6). This shows that the role of the catalyst in the positive electrode lithium replenishment material will not be greatly improved with the increase of sulfide; on the contrary, if there are too many metal sulfides, the content of the main material lithium sulfide will be reduced, and the theoretical gram capacity will decrease; and the proportion of the protective layer is reduced, which is not enough to resist moisture, and the material is easy to deteriorate, resulting in a decrease in lithium replenishment performance.
[0196] In the description of the embodiments of the present application, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship of the accompanying drawings, which are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.
[0197] What is disclosed above is only a preferred embodiment of the present application, and it certainly cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiment and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.
Claims
1. A positive electrode lithium supplement material, characterized in that: include: The inner core includes lithium-rich particles; A catalytic layer, coated on the outer surface of the inner core, the catalytic layer contains a catalyst, the catalyst contains a metal element M1, and the catalytic layer is obtained by carbonizing a metal organic material and reacting with a non-metallic element in the lithium-rich particle; A protective layer is coated on the outer surface of the catalytic layer. The protective layer includes a metal oxide. The metal oxide includes a metal element M2. The metal element M1 is different from the metal element M2. The protective layer is obtained by carbonizing the metal organic material and reacting it with a lithium source.
2. The positive electrode lithium supplement material according to claim 1, characterized in that: The catalytic layer includes a first porous carbon mesh, and the catalyst is distributed in the first porous carbon mesh; and / or the protective layer includes a second porous carbon mesh, and the metal oxide is distributed in the second porous carbon mesh.
3. The positive electrode lithium supplement material according to claim 1, characterized in that: The positive electrode lithium supplement material also includes a porous carbon framework, the lithium-rich particles are accommodated in the inner cavity of the porous carbon framework and / or attached to its skeleton, the catalyst is embedded in the skeleton inside the porous carbon framework to form the catalytic layer; and / or the metal oxide is embedded in the skeleton outside the porous carbon framework to form the protective layer.
4. The positive electrode lithium supplement material according to claim 1, characterized in that: In the catalytic layer, the content of the catalyst gradually increases from the outer side far from the inner core to the inner side close to the inner core.
5. The positive electrode lithium supplement material according to claim 1, characterized in that: The positive electrode lithium supplement material further includes a hydrophobic material, and the hydrophobic material is distributed in the catalyst layer and / or the protective layer; and / or, The positive electrode lithium supplement material further includes a hydrophobic material layer, and the hydrophobic material layer is coated on the outer surface of the protective layer.
6. The positive electrode lithium supplement material according to claim 1, characterized in that: The positive electrode lithium supplement material further includes a conductive carbon layer, and the conductive carbon layer is coated on the outer surface of the protective layer.
7. The positive electrode lithium supplement material according to claim 4, characterized in that: The lithium-rich particles include a binary lithium-rich compound, the general chemical formula of which is Li x K y , K is selected from any one of S, P, N, Br, I, F, O, B, Se, 1≤x≤5, 0<y; And / or, the catalyst is a compound composed of a metal element M1 and a non-metal element K; And / or, the metal element M1 is selected from at least one of Fe, Cu, Zn, In, Cd, Co and Ni; And / or, the metal element M2 is selected from at least one of Al, Zr, Mg, Cr, Mn, Ca, and Ti; And / or, the particle size D50 of the lithium-rich particles is 50 nm to 20 μm; And / or, the thickness of the catalytic layer is 2nm to 10nm; And / or, the thickness of the protective layer is 3nm to 15nm; And / or, the mass ratio of the inner core, the catalytic layer and the protective layer is 100:(0.01-50):(0.01-50).
8. A method for preparing a positive electrode lithium supplement material, characterized in that: include: Providing a double-layer metal organic framework, the metal organic framework comprising an inner layer framework and an outer layer framework; The lithium source and the metal organic framework are mixed and sintered to obtain the positive electrode lithium supplement material, wherein the lithium source forms the inner core, the inner layer framework forms the catalytic layer, and the outer layer framework forms the protective layer.
9. A positive electrode sheet, characterized in that: The positive electrode plate includes a current collector and an active material layer disposed on the current collector, the active material layer includes the positive electrode lithium replenishing material according to any one of claims 1 to 7, or the active material layer includes the positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material according to claim 8.
10. A secondary battery, characterized in that: The positive electrode sheet as claimed in claim 9, or the secondary battery comprises the positive electrode lithium replenishing material as claimed in any one of claims 1 to 7, or the secondary battery comprises the positive electrode lithium replenishing material obtained by the preparation method of the positive electrode lithium replenishing material as claimed in claim 8.
Citation Information
Patent Citations
Positive electrode material and preparation method and battery
CN109560259A
High-activity metal organic gel electrode material as well as preparation method and application thereof