A metal single-atom doped two-dimensional mesoporous carbon composite material and its preparation method

By employing a solution co-assembly strategy and phytic acid assistance, uniform doping of Fe and Co single atoms on two-dimensional Ti3C2Tx nanosheets and assembly of mesoporous carbon were achieved, solving the problem of uneven loading of metal single atoms in existing technologies and improving the new energy storage and catalytic performance of the composite material.

CN117865118BActive Publication Date: 2026-11-10SHANGHAI UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410024835.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-08
Publication Date
2026-11-10
Estimated Expiration
2044-01-08

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve uniform loading and controllable assembly of metal single atoms on mesoporous carbon surfaces in a simple and flexible manner, and the assembly effect of mesoporous carbon on two-dimensional Ti3C2Tx nanosheets is poor.

Method used

Using triblock copolymers poly(ethylene oxide)-poly(propylene oxide)-poly(ethylene oxide) as mesoporous templates, and with the assistance of phytic acid, a solution co-assembly strategy was employed to assemble mesoporous carbon co-doped with single atoms of Fe and Co onto two-dimensional Ti3C2Tx nanosheets. The micelle packing parameters were controlled by hydrogen bonding between the ligands formed by the metal salt and phytic acid, thereby achieving the assembly of spherical and cylindrical pore structures.

Benefits of technology

Uniform doping of single Fe and Co atoms was successfully achieved, forming a composite material with good dispersion, which improves the performance of new energy storage and catalysis and has good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117865118B_ABST
    Figure CN117865118B_ABST
Patent Text Reader

Abstract

This invention relates to a metal single-atom doped two-dimensional mesoporous carbon composite material and its preparation method. The composite material has a two-dimensional sheet-like structure, with mesoporous carbon having columnar and spherical pore structures grown on two-dimensional Ti3C2T. x The nanosheets have Fe and Co metal single atoms uniformly doped into the material structure. The preparation method involves using a triblock copolymer (ethylene oxide-propylene oxide-ethylene oxide) as a mesoporous template, with the aid of phytic acid, and employing a solution co-assembly strategy to assemble Fe and Co single-atom co-doped mesoporous carbon onto a two-dimensional Ti3C2T nanosheet. x On nanosheets. Compared with existing technologies, the composite material of this invention has potential applications in fields such as new energy storage and electrocatalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of inorganic chemistry and materials synthesis technology, and in particular to a two-dimensional mesoporous carbon composite material doped with a single metal atom and its preparation method. Background Technology

[0002] Mesoporous carbon materials, with their excellent electrical conductivity, high specific surface area, and tunable pore structure, show promising application prospects in new energy batteries and catalysis. Mesoporous carbon can not only shorten ion diffusion distances and promote reactant transport, but also effectively increase reactive sites. Studies have shown that assembling mesoporous carbon onto other substrate surfaces can further enhance their reactive properties by leveraging the structural and compositional advantages of the matrix. In recent years, Ti3C2T... x MXene has attracted increasing attention due to its unique two-dimensional layered structure and good electrical conductivity. Assembling mesoporous carbon onto two-dimensional Ti3C2T... x Nanosheets can fully combine the advantages of both, potentially significantly improving their application performance. Furthermore, previous studies have demonstrated that different pore structures have a significant impact on the properties of mesoporous carbon-based composites. However, a simple and flexible method for achieving mesoporous carbon with different pore structures in two-dimensional Ti3C2T nanosheets remains to be seen. x Controllable assembly on nanosheets remains a key focus and challenge in current research.

[0003] On the other hand, metal single atoms, due to their excellent conductivity and high activity, have shown great application potential in fields such as energy storage and conversion. Metal single atoms can not only promote the adsorption of ions on material surfaces but also effectively reduce the diffusion barrier of reactants, thereby significantly enhancing the transport kinetics of the reaction process. However, limited by the different hydrolysis and polymerization rates of metal salts and carbon precursors, it is difficult to achieve uniform loading of metal single atoms on the surface of mesoporous carbon through in-situ strategies. More importantly, there are currently few reports on the direct participation of metal atoms in the assembly process of mesoporous materials. Therefore, this study aims to develop a simple method to obtain metal single-atom-doped mesoporous carbon / Ti3C2T. x Composite materials have significant research and application value. Summary of the Invention

[0004] The purpose of this invention is to provide a two-dimensional mesoporous carbon composite material doped with a single metal atom and a method for its preparation.

[0005] The objective of this invention can be achieved through the following technical solution: a two-dimensional mesoporous carbon composite material doped with a single metal atom, wherein the composite material has a two-dimensional sheet-like structure, and the mesoporous carbon with columnar and spherical pore structures is grown on Ti3C2T x The nanosheets are surfaced with Fe and Co metal single atoms uniformly doped into the material structure.

[0006] The composite material described in this invention is mesoporous carbon / Ti3C2T co-doped with single atoms of metallic Fe and Co. x Composite materials.

[0007] Preferably, the BET specific surface area of ​​the composite material is 150–200 m². 2 / g, and the average pore size is 3-5nm.

[0008] A method for preparing the above-mentioned metal single-atom doped two-dimensional mesoporous carbon composite material, with the assistance of phytic acid, using a triblock copolymer of polyethylene oxide-polypropylene oxide-polyethylene oxide (PEO) 20 PPO 70 PEO 20 Using P123 as a mesoporous template, a solution co-assembly strategy was employed to assemble single-atom co-doped mesoporous carbon of metallic Fe and Co onto a two-dimensional Ti3C2T matrix. x Two-dimensional mesoporous carbon composite material doped with the aforementioned metal single atom was prepared on nanosheets.

[0009] Preferably, the method for preparing the metal single-atom-doped two-dimensional mesoporous carbon composite material includes the following steps:

[0010] (1) Prepare micelle solutions of triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide;

[0011] (2) Ti3C2T x The nanosheet solution and phytic acid were added to the micelle solution obtained in step (1) and stirred thoroughly to disperse them evenly.

[0012] (3) Add FeCl2·4H2O and CoCl2·6H2O to the solution obtained in step (2) and continue stirring to disperse them evenly;

[0013] (4) Add the 2,6-diaminopyridine dispersion to the solution obtained in step (3) and disperse it evenly;

[0014] (5) Add formaldehyde to the solution obtained in step (4), and after the reaction, wash and dry to obtain a gray product;

[0015] (6) The gray product obtained in step (5) is heat-treated at 500-900°C for 1-3 hours under an inert atmosphere to obtain the metal single-atom doped two-dimensional mesoporous carbon composite material.

[0016] More preferably, in the micelle solution of step (1), the solvent is deionized water, and the mass concentration of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide is 5-30 mg / mL.

[0017] More preferably, in the micelle solution of step (1), the mass concentration of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide is 5 to 15 mg / mL.

[0018] More preferably, in step (1), the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide is dissolved in deionized water and stirred at 40°C for 1 hour to obtain a micelle solution.

[0019] More preferably, in the solution obtained in step (2), Ti3C2T x The mass concentration of the nanosheets is 0.2–1.5 mg / mL.

[0020] More preferably, in the solution obtained in step (2), Ti3C2T x The mass concentration of the nanosheets is 0.5–1.0 mg / mL.

[0021] More preferably, the Ti3C2T in step (2) x The mass concentration of the nanosheet solution was 20 mg / mL.

[0022] More preferably, the total mass concentration of the metal salts (FeCl2·4H2O and CoCl2·6H2O) in the solution obtained in step (3) is 0.1 to 1.0 mg / mL.

[0023] More preferably, the total mass concentration of FeCl2·4H2O and CoCl2·6H2O in the solution obtained in step (3) is 0.15 to 0.65 mg / mL.

[0024] More preferably, in the 2,6-diaminopyridine dispersion in step (4), the solvent is deionized water, and the mass concentration of 2,6-diaminopyridine is 5-15 mg / mL.

[0025] More preferably, 2,6-diaminopyridine is added to deionized water and stirred to disperse it evenly, thus obtaining a 2,6-diaminopyridine dispersion.

[0026] More preferably, in step (5), formaldehyde is added to the solution obtained in step (4), and stirred overnight to allow for complete reaction. Subsequently, the gray precipitate is collected by centrifugation and washed several times with ethanol and deionized water, and then dried to obtain the gray product.

[0027] More preferably, in step (6), the gray product obtained in step (5) is heat-treated at 500-900°C for 2 hours under an inert atmosphere.

[0028] More preferably, in step (6), the gray product obtained in step (5) is heat-treated at 700-800°C for 2 hours under an inert atmosphere.

[0029] More preferably, the total mass of FeCl2·4H2O and CoCl2·6H2O is no more than 15% of the mass of 2,6-diaminopyridine.

[0030] More preferably, the mass ratio of phytic acid to 2,6-diaminopyridine does not exceed 200%.

[0031] More preferably, the mass ratio of formaldehyde to 2,6-diaminopyridine is 50-70%.

[0032] An application of the above-mentioned metal single-atom doped two-dimensional mesoporous carbon composite material, in which the composite material is used to prepare batteries or catalysts.

[0033] The composite material has promising applications in fields such as new energy batteries or electrocatalysts.

[0034] This invention provides a simple interface assembly engineering strategy, using a triblock copolymer of polyethylene oxide-polypropylene oxide-polyethylene oxide (PEO) with the assistance of phytic acid. 20 PPO 70 PEO 20 Using P123 as a mesoporous template, a solution co-assembly strategy was employed to assemble single-atom co-doped mesoporous carbon of metallic Fe and Co onto a two-dimensional Ti3C2T matrix. x On nanosheets. This invention selects hydroxyl-rich phytic acid as a ligand to enhance the assembly forces, successfully assembling mesoporous carbon co-doped with single atoms of metallic Fe and Co onto Ti3C2T. x On nanosheets. During assembly, the addition of metal salts not only serves as a precursor for metal single atoms, but also, driven by electrostatic interactions, the ligands formed by the metal salts and phytic acid can regulate the stacking parameters of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide micelles through hydrogen bonding, thereby enabling the assembly of mesoporous carbon with two pore structures on Ti3C2T nanosheets. x Efficient assembly on nanosheet surfaces. Thanks to its unique porous structure and the synergistic effect of multiple components, the resulting composite material shows promising application prospects in new energy storage and catalysis.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1. This invention uses only commercial triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide as a single structural directing agent, which can simultaneously form both spherical and columnar mesoporous channels, and the synthesis method is simple;

[0037] 2. In the preparation process of this invention, the addition of metal salts can not only serve as precursors for metal single atoms, but also, under the drive of electrostatic forces, the ligands formed by the metal salts and phytic acid can achieve the control of the filling parameters of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide micelles through hydrogen bonding.

[0038] 3. The synthesis method proposed in this invention has a certain degree of universality for different metal salts and can be used to prepare mesoporous carbon composite materials doped with different metal single atoms;

[0039] 4. The method of this invention is simple, the conditions are mild, and the synthesized composite material has good dispersibility;

[0040] 5. This invention employs co-doping with single metal Fe and Co atoms. Compared with single doping, constructing bimetallic single-atom-doped mesoporous carbon can integrate the advantages of different metal single atoms, thereby further improving its application performance.

[0041] 6. In the assembly process of this invention, the addition of metal salts not only serves as a precursor for metal single atoms, but also enables effective control of the P123 micelle filling parameters, thereby achieving both spherical and columnar pore structures of mesoporous carbon in two-dimensional Ti3C2T. x The successful assembly of the nanosheets, along with high-angle annular dark-field scanning transmission electron microscopy, confirmed that single Fe and Co atoms were highly uniformly distributed throughout the composite material structure.

[0042] 7. The composite material prepared by this invention has potential application prospects in the fields of new energy secondary batteries and electrocatalysis due to its unique pore structure and multi-component composition. Attached Figure Description

[0043] Figure 1 This is a TEM image of the composite material obtained in Example 1.

[0044] Figure 2 The image shows a high-angle annular dark-field scanning transmission electron microscope (HAADF-STEM) image of the composite material obtained in Example 1.

[0045] Figure 3 The nitrogen adsorption-desorption isotherm and pore size distribution diagram of the composite material obtained in Example 1 are shown.

[0046] Figure 4 The XRD patterns are those of the products obtained in Example 1 and Comparative Example 1.

[0047] Figure 5 The image shows a TEM image of the composite material obtained in Comparative Example 1. Detailed Implementation

[0048] It should be noted that the exemplary embodiments can be implemented in many forms and should not be construed as limited to the examples set forth herein; rather, these embodiments are provided to make the present invention more comprehensive and complete, and to fully convey the concept of the exemplary embodiments to those skilled in the art.

[0049] It should also be understood that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention are within the scope of protection of the present invention. The specific process parameters, etc., in the following examples are merely examples within a suitable range; that is, those skilled in the art can make appropriate selections within the appropriate range based on the description herein, and are not intended to be limited to the specific values ​​in the examples below.

[0050] The following are specific embodiments of the present invention:

[0051] Example 1

[0052] In this embodiment, a method for preparing a two-dimensional mesoporous carbon composite material doped with a metal single atom includes the following specific steps:

[0053] a. Weigh 300 mg of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide using an electronic balance and add it to 30 mL of deionized water. Stir for 1 h to disperse it evenly.

[0054] b. Use a pipette to measure 1 mL of Ti3C2T solution with a concentration of 20 mg / mL. x The solution and 0.12 mL of phytic acid were added to the solution obtained in step a, and the mixture was stirred for 0.5 h to ensure uniform dispersion.

[0055] c. Weigh 5 mg of FeCl2·4H2O and 5 mg of CoCl2·6H2O using an electronic balance, add them to the solution obtained in b, and continue stirring for 10 min to disperse them evenly.

[0056] d. Weigh 150 mg of 2,6-diaminopyridine using an electronic balance, add it to 20 mL of deionized water, stir for 10 min to disperse it evenly, then add it to the solution obtained in c, and stir for 0.5 h;

[0057] e. Using a pipette, measure 0.3 mL of formaldehyde and add it to the solution obtained in d. Stir overnight to allow the reaction to proceed completely. Subsequently, collect the gray precipitate by centrifugation and wash it several times with ethanol and deionized water. Dry it at 60°C for 12 h to obtain a gray powder.

[0058] f. The product obtained in e is heated to 700°C under N2 atmosphere at a heating rate of 2°C / min and held at that temperature for 2 hours to obtain the Fe and Co single-atom co-doped mesoporous carbon / Ti3C2T prepared in this invention.x Composite materials.

[0059] The obtained samples were characterized in terms of physical properties and morphology, and some results are shown in the attached figures. The results show that mesoporous carbon with both spherical and columnar pore structures is uniformly grown in the two-dimensional Ti3C2T composite material. x The nanosheet surface is uniformly doped with Fe and Co metal single atoms throughout the structure.

[0060] Example 2

[0061] The preparation process and steps in this embodiment are basically the same as those in Example 1, except that:

[0062] In this embodiment, a method for preparing a two-dimensional mesoporous carbon composite material doped with a metal single atom includes the following specific steps:

[0063] a. Weigh 150 mg of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide using an electronic balance and add it to 30 mL of deionized water. Stir for 1 hour to disperse it evenly.

[0064] b. Use a pipette to measure 0.5 mL of Ti3C2T solution with a concentration of 20 mg / mL. x The solution and 0.12 mL of phytic acid were added to the solution obtained in step a, and the mixture was stirred for 0.5 h to ensure uniform dispersion.

[0065] c. Weigh 5 mg of FeCl2·4H2O and 5 mg of CoCl2·6H2O using an electronic balance, add them to the solution obtained in b, and continue stirring for 10 min to disperse them evenly.

[0066] d. Weigh 150 mg of 2,6-diaminopyridine using an electronic balance, add it to 20 mL of deionized water, stir for 10 min to disperse it evenly, then add it to the solution obtained in c, and stir for 0.5 h;

[0067] e. Using a pipette, measure 0.3 mL of formaldehyde and add it to the solution obtained in d. Stir overnight to allow the reaction to proceed completely. Subsequently, collect the gray precipitate by centrifugation and wash it several times with ethanol and deionized water. Dry it at 60°C for 12 h to obtain a gray powder.

[0068] f. The product obtained in e is heated to 700℃ under N2 atmosphere at a heating rate of 2℃ / min and held for 2h to obtain mesoporous carbon / Ti3C2T co-doped with single atoms of Fe and Co. x Composite materials.

[0069] The structure of the resulting composite material is similar to that of Example 1, but due to Ti3C2T x The reduction in the amount of nanosheets resulted in the presence of a small amount of carbon particles in the product.

[0070] Example 3

[0071] The preparation process and steps in this embodiment are basically the same as those in Example 1, except that:

[0072] In this embodiment, a method for preparing a two-dimensional mesoporous carbon composite material doped with a metal single atom includes the following specific steps:

[0073] a. Weigh 300 mg of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide using an electronic balance and add it to 30 mL of deionized water. Stir for 1 h to disperse it evenly.

[0074] b. Use a pipette to measure 1 mL of Ti3C2T solution with a concentration of 20 mg / mL. x The solution and 0.12 mL of phytic acid were added to the solution obtained in step a, and the mixture was stirred for 0.5 h to ensure uniform dispersion.

[0075] c. Weigh 5 mg of FeCl2·4H2O and 5 mg of CoCl2·6H2O using an electronic balance, add them to the solution obtained in b, and continue stirring for 10 min to disperse them evenly.

[0076] d. Weigh 100 mg of 2,6-diaminopyridine using an electronic balance, add it to 20 mL of deionized water, stir for 10 min to disperse it evenly, then add it to the solution obtained in c, and stir for 0.5 h;

[0077] e. Using a pipette, measure 0.3 mL of formaldehyde and add it to the solution obtained in d. Stir overnight to allow the reaction to proceed completely. Subsequently, collect the gray precipitate by centrifugation and wash it several times with ethanol and deionized water. Dry it at 60°C for 12 h to obtain a gray powder.

[0078] f. The product obtained in e is heated to 800℃ under N2 atmosphere at a heating rate of 2℃ / min and held for 2h to obtain mesoporous carbon / Ti3C2T co-doped with single atoms of Fe and Co. x Composite materials.

[0079] The structure of the resulting composite material is similar to that of Example 1, but due to the reduced amount of 2,6-diaminopyridine, the resulting product has mesoporous carbon in Ti3C2T x The thickness on the surface becomes thinner.

[0080] Example 4

[0081] The preparation process and steps in this embodiment are basically the same as those in Example 1, except that:

[0082] In this embodiment, a method for preparing a two-dimensional mesoporous carbon composite material doped with a metal single atom includes the following specific steps:

[0083] a. Weigh 300 mg of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide using an electronic balance and add it to 30 mL of deionized water. Stir for 1 h to disperse it evenly.

[0084] b. Use a pipette to measure 1 mL of Ti3C2T solution with a concentration of 20 mg / mL. x The solution and 0.12 mL of phytic acid were added to the solution obtained in step a, and the mixture was stirred for 0.5 h to ensure uniform dispersion.

[0085] c. Weigh 10 mg of FeCl2·4H2O and 10 mg of CoCl2·6H2O using an electronic balance, add them to the solution obtained in b, and continue stirring for 10 min to disperse them evenly.

[0086] d. Weigh 150 mg of 2,6-diaminopyridine using an electronic balance, add it to 20 mL of deionized water, stir for 10 min to disperse it evenly, then add it to the solution obtained in c, and stir for 0.5 h;

[0087] e. Using a pipette, measure 0.3 mL of formaldehyde and add it to the solution obtained in d. Stir overnight to allow the reaction to proceed completely. Subsequently, collect the gray precipitate by centrifugation and wash it several times with ethanol and deionized water. Dry it at 60°C for 12 h to obtain a gray powder.

[0088] f. The product obtained in e is heated to 800℃ under N2 atmosphere at a heating rate of 2℃ / min and held for 2h to obtain mesoporous carbon / Ti3C2T co-doped with single atoms of Fe and Co. x Composite materials.

[0089] The structure of the resulting composite material is similar to that of Example 1, but due to the increase in the total mass of FeCl2·4H2O and CoCl2·6H2O, a small number of particles appear in the product.

[0090] Example 5

[0091] The preparation process and steps in this embodiment are basically the same as those in Example 1, except that:

[0092] In this embodiment, a method for preparing a two-dimensional mesoporous carbon composite material doped with a metal single atom includes the following specific steps:

[0093] a. Weigh 300 mg of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide using an electronic balance and add it to 30 mL of deionized water. Stir for 1 h to disperse it evenly.

[0094] b. Use a pipette to measure 1 mL of Ti3C2T solution with a concentration of 20 mg / mL. xThe solution was added to the solution obtained in step a, and stirred for 0.5 hours to ensure uniform dispersion.

[0095] c. Weigh 5 mg of FeCl2·4H2O and 5 mg of CoCl2·6H2O using an electronic balance, add them to the solution obtained in b, and continue stirring for 10 min to disperse them evenly.

[0096] d. Weigh 300 mg of 2,6-diaminopyridine using an electronic balance, add it to 20 mL of deionized water, stir for 10 min to disperse it evenly, then add it to the solution obtained in c, and stir for 0.5 h;

[0097] e. Using a pipette, measure 0.3 mL of formaldehyde and add it to the solution obtained in d. Stir overnight to allow the reaction to proceed completely. Subsequently, collect the gray precipitate by centrifugation and wash it several times with ethanol and deionized water. Dry it at 60°C for 12 h to obtain a gray powder.

[0098] f. The product obtained in e is heated to 700℃ under N2 atmosphere at a heating rate of 2℃ / min and held for 2h to obtain Fe and Co single-atom co-doped mesoporous carbon / Ti3C2T. x Composite materials.

[0099] The results were similar to those in Example 1, but because phytic acid was not added, the morphology of the product was very irregular, and some small particles were obviously aggregated in Ti3C2T. x Nanosheet surface.

[0100] Comparative Example 1

[0101] This comparative example illustrates a method for preparing a two-dimensional mesoporous carbon composite material, the specific steps of which are as follows:

[0102] a. Weigh 300 mg of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide using an electronic balance and add it to 30 mL of deionized water. Stir for 1 h to disperse it evenly.

[0103] b. Use a pipette to measure 1 mL of Ti3C2T solution with a concentration of 20 mg / mL. x The solution and 0.12 mL of phytic acid were added to the solution obtained in step a, and the mixture was stirred for 0.5 h to ensure uniform dispersion.

[0104] c. Weigh 150 mg of 2,6-diaminopyridine using an electronic balance, add it to 20 mL of deionized water, stir for 10 min to disperse it evenly, then add it to the solution obtained in b, and stir for 0.5 h.

[0105] d. Using a pipette, measure 0.3 mL of formaldehyde and add it to the solution obtained in c. Stir overnight to allow the reaction to proceed completely. Subsequently, collect the gray precipitate by centrifugation and wash it several times with ethanol and deionized water. Dry it at 60°C for 12 h to obtain a gray powder.

[0106] e. The product obtained in d is heated to 700℃ under N2 atmosphere at a heating rate of 2℃ / min and held at that temperature for 2h to obtain mesoporous carbon / Ti3C2T. x Composite materials.

[0107] The results are attached. Figure 5 As shown, it differs significantly from Example 1, with only a single columnar mesopore arranged on the surface of the mesoporous carbon composite material.

[0108] Comparative Example 2

[0109] The preparation process and steps of this comparative example are basically the same as those of comparative example 1, with the following differences:

[0110] In this comparative example, a method for preparing a two-dimensional carbon composite material doped with a single metal atom is described, and the specific steps are as follows:

[0111] a. Pipette 1 mL of Ti3C2T solution with a concentration of 20 mg / mL. x Add the solution and 0.12 mL of phytic acid to 30 mL of deionized water and stir for 0.5 h to disperse it evenly.

[0112] b. Weigh 5 mg of FeCl2·4H2O and 5 mg of CoCl2·6H2O using an electronic balance, add them to the solution obtained in a, and continue stirring for 10 min to disperse them evenly;

[0113] c. Weigh 150 mg of 2,6-diaminopyridine using an electronic balance, add it to 20 mL of deionized water, stir for 10 min to disperse it evenly, then add it to the solution obtained in b, and stir for 0.5 h.

[0114] d. Using a pipette, measure 0.3 mL of formaldehyde and add it to the solution obtained in c. Stir overnight to allow the reaction to proceed completely. Subsequently, collect the gray precipitate by centrifugation and wash it several times with ethanol and deionized water. Dry it at 60°C for 12 h to obtain a gray powder.

[0115] e. The product obtained in d is heated to 700℃ under N2 atmosphere at a heating rate of 2℃ / min and held for 2h to obtain Fe and Co single-atom co-doped carbon / Ti3C2T x Composite materials.

[0116] The results obtained were significantly different from those of Example 1, and no obvious mesoporous structure was found in the composite material.

[0117] Experimental test analysis:

[0118] See attached diagram. Figure 1 This is a TEM image of the metal single-atom-doped two-dimensional mesoporous carbon composite material obtained in Example 1 of this invention. TEM analysis: The morphology and structure of the material were observed using a JEOL-200CX transmission electron microscope (TEM). The TEM images show that the obtained material exhibits a distinct two-dimensional lamellar structure, and both columnar and spherical mesoporous carbon particles are present in Ti3C2T. x Nanosheet surface.

[0119] See attached diagram. Figure 2 This is a HAADF-STEM image of the metal single-atom-doped two-dimensional mesoporous carbon composite material obtained in Example 1 of this invention. HAADF-STEM analysis: High-angle annular dark-field testing was performed using a JEM-ARM300F transmission electron microscope. The HAADF-STEM image shows that the white bright spots within the circles are uniformly dispersed throughout the material framework. Based on the elemental composition of the material, these white bright spots are attributed to Fe and Co atoms. Therefore, it can be concluded that Fe and Co have been successfully doped into the entire material structure in atomic form.

[0120] See attached diagram. Figure 3 The nitrogen adsorption-desorption isotherm and pore size distribution of the composite material obtained in Example 1 of this invention are shown. BET analysis: Specific surface area and pore structure were analyzed using a Micromeritics ASAP 2460. The BET test showed that the BET specific surface area of ​​the composite material obtained in Example 1 was 188.5 m². 2 / g, and the pore distribution diagram shows that the average pore size of the composite material obtained in Example 1 is 4.0 nm, proving the formation of a mesoporous structure.

[0121] See attached diagram. Figure 4 The XRD patterns of the products obtained in Example 1 and Comparative Example 1 of this invention are shown. XRD analysis: A RigaKu D / max-2550 X-ray powder diffractometer was used. The XRD patterns clearly show that the diffraction peaks of Example 1 and Comparative Example 1 are similar, with only one obvious broad peak at 25°, belonging to the (002) crystal plane of amorphous carbon. Furthermore, no obvious Fe or Co characteristic peaks were detected in the composite material obtained in Example 1, indicating the absence of elemental Fe or Co particles.

[0122] See attached diagram. Figure 5 The image shows a TEM image of the mesoporous carbon composite material obtained in Comparative Example 1. It can be seen that the obtained material exhibits a distinct two-dimensional lamellar structure, but only columnar mesopores grow on Ti3C2T. x Nanosheet surface. This further illustrates the important role of metal salts in pore structure regulation in this invention.

[0123] In summary, this invention successfully assembled mesoporous carbon with two pore structures, co-doped with single atoms of Fe and Co, onto two-dimensional Ti3C2T using a solution co-assembly strategy. x Nanosheet surface. During assembly, the addition of metal salts not only serves as a precursor for metal single atoms, but also, driven by hydrogen bonding, the chelates formed by the metal salts and phytic acid can regulate the packing parameters of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide micelles, thereby enabling both spherical and columnar pore structures of mesoporous carbon in Ti3C2T. x Uniform loading of nanosheets.

[0124] The embodiments of the present invention have been described above with reference to the accompanying drawings. However, the present invention is not limited to the above embodiments. Various changes can be made according to the purpose of the invention. Any changes, modifications, substitutions, combinations or simplifications made based on the spirit and principle of the technical solution of the present invention shall be equivalent substitutions. As long as they meet the purpose of the invention and do not deviate from the technical principle and inventive concept of the present invention, they shall fall within the protection scope of the present invention.

Claims

1. A two-dimensional mesoporous carbon composite material doped with a single metal atom, characterized in that, The composite material has a two-dimensional sheet-like structure, with mesoporous carbon with columnar and spherical pore structures growing on two-dimensional Ti3C2T. x The nanosheets are uniformly doped with Fe and Co metal single atoms in the material structure. The preparation method of the metal single-atom doped two-dimensional mesoporous carbon composite material includes the following steps: (1) Preparation of micelle solutions of triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide; (2) Ti3C2T x The nanosheet solution and phytic acid were added to the micelle solution obtained in step (1) and stirred thoroughly to disperse them evenly. (3) Add FeCl2·4H2O and CoCl2·6H2O to the solution obtained in step (2) and continue stirring to disperse them evenly; (4) Add the 2,6-diaminopyridine dispersion to the solution obtained in step (3) and disperse evenly; (5) Add formaldehyde to the solution obtained in step (4), and after the reaction, wash and dry to obtain a gray product; (6) The gray product obtained in step (5) is heat-treated at 500-900 °C for 1-3 h in an inert atmosphere to obtain the metal single-atom doped two-dimensional mesoporous carbon composite material.

2. The two-dimensional mesoporous carbon composite material doped with a single metal atom according to claim 1, characterized in that, The composite material has a BET specific surface area of ​​150~200 m² / g and an average pore size of 3~5 nm.

3. A method for preparing a two-dimensional mesoporous carbon composite material doped with a single metal atom as described in claim 1 or 2, characterized in that, With the assistance of phytic acid, and using the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide as a mesoporous template, mesoporous carbon co-doped with single atoms of Fe and Co was assembled onto two-dimensional Ti3C2T using a solution co-assembly strategy. x Two-dimensional mesoporous carbon composite material doped with the aforementioned metal single atom was prepared on nanosheets.

4. The method for preparing the metal single-atom doped two-dimensional mesoporous carbon composite material according to claim 3, characterized in that, In step (1), the micelle solution is prepared by deionized water as the solvent, and the mass concentration of the triblock copolymer polyethylene oxide-polypropylene oxide-polyethylene oxide is 5-30 mg / mL.

5. The method for preparing the metal single-atom doped two-dimensional mesoporous carbon composite material according to claim 3, characterized in that, In the solution obtained in step (2), Ti3C2T x The mass concentration of the nanosheets is 0.2~1.5 mg / mL.

6. The method for preparing the metal single-atom doped two-dimensional mesoporous carbon composite material according to claim 3, characterized in that, The total mass concentration of the metal salt in the solution obtained in step (3) is 0.1~1.0 mg / mL.

7. The method for preparing the metal single-atom doped two-dimensional mesoporous carbon composite material according to claim 3, characterized in that, In step (4), the solvent for the 2,6-diaminopyridine dispersion is deionized water, and the mass concentration of 2,6-diaminopyridine is 5~15 mg / mL.

8. The method for preparing the metal single-atom doped two-dimensional mesoporous carbon composite material according to claim 3, characterized in that, The total mass ratio of FeCl2·4H2O and CoCl2·6H2O to the mass ratio of 2,6-diaminopyridine does not exceed 15%; The mass ratio of phytic acid to 2,6-diaminopyridine shall not exceed 200%. The mass ratio of formaldehyde to 2,6-diaminopyridine is 50-70%.

9. The application of a metal single-atom doped two-dimensional mesoporous carbon composite material as described in claim 1 or 2, characterized in that, The composite material is used to prepare batteries or catalysts.

Citation Information

Patent Citations

  • Mesoporous carbon nanomaterial as well as preparation method and application thereof

    CN115703634A