A sodium-based titanium phosphorus compound negative electrode without hydrogen evolution in a water-based battery and a preparation method thereof

By preparing NaTi2+x(PO4)3(PO3.5)2x carbon composite materials and controlling the sodium insertion/extraction potential of the materials to avoid hydrogen evolution reaction, the problem of hydrogen evolution side reaction in aqueous sodium-ion batteries was solved, and the safety and cycle stability of the batteries were improved.

CN117954600BActive Publication Date: 2026-11-10BENAN ENERGY TECH JIANGSU CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410084233.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2026-11-10
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

In aqueous sodium-ion batteries, traditional NaTi2(PO4)3 materials are prone to hydrogen evolution side reactions in high pH environments, leading to decreased battery performance and material corrosion. Existing technologies struggle to maintain excellent cycle stability while avoiding hydrogen evolution.

Method used

The NaTi2+x(PO4)3(PO3.5)2x carbon composite material is used. By introducing P2O74- with stronger electronegativity, the sodium insertion/extraction potential of the material is controlled, so that the charge/discharge platform is above the hydrogen evolution potential, thus avoiding the hydrogen evolution reaction. The preparation process of the material includes steps such as mixing, sintering and pulverizing.

Benefits of technology

This method achieves hydrogen evolution-free operation in aqueous batteries, enhancing battery safety and electrochemical performance. The material exhibits excellent cycle stability, and the preparation method is simple and highly operable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117954600B_ABST
    Figure CN117954600B_ABST
Patent Text Reader

Abstract

The application discloses a sodium-based titanium phosphorus compound negative electrode without hydrogen evolution in a water-based battery and a preparation method thereof. 2+x (PO4)3(PO 3.5 ) 2x Carbon composite material, wherein x is 0.01-1; the preparation method is as follows: Na source material, Ti source material, P source material and carbon source material are uniformly mixed, precursor powder is prepared after drying, the precursor powder is sintered in a sintering kiln in an inert or reducing atmosphere, and the NaTi 2+x (PO4)3(PO 3.5 ) 2x Carbon composite material. The sodium-based titanium phosphorus compound negative electrode without hydrogen evolution in the water-based battery and the preparation method thereof introduce P2O7 4‑ with stronger electronegativity, control the sodium extraction potential of the material, ensure that the charging and discharging platform of the material is above the hydrogen evolution potential, avoid the occurrence of the hydrogen evolution reaction side reaction, and make the material have excellent cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a hydrogen-free sodium-based titanium-phosphorus compound anode for aqueous batteries and its preparation method. Background Technology

[0002] In addressing challenges such as the global fossil fuel crisis, sodium-ion batteries possess enormous application potential due to their abundant resources and excellent electrochemical performance, and are currently being commercialized globally. As a key component of sodium-ion batteries, electrode materials directly affect battery performance. Therefore, the development of a safe, hydrogen-evolution-free aqueous sodium-ion battery anode material holds considerable promise.

[0003] In aqueous sodium-ion batteries, the occurrence of hydrogen evolution side reactions at the negative electrode is difficult to avoid due to the aqueous electrolyte. On the one hand, the hydrogen evolution potential of the electrolyte is closely related to the electrolyte pH; the higher the pH, the lower the hydrogen evolution potential. On the other hand, a high pH environment (strong alkalinity) is detrimental to the cycle stability of the material. For traditional NaTi2(PO4)3 material, its potential relative to metallic sodium is 2.1V, compared to a standard hydrogen potential of -0.62V. For aqueous solutions, the hydrogen evolution potential only falls below -0.62V when the solution pH is ≥11. Furthermore, considering polarization caused by materials and electrodes, the charge / discharge plateau of NaTi2(PO4)3 material in aqueous batteries will appear below the hydrogen evolution potential, leading to severe hydrogen evolution side reactions. Simultaneously, NaTi2(PO4)3 material exhibits corrosion in strongly alkaline solutions (http: / / dx.doi.org / 10.1016 / j.elecom.2014.04.003), affecting battery performance. In polyanionic material systems, it is feasible to control the insertion / extraction potential of materials by adjusting the type of polyanion (electronegativity of polyanion) (Adv. Funct. Mater. 2020, 2000473). Therefore, preparing a battery anode material with a safe potential and no hydrogen evolution by adjusting the type of polyanion has great advantages for use in aqueous batteries. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a hydrogen-evolution-free sodium-based titanium-phosphorus compound anode for aqueous batteries and its preparation method. The chemical formula of the hydrogen-evolution-free sodium-based titanium-phosphorus compound anode can be represented as: NaTi 2+x (PO4)3(PO 3.5 ) 2x By introducing P2O7, which has a stronger electronegativity 4- By controlling the sodium insertion / extraction potential of the material, the charge / discharge plateau of the material is kept above the hydrogen evolution potential, thus avoiding the occurrence of hydrogen evolution reaction side reactions and enabling the material to have excellent cycle stability.

[0005] The technical solution to achieve the above objective is: a hydrogen-free sodium-based titanium-phosphorus compound anode for aqueous batteries and its preparation method, wherein the chemical formula of the hydrogen-free sodium-based titanium-phosphorus compound anode is represented as NaTi. 2+x (PO4)3(PO 3.5 ) 2x Carbon composite material, where x is 0.01-1; this NaTi 2+x (PO4)3(PO 3.5 ) 2x The preparation method of carbon composite materials is as follows:

[0006] Na, Ti, P, and carbon source materials are mixed uniformly and dried to obtain precursor powder. The precursor powder is then sintered in an inert or reducing atmosphere kiln, cooled, and pulverized to obtain NaTi. 2+x (PO4)3(PO 3.5 ) 2x Carbon composite materials;

[0007] The molar ratio of Na:Ti:P in the Na source material, Ti source material and P source material is 1:(2+x):(3+2x), where x is 0.01-1;

[0008] NaTi 2+x (PO4)3(PO 3.5 ) 2x The mass ratio of carbon source material to carbon source material is (0.7-0.99):(0.01-0.3).

[0009] The above-mentioned aqueous battery non-hydrogen-evolving sodium-based titanium-phosphorus compound anode and its preparation method, wherein the Na source material is one or more of Na2CO3, NaOH, Na2SO4 and NaH2PO4;

[0010] The Ti source material is one or more of TiO2, tetrabutyl titanate and titanium tetrachloride;

[0011] The P source material is one or more of H3PO4, NH4H2PO4, (NH4)2HPO4 and P2O5.

[0012] The above-mentioned aqueous battery non-hydrogen evolution sodium-based titanium-phosphorus compound anode and its preparation method, wherein the Na source material, Ti source material, P source material and carbon source material are mixed uniformly by one or more of dry ball milling, wet ball milling and high-speed dispersion mixing.

[0013] The above-mentioned aqueous battery non-hydrogen evolution sodium-based titanium phosphorus compound anode and its preparation method, wherein the drying method of the precursor powder obtained after drying is one or more of fluidized bed drying, spray drying and disc drying.

[0014] The above-mentioned aqueous battery non-hydrogen-evolving sodium-based titanium-phosphorus compound anode and its preparation method, wherein the atmosphere of the sintering furnace is nitrogen, argon, or a hydrogen-argon mixture.

[0015] The above-mentioned aqueous battery non-hydrogen-evolving sodium-based titanium-phosphorus compound anode and its preparation method, wherein the sintering temperature of the sintering furnace is 600-1000℃, the heating rate is 1-10℃ / min, and the holding time is 4-24h.

[0016] The above-mentioned aqueous battery non-hydrogen-evolving sodium-based titanium-phosphorus compound anode and its preparation method, wherein the cooling method after sintering is one or more of active cooling and / or natural cooling.

[0017] The above-mentioned hydrogen-free sodium-based titanium-phosphorus compound anode in an aqueous battery and its preparation method, wherein the pulverization method after cooling is one or more of mechanical pulverization, air jet milling, and disc milling.

[0018] The present invention relates to a hydrogen-free sodium-based titanium-phosphorus compound negative electrode in an aqueous battery and its preparation method, which can avoid the hydrogen evolution reaction of the negative electrode in aqueous sodium-ion batteries and enhance battery safety performance; there is no hydrogen evolution side reaction, resulting in excellent battery electrochemical performance; the preparation method is simple and highly operable for mass production. Attached Figure Description

[0019] Figure 1 SEM image of the hydrogen-free sodium-based titanium phosphate compound negative electrode of the embodiment;

[0020] Figure 2 The XRD pattern of the hydrogen-free sodium-based titanium phosphate compound negative electrode is shown in the example.

[0021] Figure 3 The 0.1C charge-discharge curve of the hydrogen-free sodium-based titanium phosphate compound negative electrode is shown in the example.

[0022] Figure 4 The cycling performance diagram of the hydrogen-free sodium-based titanium phosphate compound negative electrode is shown in the example.

[0023] Figure 5 The LSV curves of the materials in the examples and comparative examples are shown. Detailed Implementation

[0024] To enable those skilled in the art to better understand the technical solution of the present invention, its specific embodiments are described in detail below with reference to the accompanying drawings:

[0025] Example

[0026] Please see Figure 1 and Figure 2A sodium-based titanium-phosphorus compound negative electrode for an aqueous battery that does not produce hydrogen evolution, with the chemical formula NaTi3(PO4)3(PO4)2. 3.5 2. Carbon composite material, prepared using the following method:

[0027] NaOH was used as the Na source, TiO2 as the Ti source, H3PO4 as the P source, and acetylene black as the carbon source; according to the molar ratio Na:Ti:P = 1:3:5, NaTi3(PO4)3(PO 3.5 The mass ratio of Na source material to carbon source material was 0.97:0.03. With a solid content of 50%, the Na, Ti, P, and carbon source materials were ball-milled for 6 hours using a horizontal sand mill to achieve uniform mixing. The resulting slurry was then processed into precursor powder using a co-flow spray dryer. The precursor powder was placed in a sintering kiln and heated to 750℃ at a rate of 2℃ / min under a nitrogen atmosphere, and held for 8 hours. After natural cooling, it was pulverized by airflow to obtain NaTi3(PO4)3(PO4)2. 3.5 )2 Carbon composite materials. Figure 1 and Figure 2 To prepare the material morphology.

[0028] Please see Figure 3 and Figure 4 The NaTi3(PO4)3(PO4)3 obtained in Example 1 was used. 3.5 A carbon composite material was used as the working electrode, an activated carbon sheet as the counter electrode, and a 1.2M Na₂SO₄ solution was used as the electrolyte. An Ag / AgCl / saturated KCl electrode was used as the reference electrode. The charge-discharge curve at 0.1C is shown below. Figure 3 As shown, in the charge / discharge voltage range of -0.35 to -0.85V, NaTi3(PO4)3(PO 3.5 The specific capacity of the carbon composite material is greater than 110 mAh / g. Cycling performance is as follows: Figure 4 As shown, the 0.2C cycle capacity test, NaTi3(PO4)3(PO 3.5 )2 Carbon composites have excellent cycle stability.

[0029] Comparative example:

[0030] NaOH was used as the Na source, TiO2 as the Ti source, H3PO4 as the P source, and acetylene black as the carbon source. The molar ratio of Na:Ti:P was 1:2:3, and the mass ratio of NaTi2(PO4)3 to C was 0.97:0.03. The Na source material, Ti source material, P source material and carbon source material were mixed evenly by ball milling in a horizontal sand mill for 6 hours with a solid content of 50%. The slurry was then processed into precursor powder by a co-flow spray drying device. The precursor powder was placed in a sintering kiln and heated to 750℃ at a heating rate of 2℃ / min under a nitrogen atmosphere and held for 8 hours. After natural cooling, the carbon composite material NaTi2(PO4)3 was obtained by air jet pulverization.

[0031] Please see Figure 5 The materials obtained in the examples and comparative examples were used as working electrodes, activated carbon sheets as counter electrodes, and 1.2M Na2SO4 solution as the electrolyte. An Ag / AgCl / saturated KCl electrode was used as the reference electrode. The reduction potentials of the materials in the examples and comparative examples were tested by linear sweep voltammetry (LSV). Figure 5 As can be seen in the example, NaTi3(PO4)3(PO 3.5 The reduction potential of the carbon composite material is between -0.6 and -0.7 V, while that of the comparative carbon composite material NaTi2(PO4) is much lower. 3的 The reduction potential is between -0.8 and -0.9 V. Therefore, the comparative material will be accompanied by a strong hydrogen evolution reaction of the electrolyte during the charging and discharging process. However, the reduction potential of the embodiment is shifted to the positive direction by 0.2 V, which greatly slows down the hydrogen evolution reaction of the electrolyte.

[0032] The aqueous battery of this invention uses a sodium-based titanium-phosphorus compound anode without hydrogen evolution. During preparation, the Na source can be one or more Na-containing compounds such as Na₂CO₃, NaOH, Na₂SO₄, and NaH₂PO₄; the Ti source can be one or more Ti-containing compounds such as TiO₂, tetrabutyl titanate, and titanium tetrachloride; the P source can be one or more P-containing phosphorus compounds such as H₃PO₄, NH₄H₂PO₄, (NH₄)₂HPO₄, and P₂O₅; the molar ratio of Na:Ti:P is 1:(2+x):(3+2x), where x is 0.01-10; NaTi 2+x (PO4)3(PO 3.5 ) 2xThe mass ratio of Na source material to carbon source material is (0.7-0.99):(0.01-0.3); the mixing method of Na source material, Ti source material, P source material and carbon source material is one or more common mixing methods such as dry ball milling, wet ball milling, high-speed dispersion mixing; the drying method is one or more conventional drying methods such as fluidized bed drying, spray drying, disc drying; the sintering kiln atmosphere is one of inert gases such as nitrogen, argon, hydrogen-argon mixture or reducing atmosphere; the kiln sintering temperature is 600-1000℃, the heating rate is 1-10℃ / min; the holding time is 4-24h; the cooling method is one or more of active cooling and natural cooling; the pulverization method is one or more of conventional pulverization methods such as mechanical pulverization, air jet mill pulverization and disc pulverization.

[0033] In summary, the aqueous battery of the present invention, which contains a hydrogen-evolving sodium-based titanium-phosphorus compound anode and its preparation method, achieves this by introducing P2O7, which has stronger electronegativity. 4- By controlling the sodium insertion / extraction potential of the material, the charge / discharge plateau of the material is kept above the hydrogen evolution potential, thus avoiding the occurrence of hydrogen evolution reaction side reactions and enabling the material to have excellent cycle stability.

[0034] Those skilled in the art should recognize that the above embodiments are merely illustrative of the present invention and are not intended to limit the present invention. Any variations or modifications to the above embodiments that are within the spirit and essence of the present invention will fall within the scope of the claims of the present invention.

Claims

1. A sodium-based titanium-phosphorus compound negative electrode for an aqueous battery that does not involve hydrogen evolution, characterized in that, The chemical formula of the non-hydrogen evolution sodium-based titanium phosphate compound negative electrode is represented as NaTi. 2+x (PO4)3(PO 3.5 ) 2x Carbon composite material, where x is 1; this NaTi 2+x (PO4)3(PO 3.5 ) 2x The preparation method of carbon composite materials is as follows: Na, Ti, P, and carbon source materials are mixed uniformly and dried to obtain precursor powder. The precursor powder is then sintered in an inert or reducing atmosphere kiln, cooled, and pulverized to obtain NaTi. 2+x (PO4)3(PO 3.5 ) 2x Carbon composite materials; The molar ratio of Na:Ti:P in the Na source material, Ti source material and P source material is 1:(2+x):(3+2x), where x is 1; NaTi 2+x (PO4)3(PO 3.5 ) 2x The mass ratio of carbon source material to carbon source material is (0.7-0.99):(0.01-0.3).

2. The aqueous battery anode without hydrogen evolution sodium-based titanium-phosphorus compound as described in claim 1, characterized in that, The Na source material is one or more of Na2CO3, NaOH, Na2SO4 and NaH2PO4; The Ti source material is one or more of TiO2, tetrabutyl titanate and titanium tetrachloride; The P source material is one or more of H3PO4, NH4H2PO4, (NH4)2HPO4 and P2O5.

3. The aqueous battery anode without hydrogen evolution sodium-based titanium-phosphorus compound as described in claim 1, characterized in that, The Na source material, Ti source material, P source material and carbon source material are mixed uniformly by one or more of the following methods: dry ball milling, wet ball milling and high-speed dispersion mixing.

4. The aqueous battery anode without hydrogen evolution sodium-based titanium-phosphorus compound as described in claim 1, characterized in that, The drying method used to obtain the precursor powder after drying is one or more of fluidized bed drying, spray drying, and disc drying.

5. The aqueous battery anode without hydrogen evolution sodium-based titanium-phosphorus compound as described in claim 1, characterized in that, The atmosphere of the sintering kiln is nitrogen, argon, or a mixture of hydrogen and argon.

6. The aqueous battery anode without hydrogen evolution sodium-based titanium-phosphorus compound as described in claim 1, characterized in that, The sintering temperature of the sintering kiln is 600-1000℃, the heating rate is 1-10℃ / min, and the holding time is 4-24h.

7. The aqueous battery anode without hydrogen evolution sodium-based titanium-phosphorus compound as described in claim 1, characterized in that, The cooling method after sintering is active cooling and / or natural cooling.

8. The aqueous battery anode without hydrogen evolution sodium-based titanium-phosphorus compound as described in claim 1, characterized in that, The pulverization method after cooling is air jet milling and / or disc milling.

Citation Information

Patent Citations

  • Carbon-coated titanium sodium phosphate composite material and prepared sodium ion battery

    CN110311098A

  • Preparation method of high-voltage sodium ion battery positive electrode material carbon composite cobalt-based mixed sodium phosphate salt

    CN115893366A