A method for improving the bonding between metal particles and plastic substrates

Through the combination of modified silica-coated metal particles and hyperbranched polyurethane, the compatibility and dispersion problems of metal particles such as copper powder and polycarbonate plastic substrates are solved, and the mechanical properties and metallic look and feel of the plastic are improved.

CN117986832BActive Publication Date: 2024-10-22FUJIAN HUASU NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410148660.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-02
Publication Date
2024-10-22
Estimated Expiration
2044-02-02

AI Technical Summary

Technical Problem

Metal powder particles such as copper have poor compatibility and dispersion with plastic substrates such as polycarbonate, which affects the mechanical properties and usability of plastics.

Method used

Modified silica-coated metal particles and hyperbranched polyurethane are used to form modified silica-coated metal particles through ultrasonic vibration and melt mixing technology, and hyperbranched polyurethane is used as a compatibilizer to improve the relationship between the metal particles and the plastic matrix. The combination and dispersion of materials.

Benefits of technology

It improves the bonding between metal particles such as copper powder and the polycarbonate plastic substrate, enhances the mechanical properties of the plastic, and gives the plastic a metallic look and feel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004694849190000021
    Figure BDA0004694849190000021
  • Figure BDA0004694849190000071
    Figure BDA0004694849190000071
Patent Text Reader

Abstract

The present invention relates to the field of plastic technology, and discloses a method for improving the binding property of metal particles to plastic substrates. Hyperbranched polyurethane has good compatibility with plastic substrates such as polycarbonate, can improve the processing performance rheology of plastic substrates such as polycarbonate, has unique dendritic molecular chains, forms an interpenetrating cross-linked network with plastic substrates such as polycarbonate, and greatly improves the mechanical properties such as impact strength and tensile strength of plastic substrates such as polycarbonate. Hyperbranched polyurethane acts as a compatibilizer to improve the dispersibility of modified silica-coated metal particles in polycarbonate plastic substrates, so that metal particles such as copper powder will not affect the mechanical properties of polycarbonate. The modified silica-coated metal particles are uniformly dispersed in the matrix of plastic substrates such as polycarbonate, giving plastic substrates such as polycarbonate a good metallic appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastics, in particular to a method for improving the bonding between metal particles and plastic substrates. Background Art

[0002] Plastics are three major polymer materials, such as polycarbonate, polypropylene, ABS acrylonitrile-butadiene-styrene polymer, polystyrene, etc., which have good mechanical properties, processing properties and chemical stability, and have important applications in various fields of industrial production. Blending metal powder particles such as copper, iron, nickel and other metals with plastic substrates such as polycarbonate can give plastics a high-gloss and colorful metallic texture and beauty. Metal spray-free plastics have the advantages of being safer and more environmentally friendly, lower cost, and easy to recycle and reuse, and have public application prospects in the plastic processing industry. However, the compatibility of metal powder particles such as copper and plastic substrates such as polycarbonate is poor, and the dispersibility is not good. Directly processing and molding with plastics such as polycarbonate will seriously affect the mechanical properties and use performance of plastics. The present invention aims to use modified silica-coated metal particles and hyperbranched polyurethane polymers to improve the binding of metal particles such as copper powder and plastic substrates such as polycarbonate, and give plastics such as polycarbonate a metallic look and feel. Summary of the invention

[0003] Technical problem solved: Provides a modified silica-coated metal particle and hyperbranched polyurethane, which improves the binding property of metal particles such as copper powder and plastic substrates such as polycarbonate, while improving the mechanical properties of plastics such as polycarbonate and giving the plastic a metallic look.

[0004] Technical solution:

[0005] A method for improving the bonding between metal particles and plastic substrates comprises the following steps:

[0006] S1. Add metal particles into ethanol, disperse them by ultrasonic vibration, then drop ethanol solution containing tetraethyl orthosilicate and ammonia water, react at 40-45°C for 10-20h, then drop aqueous solution containing KH560, continue to react for 3-5h, filter, wash with ethanol, and dry to obtain modified silica-coated metal particles.

[0007] S2. Mixing and melt-mixing plastic, modified silica-coated metal particles, hyperbranched polyurethane, and antioxidant to improve the bonding between the metal particles and the plastic substrate.

[0008] Furthermore, the mass of tetraethyl orthosilicate and KH560 in S1 is 80-150% and 2-6% of the mass of the metal particles.

[0009] Furthermore, the melt mixing method in S1 includes: adding plastic, modified silica-coated metal particles, and hyperbranched polyurethane into a high-speed mixer for mixing at a temperature of 50-70°C for 20-60 minutes; then placing them in a twin-screw extruder for melt blending, with the temperature of sections 1 to 6 being 170-260°C; and cooling and discharging.

[0010] Furthermore, the mass of the modified silica-coated metal particles and the hyperbranched polyurethane is 0.5-5% and 1-8% of the mass of the plastic.

[0011] Furthermore, the metal particles have a particle size of 5-150 um, including silver powder, copper powder, nickel powder, and iron powder.

[0012] Further, the plastic includes polycarbonate, ABS, and polypropylene.

[0013] Further, the preparation method of the hyperbranched polyurethane is:

[0014] (1) Add D,L-serine and terephthalaldehyde to a sodium hydroxide aqueous solution, react at 35-50°C for 4-8h, then add sodium borohydride at 20-30°C, react for 12-24h, add petroleum ether for extraction, collect the aqueous phase after separation, add hydrochloric acid solution to adjust the pH to 4-5 until a precipitate is precipitated, filter, and wash with water to obtain a polymerized monomer. Reaction route:

[0015]

[0016] (2) After the polymerization monomer and p-toluenesulfonic acid are mixed, a melt polycondensation reaction is carried out, and after cooling, the product is washed with methanol and dried to obtain a hyperbranched polyurethane.

[0017] Furthermore, the mass of D,L-serine in (1) is 135-150% of the mass of terephthalaldehyde.

[0018] Furthermore, the mass of p-toluenesulfonic acid in (2) is 0.7-0.9% of the mass of the polymerized monomers.

[0019] Furthermore, the melt polycondensation reaction in (2) is carried out at a temperature of 180-210° C. for 3-7 hours.

[0020] Technical effects:

[0021] The present invention utilizes D,L-serine and terephthalaldehyde to carry out Schiff base reaction, and then reduces with sodium borohydride to obtain a polymer monomer containing two carboxyl groups, two hydroxyl groups and an imino group. Under the catalysis of p-toluenesulfonic acid, the carboxyl groups and the hydroxyl groups undergo esterification cross-linking reaction to obtain a novel hyperbranched polyurethane containing an imino group. The hyperbranched polyurethane has good compatibility with plastic substrates such as polycarbonate, can improve the processing performance rheology of plastic substrates such as polycarbonate, has a unique dendritic molecular chain, forms an interpenetrating cross-linking network with plastic substrates such as polycarbonate, and greatly improves the mechanical properties such as impact strength and tensile strength of plastic substrates such as polycarbonate.

[0022] The present invention uses tetraethyl orthosilicate as a silicon source to form a transparent silicon dioxide coating layer on the surface of metal particles such as silver powder, copper powder, nickel powder, iron powder, etc., and then undergoes KH550 modification to obtain modified silicon dioxide coated metal particles. The epoxy group of KH560 on the silicon dioxide surface can react with the imino group in the hyperbranched polyurethane molecular chain, so that the hyperbranched polyurethane is used as a compatibilizer to improve the compatibility of the modified silicon dioxide coated metal particles in a polycarbonate plastic substrate, and the dispersibility is better, so that the metal particles such as silver powder, copper powder, nickel powder, iron powder, etc. will not affect the mechanical properties of polycarbonate. The modified silicon dioxide coated metal particles are uniformly dispersed in a plastic substrate matrix such as polycarbonate, giving the plastic substrate such as polycarbonate a good metal appearance. DETAILED DESCRIPTION

[0023] The present invention is not limited to the following specific embodiments. A person skilled in the art can implement the present invention in various other specific embodiments according to the contents disclosed in the present invention, or any simple changes or modifications made to the design structure and ideas of the present invention fall within the protection scope of the present invention. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0024] The copper powder used in the present invention has an average particle size of 5 μm.

[0025] Nickel powder, average particle size 15um.

[0026] Silver powder, average flake diameter 20um, average thickness 0.1um.

[0027] Example 1

[0028] (1) Add 5.4 g of D,L-serine and 4 g of terephthalaldehyde to 20 mL of 5% sodium hydroxide aqueous solution, react at 50°C for 6 h, then add 0.9 g of sodium borohydride at 20°C, react for 18 h, add petroleum ether for extraction, collect the aqueous phase after separation, add hydrochloric acid solution to adjust the pH to 4 until a precipitate is precipitated, filter, and wash with water to obtain a polymerized monomer. The structural formula is

[0029] (2) After 5 g of the polymerization monomer and 0.35 g of p-toluenesulfonic acid were mixed, a melt polycondensation reaction was carried out at a temperature of 180° C. for 7 h. After cooling, the product was washed with methanol and dried to obtain a hyperbranched polyurethane.

[0030] (3) 20 g of copper powder was added to 100 mL of ethanol and dispersed by ultrasonic vibration. Then, an ethanol solution containing 16 g of tetraethyl orthosilicate was added dropwise, and 3 mL of ammonia water was added. The mixture was reacted at 45 ° C for 10 h. Then, an aqueous solution containing 0.4 g of KH560 was added dropwise, and the reaction was continued for 3 h. The mixture was filtered, washed with ethanol, and dried to obtain modified silica-coated copper powder.

[0031] (4) 100 g of polycarbonate, 0.5 g of modified silica-coated copper powder, 1 g of hyperbranched polyurethane, and 0.6 g of antioxidant 168 were added to a high-speed mixer and mixed at a temperature of 50° C. for 20 min; then placed in a twin-screw extruder for melt mixing, and the temperatures of sections 1 to 6 were 200° C., 220° C., 250° C., 250° C., 260° C., and 240° C.; the material was cooled and discharged to obtain a polycarbonate composite material, thereby improving the bonding between the copper powder and the polycarbonate plastic substrate.

[0032] Example 2

[0033] (1) Add 5.8 g of D,L-serine and 4 g of terephthalaldehyde to 30 mL of 3% sodium hydroxide aqueous solution, react at 35° C. for 8 h, then add 0.9 g of sodium borohydride at 20° C., react for 24 h, add petroleum ether for extraction, collect the aqueous phase after separation, add hydrochloric acid solution dropwise to adjust the pH to 4, until a precipitate is precipitated, filter, and wash with water to obtain a polymerized monomer.

[0034] (2) 5 g of the polymerization monomer and 0.45 g of p-toluenesulfonic acid were mixed and subjected to melt polycondensation reaction at 210° C. for 3 h. After cooling, the product was washed with methanol and dried to obtain a hyperbranched polyurethane.

[0035] (3) 20 g of nickel powder was added to 150 mL of ethanol, and dispersed by ultrasonic vibration. Then, an ethanol solution containing 22 g of tetraethyl orthosilicate was added dropwise, and 4 mL of ammonia water was added. The mixture was reacted at 45 ° C for 10 h. Then, an aqueous solution containing 0.8 g of KH560 was added dropwise, and the reaction was continued for 5 h. The mixture was filtered, washed with ethanol, and dried to obtain modified silica-coated nickel powder.

[0036] (4) Add 100 g of polycarbonate, 3 g of modified silica-coated nickel powder, 4 g of hyperbranched polyurethane, and 0.6 g of antioxidant 168 into a high-speed mixer and mix at 60° C. for 60 min; then place in a twin-screw extruder for melt mixing, and the temperatures of sections 1 to 6 are 200° C., 220° C., 250° C., 250° C., 260° C., and 240° C.; cool and discharge to obtain a polycarbonate composite material, thereby improving the bonding between the nickel powder and the polycarbonate plastic substrate.

[0037] Example 3

[0038] (1) Add 6 g of D,L-serine and 4 g of terephthalaldehyde to 20 mL of 5% sodium hydroxide aqueous solution, react at 40° C. for 4 h, then add 0.8 g of sodium borohydride at 30° C., react for 12 h, add petroleum ether for extraction, collect the aqueous phase after separation, add hydrochloric acid solution dropwise to adjust the pH to 5, until a precipitate is precipitated, filter, and wash with water to obtain a polymerized monomer.

[0039] (2) 5 g of the polymerization monomer and 0.45 g of p-toluenesulfonic acid were mixed and subjected to melt polycondensation reaction at 200° C. for 7 h. After cooling, the product was washed with methanol and dried to obtain a hyperbranched polyurethane.

[0040] (3) 20 g of silver powder was added to 150 mL of ethanol, and dispersed by ultrasonic vibration. Then, an ethanol solution containing 30 g of tetraethyl orthosilicate was added dropwise, and 5 mL of ammonia water was added. The mixture was reacted at 40° C. for 20 h. Then, an aqueous solution containing 1.2 g of KH560 was added dropwise, and the reaction was continued for 5 h. The mixture was filtered, washed with ethanol, and dried to obtain modified silica-coated silver powder.

[0041] (4) Add 100 g of polycarbonate, 5 g of modified silica-coated silver powder, 8 g of hyperbranched polyurethane, and 0.6 g of antioxidant 168 into a high-speed mixer and mix at 70° C. for 60 min; then place in a twin-screw extruder for melt mixing, and the temperatures of sections 1 to 6 are 200° C., 220° C., 250° C., 250° C., 260° C., and 240° C.; cool and discharge to obtain a polycarbonate composite material, thereby improving the bonding between the silver powder and the polycarbonate plastic substrate.

[0042] Comparative Example 1

[0043] 100 g of polycarbonate, 0.5 g of copper powder, 1 g of hyperbranched polyurethane and 0.6 g of antioxidant 168 were added into a high-speed mixer and mixed at 50° C. for 20 min. The mixture was then placed into a twin-screw extruder for melt mixing, with the temperatures of sections 1 to 6 being 200° C., 220° C., 250° C., 250° C., 260° C. and 240° C. The material was cooled and discharged to obtain a polycarbonate composite material.

[0044] Comparative Example 2

[0045] The modified silica-coated copper powder was prepared according to the method of Example 1.

[0046] 100 g of polycarbonate, 0.5 g of modified silica-coated copper powder, and 0.6 g of antioxidant 168 were added into a high-speed mixer and mixed at 50° C. for 20 min; then placed in a twin-screw extruder for melt mixing, with the temperatures of sections 1 to 6 being 200° C., 220° C., 250° C., 250° C., 260° C., and 240° C.; the material was cooled and discharged to obtain a polycarbonate composite material.

[0047] Comparative Example 3

[0048] The hyperbranched polyurethane was prepared according to the method of Example 1.

[0049] 100 g of polycarbonate, 1 g of hyperbranched polyurethane and 0.6 g of antioxidant 168 were added into a high-speed mixer and mixed at 50° C. for 20 min. The mixture was then placed into a twin-screw extruder for melt mixing, with the temperatures of sections 1 to 6 being 200° C., 220° C., 250° C., 250° C., 260° C. and 240° C. The material was cooled and discharged to obtain a polycarbonate composite material.

[0050] The impact strength of polycarbonate plastics is tested according to the method of GB / T 1843-2008. The tensile strength is tested according to the method of GB / T1040.1-2006.

[0051] Table 1 Polycarbonate plastic performance test table

[0052]

[0053] The hyperbranched polyurethane prepared in Examples 1-3 has good compatibility with polycarbonate, can improve the processing performance and rheology of polycarbonate, has a unique dendritic molecular chain, forms an interpenetrating cross-linked network with polycarbonate, and greatly improves the mechanical properties of polycarbonate such as impact strength and tensile strength.

[0054] Using tetraethyl orthosilicate as a silicon source, a transparent silica coating layer is formed on the surface of metal particles such as copper powder, nickel powder, and silver powder, and then modified with KH550 to obtain modified silica-coated metal particles. In addition, the epoxy group of KH560 on the surface of silica can react with the imino group in the hyperbranched polyurethane molecular chain, so that the hyperbranched polyurethane acts as a compatibilizer, which improves the dispersibility and compatibility of the modified silica-coated metal particles in the polycarbonate plastic substrate, so that the copper powder, silver powder and other metal particles will not affect the mechanical properties of polycarbonate.

[0055] The hyperbranched polyurethane in Comparative Example 1 cannot interact with the copper powder, and the copper powder has poor dispersibility in the polycarbonate plastic substrate, which has a great impact on the mechanical properties of the polycarbonate. In Comparative Example 2, no hyperbranched polyurethane is added, and the modified silica-coated copper powder has poor dispersibility in the polycarbonate than in Example 1, and the mechanical properties are lower than those of Example 1.

[0056] Metallic feel observation: Observe how close the texture of the polycarbonate surface is to metal, and rate it on a scale of 1-5. The higher the level, the stronger the metallic feel.

[0057] Level 1 means no metallic feeling; Level 2 means weak metallic feeling; Level 3 means moderate metallic feeling; Level 4 means strong metallic feeling; Level 5 means strong metallic feeling. Each sample is evaluated by 20 observers and the average value is taken.

[0058] Table 2 Observation table of metal feel of polycarbonate plastic

[0059] Metallic level Example 1 3.7 Example 2 4.2 Comparative Example 3 4.6 Comparative Example 1 2.7 Comparative Example 2 3.1 Comparative Example 3 0.7

[0060] The modified silica-coated metal particles of Examples 1-3 are uniformly dispersed in the polycarbonate matrix under the action of the hyperbranched polyurethane, giving the polycarbonate a good metallic appearance.

[0061] The metal copper powder of Comparative Example 1 was not modified by coating with silica and KH560, and could not interact with the hyperbranched polyurethane, and could not improve the dispersibility of the metal copper powder in the polycarbonate plastic substrate, and the metal appearance of the polycarbonate was poor. Comparative Example 2 did not add hyperbranched polyurethane, and the dispersibility of the modified silica-coated copper powder in the polycarbonate was worse than that of Example 1, and the metal appearance grade was lower than that of Example 1. Comparative Example 3 did not add metal copper powder, and the metal appearance of the polycarbonate was the worst.

Claims

1. A method for improving the bonding between metal particles and plastic substrates, It is characterized in that The steps include: S1. Add metal particles to ethanol, disperse them by ultrasonic vibration, then drop ethanol solution containing ethyl orthosilicate and ammonia water, react at 40-45°C for 10-20h, then drop aqueous solution containing KH560, continue to react for 3-5h, filter and wash to obtain modified silica-coated metal particles; S2, mixing and melt-mixing the plastic, the modified silica-coated metal particles, the hyperbranched polyurethane, and the antioxidant to improve the bonding between the metal particles and the plastic substrate; The preparation method of the hyperbranched polyamine ester is: (1) adding D,L-serine and terephthalaldehyde to a sodium hydroxide aqueous solution, reacting at a temperature of 35-50° C. for 4-8 hours, then adding sodium borohydride at a temperature of 20-30° C., reacting for 12-24 hours, collecting the aqueous phase after extraction and separation, adding a hydrochloric acid solution dropwise to adjust the pH to 4-5, precipitating a precipitate, filtering and washing to obtain a polymerized monomer; (2) mixing the polymerization monomer and p-toluenesulfonic acid, performing a melt polycondensation reaction, cooling and washing the product to obtain a hyperbranched polyurethane; The mass of D,L-serine in (1) is 135-150% of the mass of terephthalaldehyde; The mass of p-toluenesulfonic acid in (2) is 0.7-0.9% of the mass of the polymerized monomer; The melt polycondensation reaction in (2) is carried out at a temperature of 180-210° C. for 3-7 hours.

2. The method for improving the bonding between metal particles and plastic substrates according to claim 1, It is characterized in that The mass of tetraethyl orthosilicate and KH560 in S1 is 80-150% and 2-6% of the mass of the metal particles.

3. The method for improving the bonding between metal particles and plastic substrates according to claim 1, It is characterized in that The melt mixing method in S1 comprises: adding plastic, modified silica-coated metal particles and hyperbranched polyurethane into a high-speed mixer for mixing at a temperature of 50-70° C. for 20-60 min; then placing in a twin-screw extruder for melt blending at a temperature of 170-260° C. in sections 1 to 6; and cooling and discharging.

4. The method for improving the bonding between metal particles and plastic substrates according to claim 3, It is characterized in that The metal particles have a particle size of 5-150um and include silver powder, copper powder, nickel powder and iron powder.

5. The method for improving the bonding between metal particles and plastic substrates according to claim 3, It is characterized in that The plastics include polycarbonate, ABS, and polypropylene.

6. The method for improving the bonding between metal particles and plastic substrates according to claim 3, It is characterized in that The mass of the modified silicon dioxide-coated metal particles and the hyperbranched polyurethane is 0.5-5% and 1-8% of the mass of the plastic.

Citation Information

Patent Citations

  • Nylon for producing electric kettle and preparation method of nylon

    CN107760017A

  • Thermoplastic magnetic composite material and preparation method thereof

    CN110283373A

  • High-strength antioxidant polyethylene plastic and preparation method thereof

    CN115340716A

  • KR20220080796A