A method for preparing a hollow gel tube, and the hollow gel tube and applications thereof
By introducing traction materials and metal salt solutions of different densities into sodium alginate solution, and combining them with photocuring monomers and buffer solutions, hollow gel tubes with complex patterns and good mechanical properties were prepared. This solved the problems of complexity and simple structure in the existing technology, and is suitable for biomaterials and tissue engineering scaffolds.
Patent Information
- Application Number
- CN202211391567.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-08
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-11-08
Smart Images

Figure CN118001467B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of gel technology, and more specifically, to a method for preparing a hollow gel tube, the hollow gel tube itself, and its applications. Background Technology
[0002] Hydrogel scaffolds used in vascular tissue engineering should ideally meet requirements such as permeability, biodegradability, suitable mechanical properties, and good biocompatibility. With the development of tissue engineering, many techniques have been developed to prepare tubular gel tubes as tubular scaffolds, such as mold casting, freeze-drying, 3D printing, microfluidics, self-coiling, electrospinning, phase separation, and gas foaming. Each method for preparing tubular scaffolds has its own advantages and disadvantages, which are briefly summarized in Table 1.
[0003] Table 1
[0004]
[0005]
[0006] As can be seen from the above analysis, although the above methods provide a way to construct hydrogel tubes, these methods are either structurally simple, have poor mechanical properties, or are complicated or uncontrollable. Therefore, there is an urgent need for a simple method to prepare hollow hydrogel tubes with certain mechanical properties and complex patterns. Summary of the Invention
[0007] To address the aforementioned problems, this invention provides a method for preparing hollow gel tubes, as well as the hollow gel tubes and their applications. This method enables the simple and efficient preparation of gel tubes with various complex patterns, while also possessing good mechanical properties and biocompatibility, thus allowing the gel tubes to be well applied in the fields of biomaterials and tissue engineering scaffolds.
[0008] Firstly, one of the objectives of this invention is to provide a method for preparing hollow gel tubes.
[0009] Includes the following steps:
[0010] A metal salt solution is placed into a container with an injection port. A traction material is introduced at the front end of the injection port, and the metal salt solution is injected into a sodium alginate solution by the traction material to obtain a continuous hollow gel tube. The traction material is a gas or liquid that is insoluble in water and has a different density than the sodium alginate solution.
[0011] This invention utilizes the density difference between the traction material and the sodium alginate solution. A certain volume of traction material is introduced into the tip of the syringe. By changing the direction of the metal salt solution injected into the sodium alginate solution, such as upward or downward, a continuous hollow gel tube with a complex pattern can be obtained. This preparation method is simple and efficient, and the inner diameter of the hollow gel tube can be controlled by controlling the volume of the introduced traction material.
[0012] Specifically, the sodium alginate solution has a mass concentration of 2-4%, the metal salt solution has a mass concentration greater than 0 to saturation, and the metal salt solution is Ca... 2+ Mg 2+ Al 3+ Ba 2+ Fe 2+ Fe 3+ Cu 2+ Ag + Zn 2+ Mn 2+ One of the organic or inorganic salt solutions. Considering biocompatibility, the metal salt solution is preferably Ca... 2+ The solution is an organic or inorganic salt solution, particularly preferably a CaCl2 solution, and the mass concentration of the CaCl2 solution is 1-40%, preferably 5-20%.
[0013] In a preferred embodiment of the present invention, the traction material is one or a combination of air, pentane, cyclohexane, heptane, octane, hexadecane, liquid paraffin, pentanol, dodecanol, pentanal, hexanal, epichlorohydrin, dichloromethane, carbon tetrachloride, and carbon disulfide.
[0014] Furthermore, the method for preparing gel tubes also includes the following steps:
[0015] Hollow gel tubes are immersed in a mixed solution containing a photoinitiator and a monofunctional photocurable monomer, and then removed and photocured to form a composite double-network hollow gel tube.
[0016] Preferably, the hollow gel tube is immersed in the mixed solution for 3-24 hours at room temperature until it reaches equilibrium, and then removed. More preferably, the immersion time is 12 hours, and the light curing lamp source is preferably an ultraviolet lamp.
[0017] The concentration of the monofunctional photocurable monomer aqueous solution is 10wt% to 70wt%, and the monofunctional photocurable monomer is preferably one or a combination of hydroxypropyl acrylate (HPA), N-isopropylacrylamide (NIPAM), dimethylaminoethyl methacrylate (DAMEMA), acrylic acid (AA), dimethylaminoethyl acrylate (DMAEA), acryloyloxyethyltrimethylammonium chloride (DAC), potassium 2-acrylamido-2-methylpropanesulfonate (AMPS), sodium p-styrene sulfonate (NaSS), hydroxyethyl acrylate (HEA), and acrylamide (AAm).
[0018] It is worth mentioning that the addition of monofunctional photocurable monomers enables the gel tubes to become multifunctional. For example, hydroxypropyl acrylate (HPA), N-isopropylacrylamide (NIPAM), and dimethylaminoethyl methacrylate (DAMEMA) are temperature-sensitive monomers, acrylic acid (AA) and dimethylaminoethyl acrylate (DMAEA) are pH-responsive monomers, and acryloyloxyethyltrimethylammonium chloride (DAC), potassium 2-acrylamido-2-methylpropanesulfonate (AMPS), sodium p-styrenesulfonate (NaSS), hydroxyethyl acrylate (HEA), and acrylamide (AAm) are high-strength monomers. After curing, the photocurable monomers make the gel tubes perform better and endow them with more functions.
[0019] Furthermore, the amount of photoinitiator used is 0.1% to 2% of the mass of the monofunctional photocurable monomer. The photoinitiator can be a free radical photoinitiator or a cationic photoinitiator, preferably one or a combination of 2-hydroxy-2-methyl-phenylacetone-1, 1-hydroxy-cyclohexylbenzophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenylacetone-1, bis(dodecylbenzeneiodophenone), triphenyl sulfide, and phenylthiophenyl diphenyl sulfide. It is worth mentioning that the photoinitiator 2-hydroxy-2-methyl-phenylacetone-1 has high initiation efficiency and little effect on the color of the polymer when used in small amounts.
[0020] Furthermore, in the above preparation steps, the mixed solution also includes a multifunctional photocurable monomer. The amount of the multifunctional photocurable monomer is 0.1% to 2% of the mass of the monofunctional photocurable monomer, preferably one or a combination of polyethylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, and dimethylolpropane tetraacrylate. The addition of the multifunctional photocurable monomer further improves the performance of the gel tube; for example, polyethylene glycol diacrylate can significantly improve the mechanical properties of the polymer.
[0021] It is worth mentioning that the final performance of the composite double-network hollow gel tube can be controlled by adjusting the amount of photocurable monomer and the soaking time. The composite double-network hollow gel tube further improves the mechanical and physical properties of the gel tube and realizes the multi-functionality of the gel tube.
[0022] Furthermore, the preparation method of the gel tube also includes the following steps:
[0023] The composite double-network hollow gel tube is immersed in a neutral buffer solution to obtain a photocurable monomer-based hollow gel tube, wherein the pH of the buffer solution is 5.7 to 8.0; preferably a phosphate buffer solution, more preferably a phosphate buffer solution with pH 7.2.
[0024] It is worth mentioning that, based on the composite double-network hollow gel tube, this invention utilizes the soaking of a neutral buffer solution to de-crosslink the ionicly crosslinked sodium alginate gel, thereby removing the sodium alginate from the composite double-network hollow gel tube and obtaining a hollow gel tube containing only photocurable monomer material. This not only enriches the types of gel tubes but also further fills the gap in the preparation of gel tubes using photocurable monomers, providing a method for preparing photocurable monomer-based gel tubes.
[0025] Secondly, another objective of this invention is to provide a hollow gel tube.
[0026] Specifically, hollow gel tubes include sodium alginate-based hollow gel tubes, composite double-network hollow gel tubes, and photocurable monomer-based hollow gel tubes.
[0027] The sodium alginate-based hollow gel tube exhibits a cross-linked network structure, comprising a polymer and water. The polymer is sodium alginate and its metal salt ions, and the water content in the freshly prepared gel tube is greater than 90% by mass. This invention utilizes ion exchange between metal ions and sodium ions at the carboxyl groups of sodium alginate. Both sides of the sodium alginate carboxyl groups can react with metal ions, thereby cross-linking to form a gel. The sodium alginate-based gel tube system provided by this invention does not contain small molecules, thus maintaining the good biological properties of the sodium alginate hydrogel. The polymeric chain structure of sodium alginate is as follows:
[0028]
[0029] The composite double-network hollow gel tube is formed by combining sodium alginate-based gel tube with a photocurable monomer polymer. The composite double-network hollow gel tube further improves the mechanical and physical properties of the hollow gel tube and enriches its multifunctionality.
[0030] Photocurable monomer-based hollow gel tubes are obtained by removing sodium alginate through soaking in a neutral buffer solution based on composite double-network hollow gel tubes, filling the gap in photocurable monomer-based gel tubes and enriching the types of gel tube matrix materials.
[0031] Furthermore, a third objective of this invention is to provide applications for the aforementioned hollow gel tubes, applying them to the fields of biomaterials or tissue engineering scaffolds, preferably to the field of vascular tissue engineering scaffolds.
[0032] Compared with the prior art, the present invention has the following advantages:
[0033] 1. This invention utilizes sodium alginate solution and metal ion salt solution to prepare hollow gel tubes simply and efficiently through the introduction of traction material. The prepared gel tubes have good mechanical properties and biocompatibility, while also being able to accommodate complex patterns, making them well-suited for application in the field of biomaterials.
[0034] 2. This invention utilizes the change of direction of the traction object to prepare a gel tube with a complex structure, effectively solving the problems of cumbersome preparation, simple structure, expensive equipment, and limited substrate materials for gel tubes.
[0035] 3. This invention prepares a composite double-network hollow gel tube based on sodium alginate-based gel tube, which further improves the mechanical properties of the gel tube, enriches the multifunctionality of the gel tube, and effectively solves the problem of the single substrate material of the gel tube, and solves the problem that photocurable monomers cannot be used to prepare gel tubes.
[0036] 4. The hollow gel tube provided by this invention can simulate the shape of natural blood vessels in terms of structure, creating a three-dimensional culture environment; in terms of function, the hydrogel-based vascular tissue engineering scaffold can meet various needs such as tissue transplantation, physiological and pathological research, drug development and screening, and has broad application prospects in the field of tissue engineering. Attached Figure Description
[0037] Figure 1 These are actual images of the gel tubes prepared in Examples 21-30 of the present invention.
[0038] Figure 2 These are actual images of the gel tubes prepared in Examples 31-34 of this invention.
[0039] Figure 3 Physical images of gel tubes with different complex patterns prepared in Example 35 of this invention.
[0040] Figure 4 This is a photograph of the photocurable monomer-based hollow gel tube prepared in Example 54 of the present invention.
[0041] Figure 5 This is a photograph of the hollow gel tube of Comparative Example 2 of the present invention after being immersed in a buffer solution and then dissolved. Detailed Implementation
[0042] The present invention will now be described in detail with reference to the accompanying drawings and embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.
[0043] Example 1
[0044] Prepare a 2% (w / w) sodium alginate aqueous solution and a 10% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0045] Example 2
[0046] Prepare a 2% (w / w) sodium alginate aqueous solution and a 20% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0047] Example 3
[0048] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. Specific data are shown in Table 2.
[0049] Example 4
[0050] Prepare a 2% (w / w) sodium alginate aqueous solution and a 40% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0051] Example 5
[0052] Prepare a 2.5% sodium alginate aqueous solution and a 10% calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0053] Example 6
[0054] Prepare a 2.5% sodium alginate aqueous solution and a 20% calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 1.
[0055] Example 7
[0056] Prepare a 2.5% sodium alginate aqueous solution and a 30% calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. Specific data are shown in Table 2.
[0057] Example 8
[0058] Prepare a 2.5% (w / w) sodium alginate aqueous solution and a 40% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. Specific data are shown in Table 2.
[0059] Example 9
[0060] Prepare a 3% (w / w) sodium alginate aqueous solution and a 10% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0061] Example 10
[0062] Prepare a 3% (w / w) sodium alginate aqueous solution and a 20% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. Specific data are shown in Table 2.
[0063] Example 11
[0064] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. Specific data are shown in Table 2.
[0065] Example 12
[0066] Prepare a 3% (w / w) sodium alginate aqueous solution and a 40% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. Specific data are shown in Table 2.
[0067] Example 13
[0068] Prepare a 3.5% sodium alginate aqueous solution and a 10% calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0069] Example 14
[0070] Prepare a 3.5% sodium alginate aqueous solution and a 20% calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0071] Example 15
[0072] Prepare a 3.5% sodium alginate aqueous solution and a 30% calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0073] Example 16
[0074] Prepare a 3.5% sodium alginate aqueous solution and a 40% calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0075] Example 17
[0076] Prepare a 4% (w / w) sodium alginate aqueous solution and a 10% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0077] Example 18
[0078] Prepare a 4% (w / w) sodium alginate aqueous solution and a 20% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0079] Example 19
[0080] Prepare a 4% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. Specific data are shown in Table 1.
[0081] Example 20
[0082] Prepare a 4% (w / w) sodium alginate aqueous solution and a 40% (w / w) calcium chloride aqueous solution. Using air bubbles as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube is formed, it is left for 3 minutes, then removed and washed with deionized water to remove excess calcium chloride solution. The stress, strain, fracture strength, and toughness of the prepared gel tube are measured. The specific data are shown in Table 2.
[0083] Comparative Example 1
[0084] Prepare a 3% sodium alginate aqueous solution and a 30% calcium chloride aqueous solution. Without any traction, directly inject the calcium chloride solution into the sodium alginate solution; it forms a solid gel without hollow gel tubes.
[0085] As can be seen from the experimental results of Examples 1 to 20 and Comparative Example 1, the traction material is the key to achieving the preparation of hollow gel tubes. Without the traction material to pull the metal salt ion solution, it directly gels after being injected into the sodium alginate solution.
[0086] The tensile properties (GB / T1040-2006) test method is as follows: the sample is a hollow gel tube with different inner and outer diameters, and the tensile test is carried out by a universal tensile testing machine at a tensile speed of 30 mm / min until it breaks.
[0087] Table 2 below shows the tensile property test results of Examples 1-20 and Comparative Example 1, as detailed below:
[0088]
[0089]
[0090] The experimental results from Examples 1-20 show that, under the same concentration of sodium alginate solution, the mechanical properties of the gel tube gradually improve with the increase of calcium chloride solution concentration. However, when the concentration of calcium chloride solution reaches 40%, the mechanical properties of the gel tube decrease again. This is because excessive crosslinking density leads to brittleness of the gel tube. At the same time, under the same calcium chloride solution concentration, the mechanical properties of the gel tube gradually improve with the increase of sodium alginate solution concentration. However, when the concentration of sodium alginate solution reaches 3.5%, the mechanical properties of the gel tube decrease again. This is also due to excessive crosslinking density causing the gel tube to become brittle.
[0091] Meanwhile, under the same sodium alginate solution concentration, the mechanical properties of gel tubes formed by calcium chloride solutions of different concentrations showed roughly the same trend, exhibiting an initial increase followed by a decrease. This is because, under the same sodium alginate concentration, as the concentration of calcium chloride solution increases, calcium chloride diffuses more easily to form gel tubes. However, when the concentration of calcium chloride solution is too high, the cross-linking density is too high, which deteriorates the mechanical properties of the gel tubes.
[0092] After a series of mechanical property comparisons, the gel tubes formed when the sodium alginate solution concentration was 3% and the calcium chloride solution concentration was 30% exhibited the best mechanical properties.
[0093] Example 21
[0094] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using pentanol as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, let it stand for 3 minutes, then remove the gel tube and wash away excess calcium chloride solution in deionized water. Figure 1 It can be seen that a hollow gel tube is obtained.
[0095] Example 22
[0096] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using pentane as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, let it stand for 3 minutes, then remove the gel tube and wash off excess calcium chloride solution with deionized water. Figure 1 It can be seen that a hollow gel tube is obtained.
[0097] Example 23
[0098] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using cyclohexane as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, let it stand for 3 minutes, then remove the gel tube and wash off excess calcium chloride solution with deionized water. Figure 1 It can be seen that a hollow gel tube is obtained.
[0099] Example 24
[0100] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using heptane as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, let it stand for 3 minutes, then remove the gel tube and wash off excess calcium chloride solution with deionized water. Figure 1 It can be seen that a hollow gel tube is obtained.
[0101] Example 25
[0102] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using octane as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, let it stand for 3 minutes, then remove the gel tube and wash off excess calcium chloride solution with deionized water. Figure 1 It can be seen that a hollow gel tube is obtained.
[0103] Example 26
[0104] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using hexadecane as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, let it stand for 3 minutes, then remove the gel tube and wash away excess calcium chloride solution in deionized water. Figure 1 It can be seen that a hollow gel tube is obtained.
[0105] Example 27
[0106] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using liquid paraffin as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, it is left to stand for 3 minutes, then removed and rinsed with deionized water to remove excess calcium chloride solution. Figure 1 It can be seen that a hollow gel tube is obtained.
[0107] Example 28
[0108] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using dodecyl alcohol as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, let it stand for 3 minutes, then remove the gel tube and wash away excess calcium chloride solution in deionized water. Figure 1 It can be seen that a hollow gel tube is obtained.
[0109] Example 29
[0110] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using pentanal as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, let it stand for 3 minutes, then remove the gel tube and wash away excess calcium chloride solution in deionized water. Figure 1 It can be seen that a hollow gel tube is obtained.
[0111] Example 30
[0112] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using hexanal as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, let it stand for 3 minutes, then remove the gel tube and wash away excess calcium chloride solution in deionized water. Figure 1 It can be seen that a hollow gel tube is obtained.
[0113] Example 31
[0114] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using epichlorohydrin as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. After gel formation, let the tubes stand for 3 minutes, then remove them and wash away excess calcium chloride solution in deionized water. Figure 2 It can be seen that a hollow gel tube is obtained.
[0115] Example 32
[0116] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using dichloromethane as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. After gel formation, allow the tubes to stand for 3 minutes, then remove them and wash away excess calcium chloride solution in deionized water. Figure 2 It can be seen that a hollow gel tube is obtained.
[0117] Example 33
[0118] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using carbon tetrachloride as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. After gel formation, allow the tubes to stand for 3 minutes, then remove them and wash away excess calcium chloride solution in deionized water. Figure 2 It can be seen that a hollow gel tube is obtained.
[0119] Example 34
[0120] Prepare a 3% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using carbon disulfide as a traction medium, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. After the gel tubes form, let them stand for 3 minutes, then remove them and wash away excess calcium chloride solution in deionized water. Figure 2 It can be seen that a hollow gel tube is obtained.
[0121] From the appendix Figure 1 Appendix Figure 2 As shown in Examples 21-34, hollow gel tubes were obtained when air, alkanes, and dichloromethane were used as the traction material. In Examples 21-30, when liquid paraffin alkanes and other substances with a density lower than sodium alginate solution were used as the traction material for upward formation of the gel tube, the resulting gel tubes had good formability and mechanical properties. In Examples 31-34, when dichloroethane and other substances with a density higher than sodium alginate solution were used as the traction material for downward formation of the gel tube, the resulting gel tubes had slightly poorer performance. This is because the metal salt ion liquid inside the gel tube could not stay in place, and the metal salt solution would sink due to gravity.
[0122] Example 35
[0123] Prepare a 2% (w / w) sodium alginate aqueous solution and a 10% (w / w) calcium chloride aqueous solution. Using heptane as a tractor, by changing the direction of movement of heptane and calcium chloride, hollow gel tubes with complex patterns are prepared. Figure 3 It can be seen that hollow gel tubes with various complex patterns are obtained.
[0124] From Example 35 and Appendix Figure 3 It is evident that the present invention can simply and effectively prepare hollow gel tubes with various complex clusters.
[0125] Example 36
[0126] Prepare a 2% (w / w) sodium alginate aqueous solution and a 20% (w / w) copper nitrate aqueous solution. Using air bubbles as a traction medium, the copper nitrate solution is drawn into the sodium alginate solution, forming a hollow gel tube. After the gel tube forms, it is left to stand for 3 minutes, then the gel tube is removed and washed with deionized water to remove excess copper nitrate solution, thus obtaining the hollow gel tube.
[0127] Example 37
[0128] The preparation method in this embodiment is the same as that in Example 36, except that the metal salt solution is a 20% magnesium chloride aqueous solution, which yields hollow gel tubes.
[0129] Example 38
[0130] The preparation method in this embodiment is the same as that in Example 36, except that the metal salt solution is a 20% barium chloride aqueous solution, which yields hollow gel tubes.
[0131] Example 39
[0132] The preparation method in this embodiment is the same as that in Example 36, except that the metal salt solution is a 20% ferrous chloride aqueous solution, which yields hollow gel tubes.
[0133] Example 40
[0134] The preparation method in this embodiment is the same as that in Example 36, except that the metal salt solution is a 20% ferric chloride aqueous solution, which yields hollow gel tubes.
[0135] Example 41
[0136] The preparation method in this embodiment is the same as that in Example 36, except that the metal salt solution is a 20% aqueous solution of silver chloride, which yields hollow gel tubes.
[0137] Example 42
[0138] The preparation method in this embodiment is the same as that in Example 36, except that the metal salt solution is a 20% zinc chloride aqueous solution, which yields hollow gel tubes.
[0139] Example 43
[0140] The preparation method in this embodiment is the same as that in Example 36, except that the metal salt solution is a 20% manganese chloride aqueous solution, which yields hollow gel tubes.
[0141] Example 44
[0142] The preparation method in this embodiment is the same as that in Example 36, except that the metal salt solution is a 20% aluminum chloride aqueous solution, which yields hollow gel tubes.
[0143] Example 45
[0144] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. These gel tubes are then immersed in a mixed solution of hydroxypropyl acrylate and 2-hydroxy-2-methyl-phenylacetone-1, where the hydroxypropyl acrylate concentration is 50% and the amount of 2-hydroxy-2-methyl-phenylacetone-1 is 1% of the mass of hydroxypropyl acrylate. After immersion for 12 hours, the gel tubes are removed and exposed to light at an intensity of 80 mW / cm². 2 The gel tubes were cured under a 365nm UV lamp for 10 minutes. To prevent dehydration, the gel tubes were placed in water during the curing process. The stress and strain data of the obtained composite double-network hollow gel tubes are shown in Table 3.
[0145] Example 46
[0146] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. These gel tubes are then immersed in a mixed solution of hydroxypropyl acrylate and 2-hydroxy-2-methyl-phenylacetone-1 (60% hydroxypropyl acrylate solution, 1% of the hydroxypropyl acrylate mass). After immersion for 12 hours, the gel tubes are removed and exposed to light at an intensity of 80 mW / cm². 2 The gel tubes were cured under a 365nm UV lamp for 10 minutes. To prevent dehydration, the gel tubes were placed in water during the curing process. The stress and strain data of the prepared composite double-network hollow gel tubes are shown in Table 3.
[0147] Example 47
[0148] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. These gel tubes are then immersed in a mixed solution of 70% hydroxypropyl acrylate and 1-hydroxy-2-methyl-phenylacetone (1-hydroxypropyl acrylate). After 12 hours of immersion, the gel tubes are removed and exposed to light at an intensity of 80 mW / cm². 2 The gel tubes were cured under a 365nm UV lamp for 10 minutes. To prevent dehydration, the gel tubes were placed in water during the curing process. The stress and strain data of the prepared composite double-network hollow gel tubes are shown in Table 3.
[0149] Table 3 below shows the stress and strain performance test results of the composite double-network hollow gel tubes prepared in Examples 45-47 and the hollow gel tube prepared in Example 3. The specific data comparison is as follows:
[0150]
[0151]
[0152] The experimental results of Examples 45-47 show that, under the same concentration of sodium alginate solution, the stress and strain properties of the composite double-network hollow gel tube gradually increase with the increase of the hydroxypropyl acrylate solution concentration. Moreover, the stress and strain properties of the composite double-network hollow gel tubes prepared in Examples 45-47 are much greater than those of the hollow gel tube prepared in Example 3, indicating that the composite double-network hollow gel tube improves the mechanical and physical properties of the gel tube.
[0153] Example 48
[0154] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. The resulting gel tube is then immersed in a mixed solution of hydroxyethyl acrylate, acrylic acid, and 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl acetone-1. The concentrations of hydroxyethyl acrylate and acrylic acid solutions are 60%, and the amount of 2-hydroxy-2-methyl-p-hydroxyethyl ether phenyl acetone-1 is 0.2% of the total mass of hydroxyethyl acrylate and acrylic acid. After immersion for 10 hours, the gel tube is removed and exposed to light at an intensity of 80 mW / cm². 2 The gel tube was cured under a 365nm UV lamp for 10 minutes. To prevent the gel tube from losing water, it was placed in water during the curing process to obtain a composite double-network hollow gel tube.
[0155] Example 49
[0156] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming a hollow gel tube. The resulting gel tube is then immersed in a mixed solution of acrylamide, acryloyloxyethyltrimethylammonium chloride, and 1-hydroxycyclohexyl benzophenone. The concentration of acrylamide and acryloyloxyethyltrimethylammonium chloride solution is 25%, and the amount of 1-hydroxycyclohexyl benzophenone is 0.5% of the mass of acrylamide and acryloyloxyethyltrimethylammonium chloride. After immersion for 18 hours, the gel tube is removed and exposed to light at an intensity of 80 mW / cm². 2The gel tube was cured under a 365nm UV lamp for 10 minutes. To prevent the gel tube from losing water, it was placed in water during the curing process to obtain a composite double-network hollow gel tube.
[0157] Example 50
[0158] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. These gel tubes are then immersed in a mixed solution of N-isopropylacrylamide, dimethylaminoethyl acrylate, and didodecylbenzene iodide. The concentration of N-isopropylacrylamide and dimethylaminoethyl acrylate is 15%, and the amount of didodecylbenzene iodide is 2% of the mass of N-isopropylacrylamide and dimethylaminoethyl acrylate. After immersion for 12 hours, the gel tubes are removed and exposed to light at an intensity of 80 mW / cm². 2 The gel tube was cured under a 365nm UV lamp for 10 minutes. To prevent the gel tube from losing water, it was placed in water during the curing process to obtain a composite double-network hollow gel tube.
[0159] Example 51
[0160] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. These gel tubes are then immersed in a mixed solution of hydroxypropyl acrylate, dimethylaminoethyl methacrylate, 1-hydroxy-2-methylphenylacetone, and polyethylene glycol diacrylate. The concentrations of hydroxypropyl acrylate and dimethylaminoethyl methacrylate are 50%, the amount of 1-hydroxy-2-methylphenylacetone is 0.2% of the mass of hydroxypropyl acrylate and dimethylaminoethyl methacrylate, and the amount of polyethylene glycol diacrylate is 2% of the mass of hydroxypropyl acrylate and dimethylaminoethyl methacrylate. After immersion for 12 hours, the gel tubes are removed and exposed to light at an intensity of 80 mW / cm². 2 The gel tube was cured under a 365nm UV lamp for 10 minutes. To prevent the gel tube from losing water, it was placed in water during the curing process to obtain a composite double-network hollow gel tube.
[0161] Example 52
[0162] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. These gel tubes are then immersed in a mixed solution of potassium 2-acrylamide-2-methylpropanesulfonate, sodium p-styrene sulfonate, triphenyl sulfonate, tripropylene glycol diacrylate, and trimethylolpropane triacrylate. The concentrations of potassium 2-acrylamide-2-methylpropanesulfonate and sodium p-styrene sulfonate are 60%, the amount of triphenyl sulfonate is 1% of the mass of potassium 2-acrylamide-2-methylpropanesulfonate and sodium p-styrene sulfonate, and the amount of tripropylene glycol diacrylate and trimethylolpropane triacrylate is 0.5% of the mass of potassium 2-acrylamide-2-methylpropanesulfonate and sodium p-styrene sulfonate. After immersion for 12 hours, the gel tubes are removed and exposed to light at an intensity of 80 mW / cm². 2 The gel tube was cured under a 365nm UV lamp for 10 minutes. To prevent the gel tube from losing water, it was placed in water during the curing process to obtain a composite double-network hollow gel tube.
[0163] Example 53
[0164] Prepare a 2% (w / w) sodium alginate aqueous solution and a 30% (w / w) calcium chloride aqueous solution. Using air as a tractor, the calcium chloride solution is drawn into the sodium alginate solution, forming hollow gel tubes. The resulting gel tubes are then immersed in a mixed solution of dimethylaminoethyl methacrylate, phenylthiophenyl diphenylsulfonate, and dimethylolpropane tetraacrylate. The concentration of the dimethylaminoethyl methacrylate solution is 60%, the phenylthiophenyl diphenylsulfonate is 1% of the mass of dimethylaminoethyl methacrylate, and the amount of dimethylolpropane tetraacrylate is 1% of the mass of dimethylaminoethyl methacrylate. After immersion for 12 hours, the gel tubes are removed and cured for 10 minutes under a UV lamp with an intensity of 80 mW / cm² and a wavelength of 365 nm. To prevent water loss, the gel tubes are placed in water during curing to obtain composite double-network hollow gel tubes.
[0165] Example 54
[0166] The dual-network gel tubes prepared in Example 45 were immersed in PBS buffer solution at pH 7.2 for 3 hours to obtain photocurable monomer-based hollow gel tubes. Figure 4 It can be seen that after sodium alginate is dissolved, the hollow gel tube still maintains a good hollow tubular shape.
[0167] From the appendix Figure 4It is known that the gel network structure of sodium alginate is completely dissolved in the buffer solution, while the gel tube of the photocurable monomer base remains in a hollow gel tube state after the sodium alginate cross-linked network structure is dissolved. Therefore, the present invention provides a method for preparing gel tubes using photocurable monomer as a substrate material.
[0168] Comparison Sample 2
[0169] The hollow gel tubes prepared in Example 3 were immersed in PBS buffer solution with pH=7.2 for 3 hours, and it was found that the gel tubes completely dissolved and disappeared. Figure 5 This is a photograph of a hollow gel tube dissolved after being immersed in a buffer solution. Figure 5 It can be seen that the hollow gel tube gradually dissolves and disappears in the buffer solution.
[0170] In summary, the sodium alginate gel tube preparation method of this invention is simple, economical, and effective, and can prepare gel tubes with complex structures. It effectively solves the problems of cumbersome preparation, simple structure, and poor mechanical properties of gel tubes. Furthermore, it has good biocompatibility and can be well applied in the field of biomaterials. Based on this method, this invention can also prepare composite double-network gel tubes and photocurable monomer-based gel tubes, further improving the mechanical properties of gel tubes and solving the problem of single substrate materials for hollow gel tubes.
Claims
1. A method for preparing a hollow gel tube, characterized in that, The method includes the following steps: A metal salt solution is placed into a container containing an injection port. A traction material is introduced at the front end of the injection port. The direction of the metal salt solution being injected into the sodium alginate solution is controlled by the traction material to obtain a continuous hollow gel tube. The traction material is a gas or liquid that is insoluble in water and has a different density than the sodium alginate solution. The traction material is one or a combination of air, pentane, cyclohexane, heptane, octane, hexadecane, liquid paraffin, pentanol, dodecanol, pentanal, hexanal, epichlorohydrin, dichloromethane, carbon tetrachloride, and carbon disulfide. The sodium alginate solution has a mass concentration of 2% to 4%.
2. The method for preparing hollow gel tubes according to claim 1, characterized in that, The mass concentration of the metal salt solution is greater than 0 to saturation.
3. The method for preparing hollow gel tubes according to claim 2, characterized in that, The metal salt solution is Ca. 2+ Mg 2+ Al 3+ Ba 2+ Fe 2+ Fe 3+ Cu 2+ Ag + Zn 2+ Mn 2+ One of the organic or inorganic salt solutions.
4. The method for preparing hollow gel tubes according to claim 3, characterized in that, The metal salt solution is Ca. 2+ Organic or inorganic salt solutions.
5. The method for preparing a hollow gel tube according to claim 4, characterized in that, The metal salt solution is a CaCl2 solution, and the mass concentration of the CaCl2 solution is 1-40%.
6. The method for preparing a hollow gel tube according to claim 5, characterized in that, The mass concentration of the CaCl2 solution is 5-20%.
7. The method for preparing hollow gel tubes according to claim 1, characterized in that, The method further includes: The hollow gel tube is immersed in a mixed solution containing a photoinitiator and a monofunctional photocurable monomer, and then removed and photocured to form a composite double-network hollow gel tube. The concentration of the monofunctional photocurable monomer in the solution is 10wt%~70wt%, and the amount of the photoinitiator is 0.1%~2% of the mass of the monofunctional photocurable monomer.
8. The method for preparing a hollow gel tube according to claim 7, characterized in that, The monofunctional photocurable monomer is one or a combination of hydroxypropyl acrylate, N-isopropylacrylamide, dimethylaminoethyl methacrylate, acrylic acid, dimethylaminoethyl acrylate, acryloyloxyethyltrimethylammonium chloride, potassium 2-acrylamide-2-methylpropanesulfonate, sodium p-styrenesulfonate, hydroxyethyl acrylate, and acrylamide. The photoinitiator is a free radical photoinitiator or a cationic photoinitiator.
9. The method for preparing a hollow gel tube according to claim 8, characterized in that, The photoinitiator is one or a combination of 2-hydroxy-2-methyl-phenylacetone-1, 1-hydroxy-cyclohexylbenzophenone, 2-hydroxy-2-methyl-p-hydroxyethyl ether phenylacetone-1, bis(dodecyl)phenyliodide, triphenyl sulfide, and phenylthiophenyl diphenyl sulfide.
10. The method for preparing a hollow gel tube according to claim 7, characterized in that, The mixed solution also includes a multifunctional photocurable monomer, which is one or a combination of polyethylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate and dimethylolpropane tetraacrylate, and the amount of the multifunctional photocurable monomer is 0.1% to 2% of the mass of the monofunctional photocurable monomer.
11. The method for preparing hollow gel tubes according to claim 7 or 10, characterized in that, The method further includes: The composite double-network hollow gel tube was immersed in a neutral buffer solution to obtain a photocurable monomer-based hollow gel tube. The pH of the buffer solution is 5.7 to 8.
0.
12. A hollow gel tube obtained by the method according to any one of claims 1 to 11.
13. An application of the hollow gel tube according to claim 12, characterized in that, The gel tubes are used to prepare biomaterials or tissue engineering scaffolds.
14. The application of the hollow gel tube according to claim 13, characterized in that, The gel tubes are used to prepare vascular tissue engineering scaffolds.
Citation Information
Patent Citations
Preparation method of artificial tube
CN104610494A
Preparation method for sodium alginate hydrogel hollow tube with controllable inner diameter
CN105833342A