A method for preparing a peel-and-stick double-sided adhesive tape type bone adhesive
By preparing a bone adhesive that combines Zn2+-doped SiO2 nanoparticles with acylated chitosan and polyvinyl alcohol/tannic acid hydrogel, the problems of insufficient bonding strength, slow bonding time, and low strength of existing bone adhesives in the treatment of femoral trochanteric fractures were solved, achieving high-strength instantaneous bonding and stable bone fixation.
Patent Information
- Application Number
- CN202410148640.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-02-02
AI Technical Summary
Existing bone adhesives have problems in the treatment of femoral trochanteric fractures, such as insufficient bonding strength, slow bonding time, and low adhesive strength, resulting in poor fixation effects, especially in patients with osteoporosis.
A combination of Zn2+-doped SiO2 nanoparticles, acylated chitosan, and polyvinyl alcohol/tannic acid hydrogel was used to prepare a peel-and-stick double-sided adhesive tape-type bone adhesive by curing it with a photoinitiator. The adhesive strength was enhanced by electrostatic interaction and covalent bond formation, and the tape was laser-cut into tape form for use.
It achieves high-strength instantaneous bonding with a bonding strength exceeding 100 kPa and a self-strength exceeding 100 MPa, solving the long-term tensile, compressive, and shear strength requirements of adhesives within the body, and is easy to operate.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of medical biomaterial preparation technology, specifically relating to a method for preparing a peel-and-stick double-sided adhesive tape type bone adhesive. Background Technology
[0002] Intertrochanteric fractures of the femur account for 3-4% of all fractures, endangering the health and lives of tens of millions of people worldwide each year. More than 90% of these fractures occur in individuals over 65 years of age, many of whom suffer from osteoporosis. Transverse or oblique fractures are two of the most common types. Current clinical treatments include plates, screws, or intramedullary nails, but these are only suitable for fractures with good bone quality. For patients with osteoporosis, internal fixation methods such as screws are prone to shear failure, meaning the screws cannot be properly secured and often slip out. Therefore, using adhesives to fix the fracture site or help restore bone integrity is a new approach to fracture treatment. Most existing bone adhesives use liquid-phase injection to bond bone tissue. This method is simple to operate, adaptable to complex bone shapes, and allows for localized bonding via a syringe, ensuring sufficient adhesion between the adhesive and the bonding site, which is beneficial for adequate bone fixation. However, it also has drawbacks, such as: liquid-phase contact leading to potential reactions during injection; slow curing causing diffusion during operation; and weak adhesive strength resulting in insufficient bone bond strength. Using solid bone adhesives, such as double-sided tape-type bone adhesives, would be a convenient way to treat femoral trochanter fractures if the problem of liquid adhesives could be solved by simply applying the "double-sided tape" to the bone tissue to be bonded during treatment. Therefore, improving the immediate bonding strength (>100 kPa) of the "tape" is the top priority of this invention. In addition, the tensile, compressive, and shear strength, stiffness, and fatigue performance under long-term cyclic loading in vivo must also be considered. Therefore, the problem of insufficient strength of the bone adhesive itself remains urgent.
[0003] Improving the curing time and instantaneous bond strength (>100KPa) of bone adhesives, while ensuring the adhesives possess high intrinsic strength (flexural and compressive strength >100MPa), is a pressing issue that needs to be addressed in this research field.
[0004] Chinese Patent (Application No.: CN202310402320.9, Publication Date: 2023.04.14, Publication No.: CN116350833A) discloses a lysine-based antibacterial medical bone tissue adhesive, its preparation method, and its application. This bone adhesive is composed of the following raw materials: oxidized hyaluronic acid, polylysine, and tannic acid. The preparation method includes: 1. Dissolving hyaluronic acid in water to obtain a hyaluronic acid solution; 2. Adding sodium periodate to the hyaluronic acid solution, stirring in the dark, dialyzing in water, and then freeze-drying to obtain oxidized hyaluronic acid; 3. Dissolving the oxidized hyaluronic acid in an aqueous solution to form an oxidized hyaluronic acid solution; 4. Dissolving polylysine (mass content 3-7%) and tannic acid (mass content 8-24%) in water to obtain a mixed solution of polylysine and tannic acid; 5. Stirring and mixing the oxidized hyaluronic acid solution and the mixed solution of polylysine and tannic acid (mass ratio 6:3-7:8-24) to obtain a polylysine-based antibacterial medical bone tissue adhesive. Although the bone adhesive prepared by this invention solves the problems of adhesion and antibacterial properties to bone tissue, the adhesive strength is still low (<300KPa), and the bone adhesive is used by liquid injection, which does not solve the problems of slow curing time and easy dispersion during operation.
[0005] Chinese Patent (Application No.: CN202111677247.3, Publication Date: 2023.07.11, Publication No.: CN116407668A) discloses a fast-curing and biodegradable strong bone adhesive and its preparation method. The raw materials of this bone adhesive include: cyclohexene acetal monomer, oxidant, vinyl comonomer, crosslinking agent, and reducing agent. The steps for preparing the bone adhesive include: 1. Dissolving the oxidant in a cyclohexene acetal mixture in a certain proportion to obtain a mixed solution (the optimal molar ratio between the two is 1:1 to 1:2); 2. Uniformly mixing the vinyl monomer, crosslinking agent, and reducing agent in a certain proportion to obtain a mixed solution; 3. Uniformly mixing the two mixed solutions in a certain proportion and curing in situ to obtain a strong bone adhesive. Although the bone adhesive prepared by this invention has good curing speed, high bonding strength, and good degradation performance, its coating method for bonding pulverized bone fragments increases the difficulty of clinical operation.
[0006] Chinese Patent (Application No.: CN202110858919.4, Publication Date: 2021.11.02, Publication No.: CN113577371A) discloses an organic-inorganic hybrid hydrogel bone adhesive and its preparation method. The preparation method of the bone adhesive includes: 1. Mixing polysaccharide polymer and sodium periodate in a mass ratio of 1.5:1 to 2:1 and dissolving them in phosphate buffer solution (I) in the dark, reacting, dialyzing, and freeze-drying to obtain a hydrogel precursor, and then dissolving the precursor in phosphate buffer solution (II) to obtain a hydrogel precursor solution; 2. Dissolving the hydrogel precursor solution in CaCl2 solution to obtain solution A; 3. Uniformly mixing aminopolysaccharide solution and Na2CO3 solution to obtain solution B; 4. Injecting solutions A and B in a volume ratio of 1.5:1 to 2:1 into the reaction solution to obtain the bone adhesive hydrogel. Although the hydrogel bone adhesive prepared by this invention has strong mechanical strength and waterproof bonding performance, its bonding strength is too low, failing to meet the requirement of high bonding strength for bone adhesives. In addition, the curing time of this bone adhesive is about 10 minutes, which is slow and does not solve the problem of slow bonding.
[0007] Chinese patent (application number: CN202110768897.2, publication date: 2021.10.01, publication number: CN113456881A) discloses a nano-bone adhesive and its preparation method. The preparation method of the nano-bone adhesive includes: 1. preparing a solution of Ca(NO3)2·4H2O and P2O5 to obtain CDHA; 2. preparing Si-stabilized α-tricalcium phosphate nanoparticles (93.2–96.4 wt%); 3. preparing hydroxyapatite nanoparticles (2–3 wt%). Although the prepared nano-bone adhesive has excellent antibacterial properties, its adhesive strength is insufficient, its curing time is slow, and its clinical operation efficiency is low. Summary of the Invention
[0008] The purpose of this invention is to provide a method for preparing a peel-and-stick double-sided adhesive tape type bone adhesive, which solves the problems of insufficient bonding strength (<1MPa), slow bonding time (<30S), and low strength of the adhesive itself (<100MPa) of existing bone adhesives.
[0009] The technical solution adopted in this invention is a method for preparing a peel-and-stick bone adhesive, which is implemented according to the following steps:
[0010] Step 1, Preparation of Zn 2+ Doped with SiO2 nanoparticles;
[0011] Step 2: Prepare acylated chitosan;
[0012] Step 3: Prepare polyvinyl alcohol / tannic acid (PT) hydrogel;
[0013] Step 4: The powders obtained in Steps 1, 2, and 3 are mixed with 2-hydroxy-2-methylpropenone (HMPP) as a photoinitiator in a certain proportion to obtain the final PTC@ZS adhesive.
[0014] Step 5, prepare the adhesive tape;
[0015] The preferred method is as follows: In step 1, specifically: Tetraethyl silicate (TEOS) is dissolved in ethanol and stirred vigorously to obtain a TEOS solution with a mass concentration of 4–8 wt%. Hexadecyltrimethylammonium bromide (CTAB) is dissolved in deionized water to obtain a CTAB solution with a mass concentration of 5–9 wt%. The TEOS solution and CTAB solution are mixed uniformly at a volume ratio of 1:1.5–1:2.5. Zinc chloride with a mass concentration of 0.1–0.3 wt% is slowly added to the CTAB / TEOS solution, and the pH of the solution is adjusted to 8–12 with concentrated ammonium hydroxide. After stirring for 3–8 hours, the solution is washed three times with ethanol and distilled water, and centrifuged to obtain a white gel. The gel is dried in an oven at 85–125°C for 8–12 hours, and then calcined in a muffle furnace at 400–600°C for 1–3 hours (heating rate: 2°C / min). -1 ), thus obtaining ZS.
[0016] The preferred embodiment is as follows: In step 2, chitosan is dissolved in morpholine ethanesulfonic acid solution (0.1M, pH=6) and stirred until uniformly mixed. Then, at room temperature, coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) are dissolved in the above solution and mixed uniformly. The mixture is then centrifuged and freeze-dried to obtain acylated chitosan.
[0017] The molar ratio of CS:EDC:NHS is 1:1:1 to 1:4:20, and the mass concentration of CS is 2 to 8 wt%.
[0018] The preferred method is as follows: In step 3, specifically: polyvinyl alcohol (PVA) is dissolved in dimethyl sulfoxide, and NaHSO4·H2O is added at 80–120°C; when the reaction temperature is lowered to 60–80°C, tannic acid (TA) is added, and the reaction is carried out at 80°C under N2 conditions for 24–36 hours. Afterwards, the product is purified by dialysis membrane for 3 days and then freeze-dried.
[0019] The mass ratio of PVA to TA is 1:1 to 1:1.5, and the mass concentration of polyvinyl alcohol is 20 to 40 wt%. The freezing temperature is -20 to 40°C, and the drying time is 12 to 48 hours. Tannic acid can also be replaced by polyphenols such as dopamine and its derivatives, catechol, pyrogallol, and catechol.
[0020] The preferred embodiment is as follows: In step 4, ZS, acylated chitosan, and PT prepared in steps 1, 2, and 3 are uniformly mixed at a mass ratio of 1:20:50 to 1:25:100, and 1 to 5% (w / w) of 2-hydroxy-2-methylpropenone (HMPP) is added as a photoinitiator. The mixture is then cured under a UV lamp (284nm, 10W) for 20 minutes to obtain the final PTC@ZS adhesive.
[0021] The preferred solution is as follows: In step 5, specifically, the PTC@ZS adhesive is cut into equal parts of uniform size using a laser cutter, polyethylene is selected as the release paper, the adhesive is covered on the polyethylene film, and dried in an oven (30-60 minutes, drying temperature 35-50℃) to allow the adhesive to adhere to the release paper and obtain the tape.
[0022] The beneficial effects of this invention are: the self-adhesive double-sided tape type bone adhesive prepared by this invention first prepares Zn 2+ Doped silica nanoparticles were then used to prepare PVA-TA colloids via solution polymerization. Chitosan was then acylated to prepare acylated chitosan. Finally, the prepared PVA-TA powder was... 2+ Bone adhesive is obtained by uniformly mixing doped silica nanoparticles and acylated chitosan in a certain proportion and curing them under ultraviolet light for a certain period of time. The prepared bone adhesive is then cut into specific sizes using laser cutting technology. Polyethylene is used as release paper, and the mixture is dried in an oven to ensure full adhesion between the bone adhesive and the release paper, resulting in a "tape". This prepared "tape" type bone adhesive solves the problems of low bonding strength, slow bonding time, and excessively low bonding strength during bonding, as well as the failure of the adhesive in vivo due to its own low strength.
[0023] The multidentate structure of tannic acid effectively links with polyvinyl alcohol (PVA) polymer chains. This interconnection between tannic acid and PVA chains increases the molecular weight in the form of a PVA-TA-PVA network, thus increasing the adhesive's viscosity and tackiness. In existing adhesives, a small amount of tannic acid is typically added to act as a crosslinking agent, resulting in adhesives that are usually film-like or "liquid" colloids. However, this invention, by increasing the tannic acid content (10-50 times), not only increases the molecular weight of PVA and reduces its water solubility, but also prepares a "solid" adhesive with the unique adhesive properties of tannic acid. Chitosan, a biocompatible and biodegradable polysaccharide, can form hydrogen bonds and electrostatic interactions with tannic acid, further increasing the adhesive's viscosity. To further construct a stable adhesive interface, two coupling agents, N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS), are used. Covalent bond formation is promoted through amide synthesis chemistry, constructing a covalent bond interface based on specific carboxyl groups on the tissue surface. Bridging polymers with amino functional groups can be electrostatically attracted and adsorbed onto the surface, allowing the primary amine groups to covalently bond with the carboxyl groups on both the adhesive and the tissue surface, further increasing the adhesive strength. Finally, Zn... 2+ The addition of doped silica nanoparticles leads to the continuous release of Zn. 2+ Not only does it form metal-catecholamine coordination with tannins and amines, increasing the adhesive's bonding properties, but Zn also... 2+ It also possesses good osteogenic activity and plays a positive role in enhancing bone formation. Furthermore, Zn... 2+ The doped silica nanoparticles enhance the entanglement of polymer chains, further increasing the mechanical strength of the adhesive itself. Detailed Implementation
[0024] The present invention will now be described in detail with reference to specific embodiments.
[0025] Example 1
[0026] Step 1: Tetraethyl silicate (TEOS) was dissolved in ethanol and stirred vigorously to obtain a 4 wt% TEOS solution. Hexadecyltrimethylammonium bromide (CTAB) was dissolved in deionized water to obtain a 5 wt% CTAB solution. The TEOS and CTAB solutions were mixed uniformly at a volume ratio of 1:1.5. Zinc chloride (0.1 wt%) was slowly added to the CTAB / TEOS solution, and the pH was adjusted to 8 with concentrated ammonium hydroxide. After stirring for 3 hours, the solution was washed three times with ethanol and distilled water, and centrifuged to obtain a white gel. The gel was dried in an oven at 85°C for 8 hours and then calcined in a muffle furnace at 400°C for 1 hour (heating rate: 2°C / min). -1 ), thus obtaining ZS;
[0027] Step 2: Dissolve 2 wt% chitosan in morpholine ethanesulfonic acid solution (0.1 M, pH = 6) and stir until homogeneous. Then, at room temperature, dissolve the coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) in the above solution at a molar ratio of 1:1:1 and mix them homogeneously. Centrifuge and freeze-dry to obtain acylated chitosan.
[0028] Step 3: 20 wt% polyvinyl alcohol (PVA) was dissolved in dimethyl sulfoxide, and 1% (w / v) NaHSO4·H2O was added at 80°C. When the reaction temperature was lowered to 60°C, tannic acid (TA) was added, with a PVA / TA mass ratio of 1:1. The reaction was carried out at 80°C under N2 for 12 hours. The product was then purified by dialysis for 3 days and freeze-dried (-20°C, 12 hours).
[0029] Step 4: The ZS, acylated chitosan, and PT prepared in steps 1, 2, and 3 are uniformly mixed in a mass ratio of 1:20:50, and 1% (w / w) of 2-hydroxy-2-methylpropenone (HMPP) is added as a photoinitiator. The mixture is then cured under a UV lamp (284nm, 10W) for 20 minutes to obtain the final PTC@ZS adhesive.
[0030] Step 5: Use a laser cutter to cut the PTC@ZS adhesive into uniform portions. Select polyethylene as the release paper, cover the adhesive onto the polyethylene film, and dry it in an oven (50 minutes, drying temperature 35℃) to bond the adhesive with the release paper to obtain the tape.
[0031] Example 2
[0032] Step 1: Tetraethyl silicate (TEOS) was dissolved in ethanol and stirred vigorously to obtain a 4.5 wt% TEOS solution. Hexadecyltrimethylammonium bromide (CTAB) was dissolved in deionized water to obtain a 5.5 wt% CTAB solution. The TEOS and CTAB solutions were mixed uniformly at a volume ratio of 1:1.7. Zinc chloride (0.13 wt%) was slowly added to the CTAB / TEOS solution, and the pH was adjusted to 8.5 with concentrated ammonium hydroxide. After stirring for 3.5 hours, the solution was washed three times with ethanol and distilled water, and centrifuged to obtain a white gel. The gel was dried in an oven at 90°C for 8.5 hours, and then calcined in a muffle furnace at 450°C for 1–3 hours (heating rate: 2°C / min). -1 ), thus obtaining ZS;
[0033] Step 2: Dissolve 3 wt% chitosan in morpholine ethanesulfonic acid solution (0.1 M, pH = 6) and stir until homogeneous. Then, at room temperature, dissolve the coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) in the above solution at a molar ratio of 1:1:5 and mix them homogeneously. Centrifuge and freeze-dry to obtain acylated chitosan.
[0034] Step 3: 22 wt% polyvinyl alcohol (PVA) was dissolved in dimethyl sulfoxide, and 1% (w / v) NaHSO4·H2O was added at 85°C. When the reaction temperature was lowered to 65°C, tannic acid (TA) was added, with a PVA / TA mass ratio of 1:1.1. The reaction was carried out at 80°C under N2 for 15 hours. The product was then purified by dialysis for 3 days and freeze-dried (-22°C, 15 hours).
[0035] Step 4: The ZS, acylated chitosan, and PT prepared in steps 1, 2, and 3 are uniformly mixed in a mass ratio of 1:20:60, and 1.5% (w / w) of 2-hydroxy-2-methylpropenone (HMPP) is added as a photoinitiator. The mixture is then cured under a UV lamp (284nm, 10W) for 20 minutes to obtain the final PTC@ZS adhesive.
[0036] Step 5: Use a laser cutter to cut the PTC@ZS adhesive into uniform portions. Select polyethylene as the release paper, cover the adhesive onto the polyethylene film, and dry it in an oven (50 minutes, drying temperature 40℃) to bond the adhesive with the release paper to obtain the tape.
[0037] Example 3
[0038] Step 1: Tetraethyl silicate (TEOS) was dissolved in ethanol and stirred vigorously to obtain a 5 wt% TEOS solution. Hexadecyltrimethylammonium bromide (CTAB) was dissolved in deionized water to obtain a 6 wt% CTAB solution. The TEOS and CTAB solutions were mixed uniformly at a volume ratio of 1:1.9. Zinc chloride (0.15 wt%) was slowly added to the CTAB / TEOS solution, and the pH was adjusted to 9 with concentrated ammonium hydroxide. After stirring for 4 hours, the solution was washed three times with ethanol and distilled water, and centrifuged to obtain a white gel. The gel was dried in an oven at 100°C for 9 hours, and then calcined in a muffle furnace at 450°C for 1–3 hours (heating rate: 2°C / min). -1 ), thus obtaining ZS;
[0039] Step 2: Chitosan with a mass concentration of 4 wt% was dissolved in morpholine ethanesulfonic acid solution (0.1 M, pH = 6) and stirred until homogeneous. Then, coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were dissolved in the above solution at a molar ratio of 1:3:8 and mixed homogeneously. The mixture was then centrifuged and freeze-dried to obtain acylated chitosan.
[0040] Step 3: 25 wt% polyvinyl alcohol (PVA) was dissolved in dimethyl sulfoxide, and 2% (w / v) NaHSO4·H2O was added at 90°C. When the reaction temperature was lowered to 65°C, tannic acid (TA) was added, with a PVA / TA mass ratio of 1:1.15. The reaction was carried out at 80°C under N2 for 18 hours. The product was then purified by dialysis for 3 days and freeze-dried (-25°C, 20 hours).
[0041] Step 4: The ZS, acylated chitosan, and PT prepared in steps 1, 2, and 3 are uniformly mixed in a mass ratio of 1:20:65, and 2% (w / w) of 2-hydroxy-2-methylpropenone (HMPP) is added as a photoinitiator. The mixture is then cured under a UV lamp (284nm, 10W) for 20 minutes to obtain the final PTC@ZS adhesive.
[0042] Step 5: Use a laser cutter to cut the PTC@ZS adhesive into uniform portions. Select polyethylene as the release paper, cover the adhesive onto the polyethylene film, and dry it in an oven (30 minutes, drying temperature 55℃) to bond the adhesive with the release paper to obtain the tape.
[0043] Example 4
[0044] Step 1: Tetraethyl silicate (TEOS) was dissolved in ethanol and stirred vigorously to obtain a 5.5 wt% TEOS solution. Hexadecyltrimethylammonium bromide (CTAB) was dissolved in deionized water to obtain a 6.5 wt% CTAB solution. The TEOS and CTAB solutions were mixed uniformly at a volume ratio of 1:2. Zinc chloride (0.18 wt%) was slowly added to the CTAB / TEOS solution, and the pH was adjusted to 9.5 with concentrated ammonium hydroxide. After stirring for 4.5 hours, the solution was washed three times with ethanol and distilled water, and centrifuged to obtain a white gel. The gel was dried in an oven at 105°C for 9.5 hours, and then calcined in a muffle furnace at 500°C for 1–3 hours (heating rate: 2°C / min). -1 ), thus obtaining ZS;
[0045] Step 2: Chitosan with a mass concentration of 5 wt% was dissolved in morpholine ethanesulfonic acid solution (0.1 M, pH = 6) and stirred until homogeneous. Then, coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were dissolved in the above solution at a molar ratio of 1:5:9 and mixed homogeneously. The mixture was then centrifuged and freeze-dried to obtain acylated chitosan.
[0046] Step 3: 28 wt% polyvinyl alcohol (PVA) was dissolved in dimethyl sulfoxide, and 2.5% (w / v) NaHSO4·H2O was added at 95°C. When the reaction temperature was lowered to 65°C, tannic acid (TA) was added at a PVA / TA mass ratio of 1:1.2. The reaction was carried out at 80°C under N2 for 20 h. The product was then purified by dialysis for 3 days and freeze-dried (-30°C, 25 h).
[0047] Step 4: The ZS, acylated chitosan, and PT prepared in steps 1, 2, and 3 are uniformly mixed in a mass ratio of 1:20:70, and 3% (w / w) of 2-hydroxy-2-methylpropenone (HMPP) is added as a photoinitiator. The mixture is then cured under a UV lamp (284nm, 10W) for 20 minutes to obtain the final PTC@ZS adhesive.
[0048] Step 5: Use a laser cutter to cut the PTC@ZS adhesive into uniform portions. Select polyethylene as the release paper, cover the adhesive onto the polyethylene film, and dry it in an oven (40 minutes, drying temperature 45℃) to bond the adhesive with the release paper to obtain the tape.
[0049] Example 5
[0050] Step 1: Tetraethyl silicate (TEOS) was dissolved in ethanol and stirred vigorously to obtain a 6 wt% TEOS solution. Hexadecyltrimethylammonium bromide (CTAB) was dissolved in deionized water to obtain a 7 wt% CTAB solution. The TEOS and CTAB solutions were mixed uniformly at a volume ratio of 1:2.2. Zinc chloride (0.22 wt%) was slowly added to the CTAB / TEOS solution, and the pH was adjusted to 10 with concentrated ammonium hydroxide. After stirring for 5 hours, the solution was washed three times with ethanol and distilled water, and centrifuged to obtain a white gel. The gel was dried in an oven at 110°C for 10 hours and then calcined in a muffle furnace at 550°C for 2 hours (heating rate: 2°C / min). -1 ), thus obtaining ZS;
[0051] Step 2: Chitosan with a mass concentration of 6 wt% was dissolved in morpholine ethanesulfonic acid solution (0.1 M, pH = 6) and stirred until homogeneous. Then, coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were dissolved in the above solution at a molar ratio of 1:7:10 and mixed homogeneously. The mixture was then centrifuged and freeze-dried to obtain acylated chitosan.
[0052] Step 3: 30 wt% polyvinyl alcohol (PVA) was dissolved in dimethyl sulfoxide, and 3% (w / v) NaHSO4·H2O was added at 100°C. When the reaction temperature was lowered to 70°C, tannic acid (TA) was added, with a PVA / TA mass ratio of 1:1.25. The reaction was carried out at 80°C under N2 for 25 hours. The product was then purified by dialysis for 3 days and freeze-dried (-35°C, 25 hours).
[0053] Step 4: The ZS, acylated chitosan, and PT prepared in steps 1, 2, and 3 are uniformly mixed in a mass ratio of 1:25:80, and 3.5% (w / w) of 2-hydroxy-2-methylpropenone (HMPP) is added as a photoinitiator. The mixture is then cured under a UV lamp (284nm, 10W) for 20 minutes to obtain the final PTC@ZS adhesive.
[0054] Step 5: Use a laser cutter to cut the PTC@ZS adhesive into uniform portions. Use polyethylene as the release paper and dry it in an oven (45 minutes at 40°C) to bond the adhesive with the release paper to obtain the tape.
[0055] Example 6
[0056] Step 1: Tetraethyl silicate (TEOS) was dissolved in ethanol and stirred vigorously to obtain a 6.5 wt% TEOS solution. Hexadecyltrimethylammonium bromide (CTAB) was dissolved in deionized water to obtain a 7.5 wt% CTAB solution. The TEOS and CTAB solutions were mixed uniformly at a volume ratio of 1:2.3. Zinc chloride (0.25 wt%) was slowly added to the CTAB / TEOS solution, and the pH was adjusted to 11 with concentrated ammonium hydroxide. After stirring for 6 hours, the solution was washed three times with ethanol and distilled water, and centrifuged to obtain a white gel. The gel was dried in an oven at 115°C for 11 hours and then calcined in a muffle furnace at 550°C for 2 hours (heating rate: 2°C / min). -1 ), thus obtaining ZS;
[0057] Step 2: Chitosan with a mass concentration of 7 wt% was dissolved in morpholine ethanesulfonic acid solution (0.1 M, pH = 6) and stirred until homogeneous. Then, coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were dissolved in the above solution at a molar ratio of 1:5:15 and mixed homogeneously. The mixture was then centrifuged and freeze-dried to obtain acylated chitosan.
[0058] Step 3: 35 wt% polyvinyl alcohol (PVA) was dissolved in dimethyl sulfoxide, and 4% (w / v) NaHSO4·H2O was added at 105 °C. When the reaction temperature was lowered to 75 °C, tannic acid (TA) was added, with a PVA / TA mass ratio of 1:1.3. The reaction was carried out at 80 °C under N2 for 28 h. Afterwards, the product was purified by dialysis for 3 days and then freeze-dried (-35 °C, 40 h).
[0059] Step 4: The ZS, acylated chitosan, and PT prepared in steps 1, 2, and 3 are uniformly mixed in a mass ratio of 1:25:85, and 4% (w / w) of 2-hydroxy-2-methylpropenone (HMPP) is added as a photoinitiator. The mixture is then cured under a UV lamp (284nm, 10W) for 20 minutes to obtain the final PTC@ZS adhesive.
[0060] Step 5: Use a laser cutter to cut the PTC@ZS adhesive into uniform portions. Select polyethylene as the release paper, cover the adhesive onto the polyethylene film, and dry it in an oven (55 minutes, drying temperature 35℃) to bond the adhesive with the release paper to obtain the tape.
[0061] Example 7
[0062] Step 1: Tetraethyl silicate (TEOS) was dissolved in ethanol and stirred vigorously to obtain a 7 wt% TEOS solution. Hexadecyltrimethylammonium bromide (CTAB) was dissolved in deionized water to obtain an 8 wt% CTAB solution. The TEOS and CTAB solutions were mixed uniformly at a volume ratio of 1:2.5. Zinc chloride (0.28 wt%) was slowly added to the CTAB / TEOS solution, and the pH was adjusted to 12 with concentrated ammonium hydroxide. After stirring for 7 hours, the solution was washed three times with ethanol and distilled water, and centrifuged to obtain a white gel. The gel was dried in an oven at 120°C for 11.5 hours and then calcined in a muffle furnace at 580°C for 2.5 hours (heating rate: 2°C / min). -1 ), thus obtaining ZS;
[0063] Step 2: Chitosan with a mass concentration of 7 wt% was dissolved in morpholine ethanesulfonic acid solution (0.1 M, pH = 6) and stirred until homogeneous. Then, coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were dissolved in the above solution at a molar ratio of 1:6:15 and mixed homogeneously. The mixture was then centrifuged and freeze-dried to obtain acylated chitosan.
[0064] Step 3: Polyvinyl alcohol (PVA) with a mass concentration of 35 wt% was dissolved in dimethyl sulfoxide, and 4.5% (w / v) NaHSO4·H2O was added at 110 °C. When the reaction temperature was lowered to 75 °C, tannic acid (TA) was added, with a polyvinyl alcohol / tannic acid mass ratio of 1:1.4. The reaction was carried out at 80 °C under N2 purging for 30 h. Afterwards, the product was purified by dialysis membrane for 3 days and then freeze-dried (-35 °C, 45 h).
[0065] Step 4: The ZS, acylated chitosan, and PT prepared in steps 1, 2, and 3 are uniformly mixed in a mass ratio of 1:25:90, and 4.5% (w / w) of 2-hydroxy-2-methylpropenone (HMPP) is added as a photoinitiator. The mixture is then cured under a UV lamp (284nm, 10W) for 20 minutes to obtain the final PTC@ZS adhesive.
[0066] Step 5: Use a laser cutter to cut the PTC@ZS adhesive into uniform portions. Select polyethylene as the release paper, cover the adhesive onto the polyethylene film, and dry it in an oven (40 minutes, drying temperature 50℃) to bond the adhesive with the release paper to obtain the tape.
[0067] Example 8
[0068] Step 1: Tetraethyl silicate (TEOS) was dissolved in ethanol and stirred vigorously to obtain an 8 wt% TEOS solution. Hexadecyltrimethylammonium bromide (CTAB) was dissolved in deionized water to obtain a 9 wt% CTAB solution. The TEOS and CTAB solutions were mixed uniformly at a volume ratio of 1:2.5. Zinc chloride (0.3 wt%) was slowly added to the CTAB / TEOS solution, and the pH was adjusted to 12 with concentrated ammonium hydroxide. After stirring for 3-8 hours, the solution was washed three times with ethanol and distilled water, and centrifuged to obtain a white gel. The gel was dried in an oven at 125°C for 12 hours, and then calcined in a muffle furnace at 600°C for 3 hours (heating rate: 2°C / min). -1 ), thus obtaining ZS;
[0069] Step 2: Chitosan with a mass concentration of 7 wt% was dissolved in morpholine ethanesulfonic acid solution (0.1 M, pH = 6) and stirred until homogeneous. Then, coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were dissolved in the above solution at a molar ratio of 1:5:20 and mixed homogeneously. The mixture was then centrifuged and freeze-dried to obtain acylated chitosan.
[0070] Step 3: 40 wt% polyvinyl alcohol (PVA) was dissolved in dimethyl sulfoxide, and 5% (w / v) NaHSO4·H2O was added at 120°C. When the reaction temperature was lowered to 80°C, tannic acid (TA) was added, with a PVA / TA mass ratio of 1:1.5. The reaction was carried out at 80°C under N2 purging for 36 hours. The product was then purified by dialysis for 3 days and freeze-dried (-40°C, 48 hours).
[0071] Step 4: The ZS, acylated chitosan, and PT prepared in steps 1, 2, and 3 are uniformly mixed in a mass ratio of 1:25:90, and 5% (w / w) of 2-hydroxy-2-methylpropenone (HMPP) is added as a photoinitiator. The mixture is then cured under a UV lamp (284nm, 10W) for 20 minutes to obtain the final PTC@ZS adhesive.
[0072] Step 5: Use a laser cutter to cut the PTC@ZS adhesive into uniform portions. Select polyethylene as the release paper, cover the polyethylene film with the adhesive, and dry it in an oven (30 minutes, drying temperature 50℃) to bond the adhesive with the release paper to obtain the tape.
[0073] The following are comparisons of the bonding performance, bonding time, and degradation rate of the adhesive tape bone adhesive and the light-cured liquid injection bone adhesive prepared in the embodiments of the present invention at different times (the bonding substrate is bone fragments).
[0074] Table 1 Comparison of bonding performance between other bone adhesives and the bone adhesive of this invention
[0075]
[0076]
[0077] Table 2 Comparison of bonding performance of other bone adhesives and the bone adhesive of the present invention at different time points in PBS solution.
[0078]
[0079] Table 3 Comparison of intrinsic strength properties between other bone adhesives and the bone adhesive of this invention.
[0080]
[0081]
[0082] As can be seen from Tables 1 and 2, compared with existing light-cured bone adhesives, the peelable tape-type bone adhesive prepared by this invention has the advantages of being a solid colloid formed directly from tannins and polyvinyl alcohol, and having a cross-linked polymer network with Zn. 2+ The doped silica agglomerates wrapped around the surface of the nanoparticles facilitate curing. Therefore, compared to photocuring, the curing time is significantly shortened, which is beneficial for the immediate bonding of small bone fragments. The hydrogen bonding interaction between the catechol groups in tannic acid and the tissue, and the covalent interaction between oxidized catechol quinones and the tissue, are the main reasons for the rapid bonding of the adhesive. 2+ The silica in the doped silica aggregates can provide oxygen to accelerate the oxidation of tannic acid, and the nanoparticles enhance the entanglement of the polymer network, thus facilitating the polymer / Zn exchange process. 2+ The debonding process of doped silica complexes provides energy dissipation sites, and the combined effect of these factors enhances the mechanical properties of the adhesive.
Claims
1. A method for preparing a peel-and-stick double-sided adhesive tape-type bone adhesive, characterized in that, The specific steps are as follows: Step 1, Preparation of Zn 2+ Doped with SiO2 nanoparticles; Step 2, preparation of acylated chitosan: Chitosan is dissolved in a 0.1M, pH 6 morpholine ethanesulfonic acid solution and stirred until homogeneous. Then, at room temperature, the coupling agents N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide are dissolved in the above solution and mixed homogeneously. The mixture is then centrifuged and freeze-dried to obtain acylated chitosan. The molar ratio of chitosan to N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride to N-hydroxysuccinimide is 1:1:1 to 1:4:20, and the mass concentration of chitosan is 2-8 wt%. Step 3: Prepare polyvinyl alcohol / tannic acid hydrogel; Step 4, the Zn prepared in steps 1, 2, and 3 2+ SiO2 nanoparticles, acylated chitosan, and polyvinyl alcohol / tannic acid hydrogel were uniformly mixed at a mass ratio of 1:20:50 to 1:25:100, and 2-hydroxy-2-methylpropenone was added as a photoinitiator. The mass percentage of the photoinitiator was 1% to 5% of the total mass of the three components. The mixture was cured under a UV lamp for 20 minutes to obtain the final PTC@ZS adhesive.
2. The preparation method according to claim 1, characterized in that, The specific steps of step 3 are as follows: dissolve polyvinyl alcohol in dimethyl sulfoxide, add NaHSO4·H2O at 80~120℃; when the reaction temperature is reduced to 60~80℃, add tannic acid, and react at 80℃ under N2 conditions for 24~36h; then purify by dialysis membrane for 3 days, and freeze dry.
3. The preparation method according to claim 2, characterized in that, The mass ratio of polyvinyl alcohol to tannic acid is 1:1 to 1:1.5, the mass concentration of polyvinyl alcohol is 20 to 40 wt%, the freezing temperature is -20 to -40℃, and the drying time is 12 to 48 h.
4. The preparation method according to claim 1, characterized in that, In step 4, the ultraviolet lamp has a wavelength of 284nm and a power of 10W.
5. A peel-and-stick bone adhesive tape, characterized in that, The preparation steps are as follows: The PTC@ZS adhesive obtained by any of the preparation methods described in claims 1-4 is cut into equal portions of uniform size using a laser cutting machine. Polyethylene is selected as the release paper, and the adhesive is covered on the polyethylene film. The film is then dried in an oven for 30-60 minutes at a drying temperature of 35-50°C to bond the adhesive with the release paper and obtain the tape.
Citation Information
Patent Citations
Nano bone adhesive and preparation method thereof
CN113456881A
Organic-inorganic hybrid hydrogel bone adhesive and preparation method thereof
CN113577371A
Polylysine-based antibacterial medical bone tissue adhesive as well as preparation method and application thereof
CN116350833A
A polylysine-based antibacterial medical bone tissue adhesive and its preparation method and application
CN116350833B
Fast-curing and degradable strong bone adhesive and preparation method thereof
CN116407668A