A method for preparing ferrochromium electrolyte by leaching carbon ferrochrome from ferric chloride

Through the method of leaching carbon ferrochromium chromium leaching solution by ferrochromium leaching solution in the prior art, the low-cost production of high-purity iron chromium electrolyte is achieved, and safety hazards in the acid dissolution process are avoided. and high cost issues.

CN118099495BActive Publication Date: 2024-10-253R ENVIRONMENTAL TECH CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202311274737.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-28
Publication Date
2024-10-25
Estimated Expiration
2043-09-28

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove impurities in carbon ferrochromium leaching liquid, which makes it difficult for the purity of the iron-chromium electrolyte to meet the requirements of industrial application, and the acid dissolution process has safety hazards and high costs.

Method used

The method of ferric chloride leaching carbon ferrochromium is used to remove impurities through filtration, dilution, iron removal and evaporation and concentration, and a high-purity iron-chromium electrolyte is used to avoid hydrogen and harmful substances generated during acid dissolution. .

Benefits of technology

实现了低成本、高效地去除碳素铬铁中的杂质,获得高纯度铁铬电解液,降低了原料成本和生产风险,适合大规模工业应用。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118099495B_ABST
    Figure CN118099495B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of electrolyte production, and in particular to a method for preparing an iron-chromium electrolyte by leaching carbon ferrochrome from ferric chloride. The method comprises S1. adding a ferric chloride solution to carbon ferrochrome, heating and dissolving, and obtaining a ferrochrome solution; S2. adding iron powder to the ferrochrome solution, so that the chromium chloride in the ferrochrome solution is precipitated into chromium hydroxide; S3. beating after dilution, removing excess iron powder in the solid-liquid mixture with an iron remover, solid-liquid separation, chromium mud water washing and filter pressing, and dissolving the chromium mud with hydrochloric acid to obtain chromium chloride crystals; adding elemental iron to the first ferrous chloride solution for impurity removal, evaporating and concentrating the second ferrous chloride solution, cooling and crystallizing, and obtaining ferrous chloride crystals; S4. mixing chromium chloride crystals, ferrous chloride crystals, hydrochloric acid and water in proportion, and compounding them into an iron-chromium electrolyte. The method uses carbon ferrochrome as a raw material, and obtains an iron-chromium electrolyte product with low impurities without introducing impurities, and has the advantage of low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrolyte production, and in particular to a method for preparing ferrochromium electrolyte by leaching carbon ferrochrome with ferric chloride. Background Art

[0002] Due to the rapid development of renewable energy such as wind power and solar energy, it is urgent to develop large-scale energy storage systems to achieve the effective storage and utilization of such renewable energy with intermittent and unstable output characteristics. Iron-chromium redox flow battery is the earliest proposed and commercially applied flow battery. It has significant advantages such as independent system energy and power, low material cost, easy expansion, high safety, fast response speed, long cycle life, and high energy efficiency. It is a large-scale energy storage product with great potential.

[0003] As a carrier of active substances in iron-chromium redox flow batteries, electrolyte plays a vital role in the performance of batteries. In 1974, NASA proposed using ferrous chloride and chromic chloride dissolved in hydrochloric acid as positive and negative electrolytes, respectively. In order to continuously improve the electrochemical performance of batteries, the electrolyte of iron-chromium flow batteries has been developed into Fe 3+ / Fe 2+ and Cr 3+ / Cr 2+ They are used as positive and negative electrodes respectively and are redox coupled in a mixed electrolyte of hydrochloric acid solution to achieve discharge and charge. At present, the key material of the basic electrolyte of iron-chromium flow battery is a mixed solution of chromium chloride, ferrous chloride and hydrogen chloride.

[0004] With the development of iron-chromium redox flow batteries, people have tried to find widely available and inexpensive chromium-containing and iron-containing raw materials to prepare iron-chromium redox flow battery electrolytes, such as Chinese patents CN 112234238 B, CN 115832378A, CN 115832379 A, ​​and CN115842148A. Among them, carbon ferrochrome contains ferrochrome and is cheap, but the impurity content of carbon ferrochrome is high. In the prior art, acid is used to dissolve carbon ferrochrome, and then the leaching solution is removed. Since a large amount of hydrogen will be generated during the acid dissolution process, there are safety hazards during industrial production. In Chinese patent CN115832379A, a non-oxidizing gas including any one or a combination of at least two of nitrogen, argon or helium is added to dilute the hydrogen generated during the acid dissolution process to within the lower explosion limit. This method is costly.

[0005] Chinese patent CN115832379A discloses that materials containing iron metal and chromium metal are added to an acidic solution and mixed, and then solid-liquid separation is performed to obtain a leachate, and an impurity remover is selected for the leachate to adsorb impurities or generate insoluble solids to remove them, thereby obtaining a purified electrolyte. Most of the impurity removers selected in this patent are soluble in water, and the impurity removers are mixtures. A large amount of impurities are introduced during impurity removal, and each metal impurity can only be removed to within 50 mg / L. For some impurities with strict requirements, such as copper and nickel that are easy to cause hydrogen evolution at the negative electrode, when the requirement is <10 mg / L, this technical means cannot meet the purity requirements of the iron-chromium electrolyte.

[0006] Chinese patent CN113564680B discloses a method for purifying an iron-chromium electrolyte and the iron-chromium electrolyte obtained thereby. The patent mentions that the electrolyte is purified by electrolysis, but the patent can only be used to purify high-purity electrolytes. For example, the patent records that "in the present invention, To be purified In the iron-chromium electrolyte, the total concentration of impurity metal ions is below 20 ppm, preferably below 10 ppm, more preferably below 5 ppm, even more preferably below 3 ppm, and most preferably around 1 ppm". However, an iron-chromium electrolyte with a total impurity ion concentration of less than 20 ppm is difficult to obtain in the prior art. Therefore, the patented technology requires such a high purity for the raw electrolyte, which obviously limits the industrial application of the technical solution.

[0007] In addition, the prior art also removes impurities from carbon ferrochrome through a chromium salt production process, but the chromium salt production process involves hexavalent chromium, which is a highly toxic substance and cannot be used to purify carbon ferrochrome in an environmentally friendly manner. In fact, there is no method in the prior art to efficiently remove impurities from carbon ferrochrome leachate and obtain an electrolyte that meets the requirements, and there is a lack of a method for producing a high-purity ferrochrome electrolyte at a low cost. Summary of the invention

[0008] One of the purposes of the present invention is to provide a method for preparing an iron-chromium electrolyte by leaching carbon ferrochrome with ferric chloride. The method uses carbon ferrochrome as a raw material and uses ferric chloride for leaching, thereby avoiding the problem of a large amount of hydrogen caused by acid leaching, and obtaining an iron-chromium electrolyte product with a low impurity content without introducing impurities, and has the advantage of low cost.

[0009] To achieve one of the above purposes, the present invention provides the following technical solutions:

[0010] Provided is a method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride, comprising the following steps:

[0011] S1. The ferric chloride solution is added to the carbon ferrochrome to dissolve the carbon ferrochrome, and then filtered to separate to obtain a ferrochrome solution containing chromium chloride and ferrous chloride;

[0012] S2. adding iron powder to the ferrochrome solution to generate chromium hydroxide from the chromium chloride in the ferrochrome solution and precipitate to obtain a solid-liquid mixture;

[0013] S3. After dilution, under stirring, removing excess iron powder in the solid-liquid mixture with an iron remover, followed by solid-liquid separation to obtain a first ferrous chloride solution and solid chromium hydroxide;

[0014] The solid chromium hydroxide is washed with water, then dissolved in hydrochloric acid to obtain a chromium chloride solution, and the chromium chloride solution is sequentially evaporated and concentrated, cooled and crystallized to obtain chromium chloride crystals;

[0015] adding elemental iron to the first ferrous chloride solution to remove impurities, followed by solid-liquid separation to obtain a second ferrous chloride solution, and evaporating and concentrating the second ferrous chloride solution, cooling and crystallizing to obtain ferrous chloride crystals;

[0016] S4. Mix the chromium chloride crystals, the ferrous chloride crystals, hydrochloric acid and water in proportion to prepare an iron-chromium electrolyte.

[0017] The working principle of the above method for preparing ferrochromium electrolyte by leaching carbon ferrochromium with ferric chloride is as follows:

[0018] The iron and chromium in carbon ferrochrome are mainly elemental iron and elemental chromium. Ferric chloride can undergo redox reaction with elemental iron and elemental chromium to generate ferrous chloride and chromium chloride respectively. The leaching solution is a solution of chromium chloride and ferrous chloride, which is called ferrochrome solution. Iron powder is used as an acid-consuming agent to hydrolyze all chromium chloride to form chromium hydroxide precipitation, and obtain a solid-liquid mixture of chromium hydroxide and ferrous chloride solution. This solid-liquid mixture also contains a small amount of excess iron powder. Since the iron powder contains a large amount of impurities, it is not conducive to purification. The iron powder is magnetic and can be removed by an iron remover. The solid-liquid mixture after iron removal is solid-liquid separated to obtain chromium hydroxide and the first ferrous chloride solution. After separation, it is convenient to remove impurities from chromium chloride and ferrous chloride separately in the subsequent process. The chromium hydroxide is washed online with water by a filter press to remove free impurities, and solid-liquid separation is performed to obtain purified chromium hydroxide. The chromium hydroxide is dissolved in hydrochloric acid to obtain a chromium chloride solution. The chromium chloride solution is evaporated and concentrated, cooled and crystallized to obtain purified chromium chloride crystals. The first ferrous chloride solution is added with elemental iron to replace the impurities such as copper, nickel, and cobalt in the first ferrous chloride solution, and the solid-liquid separation is performed to obtain a ferrous chloride solution with impurities removed. This solution is evaporated, concentrated, cooled, and crystallized to obtain ferrous chloride crystals with less impurities. Finally, the chromium chloride crystals, ferrous chloride crystals, hydrochloric acid, and water after impurities removal are mixed in proportion to obtain an iron-chromium electrolyte.

[0019] In some embodiments, in step S1, after adding the ferric chloride solution to the carbon ferrochrome, the temperature is raised to 80° C. to 100° C. to dissolve the carbon ferrochrome.

[0020] At room temperature, carbon ferrochrome is almost insoluble in ferric chloride, but at a temperature of 80℃~100℃, ferric chloride can dissolve carbon ferrochrome better and improve the dissolution efficiency of carbon ferrochrome.

[0021] In some embodiments, in step S1, the time for dissolving carbon ferrochrome is 10 to 60 minutes, until the Fe in the ferric chloride solution is 3+ <0.05%.

[0022] The concentration of trivalent iron ions in the leaching solution is used to determine whether the reaction is complete. 3+ <0.05% indicates that ferric chloride has fully reacted with carbon ferrochrome to produce corresponding chromium chloride and ferrous chloride.

[0023] In some embodiments, in step S2, before adding the iron powder, the ferrochrome solution is diluted to a chromium concentration of 1-2%.

[0024] The chromium concentration in the ferrochrome solution is relatively high, and it needs to be diluted before adding iron powder to prepare chromium hydroxide. Otherwise, the chromium chloride cannot be completely precipitated, and the resulting chromium mud (chromium hydroxide) cannot be filtered and washed. Taking into account that the ferrous chloride after solid-liquid separation should be kept at a relatively high concentration, the ferrochrome solution is diluted to a chromium concentration of 1-2%. The diluent used to dilute the ferrochrome solution can be tap water, preferably a ferrous chloride solution. Ferrous chloride solution is an electrolyte component, and the use of ferrous chloride solution as a diluent can increase the concentration of the first ferrous chloride solution and reduce the load of subsequent ferrous chloride evaporation and concentration; the preferred chromium concentration in the diluted solution is 1.5%.

[0025] In some embodiments, in step S2, after the reduced iron powder is added, the temperature is raised to 80-90° C. to convert the chromium chloride in the ferrochrome solution into chromium hydroxide.

[0026] After heating, the reduced iron powder can react with the ferrochrome solution faster to generate chromium hydroxide.

[0027] In some embodiments, in step S2, the amount of iron powder added is 1.1 to 1.3 times the theoretical amount. When the amount of iron powder is small, the chromium chloride precipitation is incomplete, and when the amount of iron powder is too much, the burden of subsequent iron removal by the iron remover is increased, and the chromium loss is also increased.

[0028] In some embodiments, in step S2, after adding iron powder, the pH of the ferrochrome solution is measured. When the pH is 2.3-3.0, the chromium concentration in the solution is lower than 50 mg / L, indicating that chromium chloride has completely formed chromium hydroxide precipitate, which is convenient for monitoring chromium recovery and improves the chromium recovery rate.

[0029] In some embodiments, in step S3, tap water or dilute acid water or ferrous chloride solution with a mass of 0.5 to 2 times of the solution is added to dilute the solid-liquid mixture of step S2 and slurry it to form a thinner slurry, thereby reducing the iron powder contained in the chromium mud, facilitating iron removal by the iron remover, and reducing the loss of chromium mud during the iron removal process.

[0030] In some embodiments, in step S3, the magnetic force of the iron remover is greater than 12000 Gs. If the magnetic force is too small, it is not enough to completely remove the iron powder with a small particle size by magnetic attraction. The iron removal step must be performed before the solid-liquid separation of the chromium hydroxide and ferrous chloride solution. If the iron remover is used to remove the iron after the solid-liquid separation, since the chromium hydroxide is in the form of flocculent and viscous mud, there will still be clumped chromium mud containing iron powder when the diluent is added for pulping after pressure filtration, resulting in the iron powder not being completely removed, affecting the purity of the chromium mud.

[0031] In some embodiments, in step S3, the solid chromium hydroxide is washed online with water using a filter press; and the amount of hydrochloric acid used to dissolve the solid chromium hydroxide is 1.1 to 1.5 times the theoretical amount of hydrochloric acid.

[0032] In some embodiments, in step S3, the chromium chloride solution is concentrated to a sum of iron and chromium concentrations of 15.5% to 16.5%.

[0033] In some embodiments, in step S3, the cooling crystallization temperature of the chromium chloride solution is 20°C to 35°C.

[0034] In some embodiments, in step S3, the mass of the elemental iron is 2% to 10% of the mass of the solution.

[0035] The method for preparing ferrochromium electrolyte by leaching carbon ferrochrome from ferric chloride of the present invention has the following beneficial effects:

[0036] (1) The present invention uses carbon ferrochrome as the source of chromium and iron. Carbon ferrochrome is priced only by the chromium content, and the iron is equivalent to a gift. The price of 100% chromium is about 25,000 yuan / ton, while chromium chloride is about 68,000 yuan / ton, which greatly reduces the cost of raw materials.

[0037] (2) The use of ferric chloride to leach carbon ferrochrome avoids the generation of large amounts of hydrogen during acid leaching, thus eliminating potential safety hazards in industrial production.

[0038] (3) Use an iron remover to remove excess iron powder. Most of the solid impurities in the chrome mud can be removed using only physical methods. The removal effect is significant and the cost is low.

[0039] (4) The entire production process does not use traditional chromium salt purification technology, does not involve hexavalent chromium, and does not produce any harmful substances. It is green and environmentally friendly, in line with the general trend of technological improvement. In addition, the entire purification process does not introduce impurities, ensuring the purity of the electrolyte.

[0040] (5) The present invention has low requirements on the purity of raw materials. Even raw materials with high impurities can be well purified. It is suitable for large-scale production and has a wide range of applications.

[0041] (6) Iron-chromium electrolyte can be produced by using only one cheap raw material containing iron and chromium. There is no need to completely separate iron and chromium and then purify them separately. No toxic substances are used for impurity removal, and the purification cost is low.

[0042] To achieve the second objective above, the present invention provides the following technical solutions:

[0043] Provided is an electrolyte, the electrolyte containing an iron-chromium electrolyte, the iron-chromium electrolyte being prepared by the above-mentioned method for preparing an iron-chromium electrolyte by leaching carbon ferrochrome with ferric chloride.

[0044] To achieve the third objective above, the present invention provides the following technical solutions:

[0045] Provided is an iron-chromium redox flow battery containing the above-mentioned electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is the classification standard for carbon ferrochrome in GB / T 5683-2008 Ferrochrome. DETAILED DESCRIPTION

[0047] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0048] The terminology used in the present invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the present invention.

[0049] Example 1

[0050] This embodiment discloses a method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride, comprising the following steps:

[0051] S1. The ferric chloride solution is added to the carbon ferrochrome to dissolve the carbon ferrochrome, and then filtered to separate the resulting liquid as a ferrochrome solution containing chromium chloride and ferrous chloride;

[0052] Since carbon ferrochrome is almost insoluble in ferric chloride at room temperature, it is preferred to dissolve carbon ferrochrome at a temperature of 80°C to 100°C. This temperature allows ferric chloride to dissolve carbon ferrochrome better, thereby improving the dissolution efficiency of carbon ferrochrome.

[0053] The time for dissolving carbon ferrochrome is 30 minutes, until the Fe 3+ <0.05%. The concentration of trivalent iron ions in the leaching solution is used to determine whether the carbon ferrochrome has reacted completely to generate the corresponding chromium chloride and ferrous chloride.

[0054] S2. iron powder is added to the ferrochrome solution to generate chromium hydroxide in the ferrochrome solution and precipitate out, the solid-liquid mixture containing ferrous chloride solution and solid chromium hydroxide;

[0055] Before adding the iron powder, the ferrochrome solution is diluted to a chromium concentration of 1%, preferably 1.5%.

[0056] The chromium concentration in the ferrochrome solution is relatively high, and it needs to be diluted before forming chromium hydroxide. Otherwise, the chromium chloride cannot be completely formed into chromium hydroxide, and the resulting chromium mud (chromium hydroxide) cannot be filtered and washed. Therefore, the ferrochrome solution is diluted to a chromium concentration of 1%. The diluent used to dilute the ferrochrome solution can be tap water, preferably a ferrous chloride solution. Using a ferrous chloride solution as a diluent can increase the concentration of the first ferrous chloride solution and reduce the load of subsequent ferrous chloride evaporation and concentration; the preferred chromium concentration in the diluted solution is 1.5%.

[0057] After adding the reduced iron powder, the temperature is raised to 80° C., so that the chromium chloride in the ferrochrome solution is converted into chromium hydroxide. After the temperature is raised, the reduced iron powder can accelerate the reaction with the ferrochrome solution to generate chromium hydroxide.

[0058] The amount of iron powder added is 1.1 times the theoretical amount of iron powder added. Here, the amount of iron powder added is reduced as much as possible to avoid introducing iron powder impurities. The amount of iron powder added is 1.1-1.3 times the theoretical amount of iron powder added, which can ensure that the iron powder completely replaces chromium chloride with chromium hydroxide and reduce the loss of chromium mud when removing iron powder.

[0059] After adding iron powder, the pH of the ferrochrome solution is measured. When the pH is 2.3, it indicates that the chromium chloride has reached the end point of the reaction. After the chromium chloride generates chromium hydroxide, the chromium ions in the solution decrease. When the pH is 2.3, the chromium concentration in the solution is lower than 50 mg / L, indicating that the chromium chloride reaction is complete, which is convenient for monitoring the chromium recovery and improving the chromium recovery rate.

[0060] S3. Add 0.5 times water to dilute the solid-liquid mixture, and under stirring, remove the iron powder in the solid-liquid mixture with an iron remover until there is no iron powder in the chrome mud, and then separate the solid and liquid, preferably by means of a filter press, to obtain a first ferrous chloride solution and a solid chromium hydroxide;

[0061] The magnetic force of the iron remover is 12000Gs;

[0062] The solid chromium hydroxide is washed online with water by a filter press to remove most of the free impurities.

[0063] Solid chromium hydroxide is dissolved in hydrochloric acid to obtain a chromium chloride solution, and the chromium chloride solution is sequentially evaporated and concentrated, cooled and crystallized to obtain chromium chloride crystals with qualified impurities. The amount of hydrochloric acid used to dissolve the solid chromium hydroxide is 1.1 to 1.5 times the theoretical amount of hydrochloric acid. Excessive hydrochloric acid is conducive to the dissolution of chromium hydroxide and the subsequent crystallization of chromium chloride. Chromium chloride needs to be under a certain acidity to be easy to crystallize.

[0064] The chromium chloride solution is concentrated to a total concentration of 15.5% of iron and chromium. After the chromium chloride solution is concentrated, the crystallization operation can be better performed to improve the crystallization efficiency. The cooling crystallization temperature of the chromium chloride solution is 20°C.

[0065] Subsequently, elemental iron is added to part of the first ferrous chloride solution for impurity removal, wherein the mass of the elemental iron is 2% of the mass of the solution, and then solid-liquid separation is performed, and the solid-liquid separation method is a filter press method, so that excess elemental iron and the first ferrous chloride are separated, and then a second ferrous chloride solution can be obtained, and the second ferrous chloride solution is evaporated and concentrated, cooled and crystallized to obtain ferrous chloride crystals; considering that the amount of the second ferrous chloride required for the electrolyte is small, therefore, part of the first ferrous chloride is oxidized into a ferric chloride solution, and the ferric chloride solution is returned to dissolve carbon ferrochrome, so as to save ferric chloride.

[0066] S4. Mix the chromium chloride crystals, the ferrous chloride crystals, hydrochloric acid and water in proportion to prepare an iron-chromium electrolyte.

[0067] Example 2

[0068] This embodiment discloses a method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride, comprising the following steps:

[0069] S1. The ferric chloride solution is added to the carbon ferrochrome to dissolve the carbon ferrochrome, and then filtered to separate the resulting liquid as a ferrochrome solution containing chromium chloride and ferrous chloride;

[0070] Since carbon ferrochrome is almost insoluble in ferric chloride at room temperature, it is preferred to dissolve carbon ferrochrome at a temperature of 80°C. This temperature allows ferric chloride to dissolve carbon ferrochrome better, thereby improving the dissolution efficiency of carbon ferrochrome.

[0071] The time for dissolving carbon ferrochrome is 30 minutes, until the Fe 3+ <0.05%. The concentration of trivalent iron ions in the leaching solution is used to determine whether the carbon ferrochrome has reacted completely. The leaching solution is a mixed solution of chromium chloride and ferrous chloride.

[0072] S2. adding iron powder to the ferrochrome solution to reduce the chromium chloride in the ferrochrome solution to generate chromium hydroxide and precipitate the chromium hydroxide as chromium mud to obtain a solid-liquid mixture containing ferrous chloride and chromium hydroxide;

[0073] Before adding the iron powder, the ferrochrome solution is diluted to a chromium concentration of 1%.

[0074] The chromium concentration in the ferrochrome solution is relatively high, and it needs to be diluted before forming chromium hydroxide, otherwise the resulting chromium mud (chromium hydroxide) cannot be filtered and washed. Therefore, the ferrochrome solution is diluted to a chromium concentration of 1%, which is convenient for fully generating chromium mud and for washing the chromium mud. The diluent used to dilute the ferrochrome solution can be tap water, preferably ferrous chloride solution, which is an electrolyte component. Using ferrous chloride solution as a diluent can avoid the introduction of impurities; the preferred chromium concentration in the solution after dilution is 1.5%.

[0075] After adding the reduced iron powder, the temperature is raised to 80° C., so that the chromium chloride in the ferrochrome solution is converted into chromium hydroxide. After the temperature is raised, the reduced iron powder can react with the ferrochrome solution faster to generate chromium hydroxide.

[0076] The amount of iron powder added is 1.2 times the theoretical amount of iron powder added. Here, the amount of iron powder added is reduced as much as possible to avoid introducing iron powder impurities. Making the amount of iron powder added 1.2 times the theoretical amount of iron powder added can not only ensure that the iron powder completely replaces chromium chloride with chromium hydroxide, but also reduce the loss of chromium mud when removing iron powder.

[0077] After adding iron powder, the pH of the ferrochrome solution is measured. When the pH is 3.0, it indicates that the chromium chloride has reached the end point of the reaction. After the chromium chloride produces chromium hydroxide, the chromium ions in the solution decrease. When the pH is 3.0, it indicates that the chromium concentration in the solution is lower than 50 mg / L, indicating that the chromium chloride reaction is complete, which is conducive to monitoring the chromium recovery and improving the chromium recovery rate.

[0078] S3. Add 1 times pH ≈ 2.5 of dilute acid water to dilute the solid-liquid mixture, and under stirring, remove the iron powder in the solid-liquid mixture with an iron remover until there is no iron powder in the chrome mud, followed by solid-liquid separation, preferably by filter press to obtain a first ferrous chloride solution and solid chromium hydroxide;

[0079] The magnetic force of the iron remover is 14000Gs;

[0080] The solid chromium hydroxide is washed online with water by a filter press to remove most of the free impurities.

[0081] Solid chromium hydroxide is dissolved in hydrochloric acid to obtain a chromium chloride solution, and the chromium chloride solution is sequentially evaporated and concentrated, cooled and crystallized to obtain chromium chloride crystals with qualified impurities. The amount of hydrochloric acid used to dissolve the solid chromium hydroxide is 1.5 times the theoretical amount of hydrochloric acid. Excessive hydrochloric acid is conducive to the dissolution of chromium hydroxide and the subsequent crystallization of chromium chloride. Chromium chloride needs to be under a certain acidity to be easy to crystallize.

[0082] The chromium chloride solution is concentrated to a total concentration of 16.5% of iron and chromium, and the concentrated chromium chloride solution can be cooled and crystallized better, thereby improving the efficiency of cooling and crystallization. The cooling and crystallization temperature of the chromium chloride solution is 35°C.

[0083] Subsequently, elemental iron is added to the first ferrous chloride solution for reaction, wherein the mass of the elemental iron is 10% of the mass of the solution, and then solid-liquid separation is performed, and the solid-liquid separation method is a filter press method, so that excess elemental iron and the first ferrous chloride are separated, and then a second ferrous chloride solution can be obtained, and the second ferrous chloride solution is evaporated and concentrated, cooled and crystallized to obtain ferrous chloride crystals; considering that the amount of the second ferrous chloride required for the electrolyte is small, therefore, part of the second ferrous chloride is oxidized into a ferric chloride solution, and the ferric chloride solution is returned to dissolve carbon ferrochrome, thereby saving ferric chloride.

[0084] S4. Mixing the chromium chloride crystals with the ferrous chloride crystals, adding hydrochloric acid and water, and preparing an iron-chromium electrolyte.

[0085] Example 3

[0086] This embodiment discloses a method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride, comprising the following steps:

[0087] S1. The ferric chloride solution is added to the carbon ferrochrome to dissolve the carbon ferrochrome, and then filtered to separate the resulting liquid as a ferrochrome solution containing chromium chloride and ferrous chloride;

[0088] Since carbon ferrochrome is almost insoluble in ferric chloride at room temperature, it is preferred to dissolve carbon ferrochrome at a temperature of 90°C, at which temperature ferric chloride can better dissolve carbon ferrochrome and improve the dissolution efficiency of carbon ferrochrome.

[0089] The time for dissolving carbon ferrochrome is 20 minutes, until the Fe 3+ <0.05%. The concentration of trivalent iron ions in the leaching solution is used to determine whether the carbon ferrochrome has reacted completely to generate the corresponding chromium chloride and ferrous chloride.

[0090] S2. adding iron powder to the ferrochrome solution to reduce the chromium chloride in the ferrochrome solution to generate chromium hydroxide and precipitate the chromium hydroxide as chromium mud to obtain a solid-liquid mixture containing ferrous chloride and chromium hydroxide;

[0091] Before adding the iron powder, the ferrochrome solution is diluted to a chromium concentration of 1.5%.

[0092] The chromium concentration in the ferrochrome solution is relatively high, and it needs to be diluted before forming chromium hydroxide, otherwise, the resulting chromium mud (chromium hydroxide) cannot be filtered and washed. Therefore, the ferrochrome solution is diluted to a chromium concentration of 1.5%, which is convenient for fully generating chromium mud and for washing the chromium mud. The diluent used to dilute the ferrochrome solution can be tap water, preferably ferrous chloride solution, which is a component of the electrolyte. Using ferrous chloride solution as a diluent can avoid the introduction of impurities.

[0093] After adding the reduced iron powder, the temperature is raised to 85° C., so that the chromium chloride in the ferrochrome solution is converted into chromium hydroxide. After the temperature is raised, the reduced iron powder can react with the ferrochrome solution faster to generate chromium hydroxide.

[0094] The amount of iron powder added is 1.3 times the theoretical amount of iron powder added. Here, the amount of iron powder added is reduced as much as possible to avoid introducing iron powder impurities. Making the amount of iron powder added 1.3 times the theoretical amount of iron powder added can not only ensure that the iron powder completely replaces chromium chloride with chromium hydroxide, but also reduce the loss of chromium mud when removing iron powder.

[0095] After adding iron powder, the pH of the ferrochrome solution is measured. When the pH is 2.8, it indicates that the chromium chloride has reached the end point of the reaction. After the chromium chloride produces chromium hydroxide, the chromium ions in the solution decrease. When the pH is 2.8, it indicates that the chromium concentration in the solution is lower than 50 mg / L, indicating that the chromium chloride reaction is complete, which is conducive to monitoring the chromium recovery and improving the chromium recovery rate.

[0096] S3. Add 1.5 times the first ferrous chloride solution in Example 2 to dilute the solid-liquid mixture, and under stirring, remove the iron powder in the solid-liquid mixture with a deironing device until there is no iron powder in the chromium mud, and then separate the solid and liquid, preferably by means of a filter press, to obtain a first ferrous chloride solution and a solid chromium hydroxide;

[0097] The magnetic force of the iron remover is 16000Gs;

[0098] The solid chromium hydroxide is washed online with water by a filter press to remove most of the free impurities.

[0099] Solid chromium hydroxide is dissolved in hydrochloric acid to obtain a chromium chloride solution, and the chromium chloride solution is sequentially evaporated and concentrated, cooled and crystallized to obtain chromium chloride crystals with qualified impurities. The amount of hydrochloric acid used to dissolve the solid chromium hydroxide is 1.2 times the theoretical amount of hydrochloric acid. Excessive hydrochloric acid is conducive to the dissolution of chromium hydroxide and the subsequent crystallization of chromium chloride. Chromium chloride needs to be under a certain acidity to be easy to crystallize.

[0100] The chromium chloride solution is concentrated to a total concentration of 16% of iron and chromium, and the concentrated chromium chloride solution can be cooled and crystallized better, thereby improving the efficiency of cooling and crystallization. The cooling and crystallization temperature of the chromium chloride solution is 25°C.

[0101] Subsequently, elemental iron is added to the first ferrous chloride solution for reaction, wherein the mass of the elemental iron is 8% of the mass of the solution, and then solid-liquid separation is performed, and the solid-liquid separation method is a filter press method, so that excess elemental iron and the first ferrous chloride are separated, and then a second ferrous chloride solution can be obtained, and the second ferrous chloride solution is evaporated and concentrated, cooled and crystallized to obtain ferrous chloride crystals; considering that the amount of the second ferrous chloride required for the electrolyte is small, therefore, part of the second ferrous chloride is oxidized into a ferric chloride solution, and the ferric chloride solution is returned to dissolve carbon ferrochrome, thereby saving ferric chloride.

[0102] S4. Mixing the chromium chloride crystals with the ferrous chloride crystals, adding hydrochloric acid and water, and preparing an iron-chromium electrolyte.

[0103] Example 4

[0104] This embodiment discloses a method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride, comprising the following steps:

[0105] S1. The ferric chloride solution is added to the carbon ferrochrome to dissolve the carbon ferrochrome, and then filtered to separate the resulting liquid as a ferrochrome solution containing chromium chloride and ferrous chloride;

[0106] Since carbon ferrochrome is almost insoluble in ferric chloride at room temperature, it is preferred to dissolve carbon ferrochrome at a temperature of 90°C, at which temperature ferric chloride can better dissolve carbon ferrochrome and improve the dissolution efficiency of carbon ferrochrome.

[0107] The time for dissolving carbon ferrochrome is 15 minutes, until the Fe 3+ <0.05%. The concentration of trivalent iron ions in the leaching solution is used to determine whether the carbon ferrochrome has reacted completely to generate the corresponding chromium chloride and ferrous chloride.

[0108] S2. adding iron powder to the ferrochrome solution to reduce the chromium chloride in the ferrochrome solution to generate chromium hydroxide and precipitate the chromium hydroxide as chromium mud to obtain a solid-liquid mixture containing ferrous chloride and chromium hydroxide;

[0109] Before adding the iron powder, the ferrochrome solution was diluted to a chromium concentration of 1.8%.

[0110] The chromium concentration in the ferrochrome solution is relatively high, and it needs to be diluted before forming chromium hydroxide, otherwise, the resulting chromium mud (chromium hydroxide) cannot be filtered and washed. Therefore, the ferrochrome solution is diluted to a chromium concentration of 1.8%, which is convenient for fully generating chromium mud and for washing the chromium mud. The diluent used to dilute the ferrochrome solution can be tap water, preferably ferrous chloride solution, which is an electrolyte component. Using ferrous chloride solution as a diluent can avoid the introduction of impurities.

[0111] After adding the reduced iron powder, the temperature is raised to 83° C., so that the chromium chloride in the ferrochrome solution is converted into chromium hydroxide. After the temperature is raised, the reduced iron powder can react with the ferrochrome solution faster to generate chromium hydroxide.

[0112] The amount of iron powder added is 1.1 times the theoretical amount of iron powder added. Here, the amount of iron powder added is reduced as much as possible to avoid introducing iron powder impurities. Making the amount of iron powder added 1.1 times the theoretical amount of iron powder added can not only ensure that the iron powder completely replaces chromium chloride with chromium hydroxide, but also reduce the loss of chromium mud when removing iron powder.

[0113] After adding iron powder, the pH of the ferrochrome solution is measured. When the pH is 2.7, it indicates that the chromium chloride has reached the end point of the reaction. After the chromium chloride produces chromium hydroxide, the chromium ions in the solution decrease. When the pH is 2.7, it indicates that the chromium concentration in the solution is lower than 50 mg / L, indicating that the chromium chloride reaction is complete, which is conducive to monitoring the chromium recovery and improving the chromium recovery rate.

[0114] S3. Add 2 times the dilute acid water of pH ≈ 3.0 to dilute the solid-liquid mixture, and under stirring, remove the iron powder in the solid-liquid mixture with an iron remover until there is no iron powder in the chromium mud, followed by solid-liquid separation, preferably by means of a filter press, to obtain a first ferrous chloride solution and a solid chromium hydroxide;

[0115] The magnetic force of the iron remover is 18000Gs;

[0116] The solid chromium hydroxide is washed online with water by a filter press to remove most of the free impurities.

[0117] Solid chromium hydroxide is dissolved in hydrochloric acid to obtain a chromium chloride solution, and the chromium chloride solution is sequentially evaporated and concentrated, cooled and crystallized to obtain chromium chloride crystals with qualified impurities. The amount of hydrochloric acid used to dissolve the solid chromium hydroxide is 1.2 times the theoretical amount of hydrochloric acid. Excessive hydrochloric acid is conducive to the dissolution of chromium hydroxide and the subsequent crystallization of chromium chloride. Chromium chloride needs to be under a certain acidity to be easy to crystallize.

[0118] The chromium chloride solution is concentrated to a total concentration of 16.2% of iron and chromium, and the concentrated chromium chloride solution can be cooled and crystallized well, thereby improving the efficiency of cooling and crystallization. The cooling and crystallization temperature of the chromium chloride solution is 30°C.

[0119] Subsequently, elemental iron is added to the first ferrous chloride solution for reaction, wherein the mass of the elemental iron is 7% of the mass of the solution, and then solid-liquid separation is performed, and the solid-liquid separation method is a filter press method, so that excess elemental iron and the first ferrous chloride are separated, and then a second ferrous chloride solution can be obtained, and the second ferrous chloride solution is evaporated and concentrated, cooled and crystallized to obtain ferrous chloride crystals; considering that the amount of the second ferrous chloride required for the electrolyte is small, therefore, part of the second ferrous chloride is oxidized into a ferric chloride solution, and the ferric chloride solution is returned to dissolve carbon ferrochrome, thereby saving ferric chloride.

[0120] S4. Mixing the chromium chloride crystals with the ferrous chloride crystals, adding hydrochloric acid and water, and preparing an iron-chromium electrolyte.

[0121] Test example

[0122] In order to illustrate the quality of the iron-chromium electrolyte prepared by the present invention and the technical effects of the key technical means, a specific test example is used for description:

[0123] Test Example 1

[0124] This test example proposes a method for producing an electrolyte from carbon ferrochrome, comprising the following steps:

[0125] S1: adding 24.5 tons of ferric chloride solution to 1 ton of carbon ferrochrome, heating to above 80°C to dissolve the carbon ferrochrome, filtering and separating to obtain a mixed solution of 25.5 tons of chromium chloride and ferrous chloride, i.e., ferrochrome solution;

[0126] S2: Add 3.8 tons of water to dilute the ferrochrome solution to a chromium concentration of 2%, add 1.1 tons of reduced iron powder, and heat to 85°C to precipitate all the chromium chloride into chromium hydroxide (chromium mud for short);

[0127] S3: Add 15 tons of tap water, and use a magnetic force 12000Gs iron remover to remove a small amount of iron powder in the chrome mud under stirring until there is no iron powder in the chrome mud, and filter press to obtain chrome mud and ferrous chloride solution;

[0128] S4: The chromium mud is washed online with 14 tons of water using a filter press to remove most of the free impurities, and filtered to obtain washed chromium mud. The washed chromium mud is added with 4.5 tons of industrial hydrochloric acid and heated to 60°C to dissolve into chromium chloride solution;

[0129] S5: The chromium chloride solution is concentrated by evaporation to a total of 16.5% of iron and chromium, cooled to 30°C for 2 hours for crystallization, and centrifuged to obtain 1.8 tons of chromium chloride crystals with qualified impurities;

[0130] S6: add 0.13 tons of elemental iron to 4.2 tons of ferrous chloride solution in S3, stir and heat to 85°C, react for 2 hours, remove impurities such as copper and nickel in the solution, filter press to separate solid and liquid to obtain purified ferrous chloride solution, evaporate and concentrate to Fe=20%, cool to 20°C, crystallize for 1 hour, and centrifuge to obtain qualified ferrous chloride crystals;

[0131] S7: oxidizing the 20 tons of ferrous chloride solution in S3 to obtain ferric chloride, which is then reused in step S1 to continue dissolving carbon ferrochrome;

[0132] S8: The chromium chloride crystals and ferrous chloride crystals obtained in S5 and S6 are supplemented with appropriate amounts of hydrochloric acid and water to prepare the required iron-chromium electrolyte product.

[0133] Finally, the content of substances after impurities removal in each step is shown in Table 1.

[0134] Table 1 Product testing data for each step of Test Example 1

[0135] ;

[0136] The main components of carbon ferrochrome are chromium and iron, and also contain impurities such as Ca, Mg, Mn, Cu, and Ni. Cu and Ni easily lead to hydrogen evolution side reactions at the negative electrode, which affects the service life of the electrolyte. The Ca, Mg, Mn, Cu, and Ni in the iron-chromium electrolyte obtained in this test example 1 are all less than 40ppm, among which the key impurities Cu and Ni are less than 1.1ppm, and the total impurities are less than 60ppm, with high purity.

[0137] Test Example 2

[0138] This test example proposes a method for producing an electrolyte from carbon ferrochrome, comprising the following steps:

[0139] S1: Add 24.5 tons of ferric chloride solution into 2 tons of carbon ferrochrome, raise the temperature to above 70°C, dissolve the carbon ferrochrome, filter and separate, and obtain 25.5 tons of chromium chloride and ferrous chloride mixed solution (referred to as ferrochrome solution);

[0140] S2: adding 10 tons of ferrous chloride solution in step S3 of test example 1 to dilute the ferrochrome solution to a chromium concentration of 1.5%, adding 0.45 tons of reduced iron powder, and heating to 100° C. to precipitate all chromium chloride into chromium hydroxide (hereinafter referred to as chromium mud);

[0141] S3: Add 40 tons of ferrous chloride solution with pH>2.5, and remove a small amount of iron powder in the chrome mud with a magnetic force of 15000Gs under stirring until there is no iron powder in the chrome mud, and filter press to obtain chrome mud and ferrous chloride solution;

[0142] S4: During the filter press, the chromium mud is washed online with 7 tons of water to remove most of the free impurities, and then filtered to obtain washed chromium mud. The washed chromium mud is added with 4.5 tons of industrial hydrochloric acid and heated to 80°C to dissolve into chromium chloride solution;

[0143] S5: The chromium chloride solution is concentrated by evaporation to a total of 17% of iron and chromium, cooled to 20°C for crystallization for 2 hours, and centrifuged to obtain 1.5 tons of chromium chloride crystals with qualified impurities;

[0144] S6: add 0.4 ton of elemental iron to 8.5 ton of ferrous chloride solution in S3, stir and heat to 100°C, react for 0.5h, remove impurities such as copper and nickel in the solution, filter press to separate solid and liquid to obtain purified ferrous chloride solution, evaporate and concentrate to Fe=20.3%, cool to 30°C for crystallization for 0.5h, and centrifuge to obtain ferrous chloride crystals;

[0145] S7: Add water to the ferrous chloride crystals obtained in S6 until Fe=20.5%, raise the temperature to 50~70℃, wait for the crystals to completely dissolve, cool to 20~25℃ for crystallization, centrifuge for solid-liquid separation, and obtain recrystallized ferrous chloride crystals.

[0146] S8: oxidizing the 22 tons of ferrous chloride solution in S3 to obtain ferric chloride, which is then reused in step S1 to continue dissolving carbon ferrochrome;

[0147] S9: The chromium chloride crystals and ferrous chloride crystals obtained in S5 and S7 are supplemented with appropriate amounts of hydrochloric acid and water to prepare the required iron-chromium electrolyte product.

[0148] Finally, the content of substances after impurities removal in each step is shown in Table 2.

[0149] Table 2 Product testing data for each step of Test Example 2

[0150] ;

[0151] The main components of carbon ferrochrome are chromium and iron, and also contain soluble impurities such as Ca, Mg, Mn, Cu, and Ni. Cu, Ni, etc. easily cause hydrogen evolution side reaction at the negative electrode, affecting the service life of the electrolyte. The impurities of Ca, Mg, Mn, Cu, and Ni in the iron-chromium electrolyte obtained by this test example 2 are all lower than 13ppm, among which the key impurities Cu and Ni are lower than 2ppm, and the total impurities are lower than 30ppm, and the purity is relatively high. By recrystallization of ferrous chloride, impurities in the electrolyte, especially the manganese content, can be significantly reduced.

[0152] Comparative Test Example 3

[0153] Take 1.5 kg of the mixed solution of chromium hydroxide and ferrous chloride obtained in step S2 of Test Example 2, 500 g per portion, and conduct the following three groups of comparative tests respectively:

[0154] ① Take 500 g of the mixed solution, add 1500 g of water, stir at 1000 r / min for 10 min, and obtain about 150 g of chromium mud 1 after solid-liquid separation by suction filtration;

[0155] ② Take 500 g of the mixed solution and separate it by suction filtration to obtain about 170 g of chromium mud 2 and about 330 g of ferrous chloride solution. Mix all the chromium mud 2 and the ferrous chloride solution, add 1500 g of water and stir at 1000 r / min for 10 min, remove iron with a 12000 Gs iron remover, and obtain about 144 g of chromium mud 3 after solid-liquid separation by suction filtration;

[0156] ③ Take 500 g of the mixed solution, add 1500 g of water and stir at 1000 r / min for 10 min. Use a 12000 Gs iron remover to remove iron. After solid-liquid separation by suction filtration, about 140 g of chromium mud 4 is obtained.

[0157] The chromium mud test data obtained from the three groups of tests are shown in Table 3:

[0158] Table 3 Detection data of chrome mud obtained in comparative test example 3

[0159] ;

[0160] From the data in Table 3, we can see that:

[0161] (1) From the comparison between tests ① and ③, it can be seen that after the slurry was diluted and washed with the same amount of water, the iron content and impurity content in the chrome sludge 1 obtained in test ① were higher, mainly because there was still unreacted iron powder in the chrome sludge 1. In test ③, the impurity content in the chrome sludge 3 obtained after the iron powder was removed by the iron remover during water washing was significantly reduced, and the iron remover had a significant impurity removal effect.

[0162] (2) From the comparison between Experiment ② and Experiment ③, it can be seen that since the filtrate ferrous chloride contains impurities, in order to ensure the consistency of free impurities in the chromium mud, after the filtration of Experiment ②, all the chromium mud and the filtrate are mixed again. After the same amount of water beating, washing, and iron removal by the iron remover, the impurities in chromium mud 2 are higher than those in chromium mud 3, indicating that the iron remover of Experiment ③ has a good effect. The reason for the analysis is that after the chromium mud slurry is filtered, since the chromium mud (chromium hydroxide) is an amorphous non-crystalline state and a relatively viscous paste-like solid, it is difficult to break up the chromium mud into slurry after the filter press. In the experiment, it is always found that there is still some clumped chromium mud. It is difficult to break up all the chromium mud after adjusting the type of stirring paddle, stirring speed, water volume, container size, etc. The clumped chromium mud also contains iron powder, which is difficult to be removed by the iron remover, resulting in a high impurity content in the final chromium mud.

[0163] Experimental summary:

[0164] (1) The iron remover can effectively remove impurities introduced into the iron powder;

[0165] (2) Iron removal by an iron remover should be carried out in the solution generated by chromium hydroxide and before solid-liquid separation. The effect of iron removal after chromium mud filter pressing is poor.

[0166] Comparative Test Example 4

[0167] (1) Take 2.5 kg of the mixed solution of chromium hydroxide and ferrous chloride obtained in step S2 of Test Example 2, 500 g per portion, and conduct the following five groups of comparative tests respectively:

[0168] ④ After removing iron from 500g of the mixed solution with a 12000Gs iron remover, filter it, detect the weight and chromium content of the chromium mud 4, and calculate the chromium recovery rate and loss rate;

[0169] ⑤ Add 0.5 times tap water to 500g of the mixed solution, beat for 10min, remove iron with a 12000Gs iron remover, filter, detect the weight and chromium content of the chromium mud, and calculate the chromium recovery rate and loss rate;

[0170] The difference between test ⑥ and test ⑤ is that 1 times of tap water is added;

[0171] The difference between test ⑦ and test ⑤ is that 1.5 times of tap water is added;

[0172] The difference between test ⑧ and test ⑤ is that 2 times of tap water is added.

[0173] (2) Add 1000g of 1% Cr-iron solution to 1.2 times the amount of iron powder and heat to 100°C to allow all the chromium chloride to precipitate as chromium hydroxide (chrome mud).

[0174] In test ⑨, 500 g of the solid-liquid mixture in (2) was removed by a 12000 Gs iron remover, and then filtered to detect the weight and chromium content of the chromium mud 9, and the chromium recovery rate and loss rate were calculated.

[0175] The difference between test ⑩ and test ⑨ is that 500 g of solid-liquid mixture is added to 500 g of water and slurried for 10 min before iron removal by an iron remover.

[0176] The experimental data of the 7 groups of experiments are shown in Table 4.

[0177] Table 4 Comparative test example 4 chromium mud detection data table

[0178] ;

[0179] Analysis of the test data in Table 4:

[0180] (1) The mixed solution of chromium hydroxide and ferrous chloride obtained by precipitating chromium from a solution containing 1.5% chromium has a high chromium loss rate when the iron is removed by the iron remover. The reason for this is that chromium hydroxide (chromium mud) is amorphous and non-crystalline, and is a flocculent precipitate. It is easy to enclose iron powder in it during precipitation. When the iron is removed by the iron remover, the chromium mud on the surface of the iron powder is removed together, resulting in a high chromium loss rate.

[0181] (2) After adding solution for dilution, the slurry is then beaten to remove the chromium mud adhering to the surface of the iron powder, and the chromium loss rate drops rapidly. When 1.5 times the amount of water is added, the chromium mud loss rate is close to the minimum. When the amount of water for beating is increased, the chromium loss rate does not change significantly. At this time, the chromium in the slurry = 1%.

[0182] (3) Even if the chromium concentration in the ferrochrome solution is diluted to a lower level, the mixed solution still needs to be diluted with solution and then slurried to make the chromium mud attached to the surface of the iron powder fall off. The reason for this is that chromium hydroxide is a monomer when it is generated. As time goes by and the solution changes, it will aggregate into large-particle polymers. The molecular weight of the polymer is closely related to the chromium concentration in the solution. When the chromium concentration in the solution is high, the molecular weight of the polymer is small, and when the chromium concentration is low, the molecular weight of the polymer is large. The experiment found that regardless of the chromium concentration in the ferrochrome solution, after the chromium hydroxide precipitate is formed, the chromium hydroxide is evenly distributed in the entire solution, and the dilute ferrochrome solution does not show chromium mud precipitation and stratification. When the flocculent monomers polymerize, they will inevitably wrap the solution and iron powder. When chromium chloride completely forms chromium hydroxide precipitate, the shape of chromium hydroxide in the solution is fixed. When the solution is added to dilute the chromium hydroxide, the balance in the original solution can be broken, and stirring is given. The polymerized chromium hydroxide is formed into small molecules through shear force, thereby releasing the wrapped solution and iron powder, causing the chromium hydroxide attached to the surface of the iron powder to fall off.

[0183] Experimental summary:

[0184] The mixed solution of chromium hydroxide and chromium chloride must be diluted and slurried before using an iron remover to remove iron powder, which can effectively reduce the loss rate of chromium.

[0185] Test Example 5

[0186] From the attached Figure 1 According to GB / T 5683-2008 Ferrochrome, carbon ferrochrome is divided into four specifications according to the carbon content: high carbon ferrochrome, medium carbon ferrochrome, low carbon ferrochrome, and micro carbon ferrochrome. The smelting process of high carbon ferrochrome is: chromite is added with coke as a reducing agent to reduce chromium and iron to obtain high carbon ferrochrome; medium, low and micro carbon ferrochrome use high carbon ferrochrome as raw material, add chromite to decarbonize high carbon ferrochrome, and obtain different products according to the degree of decarbonization. The index requirements for Si, P and S in carbon ferrochrome are similar, and there are no requirements for other impurities.

[0187] In the prior art, acid is used to dissolve high carbon ferrochrome, and chromium and iron products are extracted after iron and chromium are separated. The acid dissolution process generally requires high temperature and high acidity conditions to improve the dissolution efficiency, and then produces a high temperature mixed gas with acid mist and H2, which has high anti-corrosion requirements for industrial production equipment and tail gas treatment systems. In addition, the amount of H2 is large, the explosion range is extremely wide, and it is easy to cause safety accidents, which is not conducive to the safety of operators and hinders the industrial application of technical solutions. However, there is no research report on the use of medium, low and micro carbon ferrochrome as chromium extraction raw materials. When the inventor screened different types of carbon ferrochrome as raw materials for iron-chromium electrolyte, he found that different carbon ferrochromes had very different acid solubility. He conducted experiments on dissolving carbon ferrochrome and metallic chromium at different hydrochloric acid concentrations and different temperatures, and investigated the changes in chromium dissolution rate and hydrogen concentration. The test data are shown in Table 5.

[0188] Table 5 Test data of hydrochloric acid dissolving carbon ferrochrome and metallic chromium

[0189] ;

[0190] According to the test data in Table 5, the following analysis is performed:

[0191] (1) Using equivalent hydrochloric acid, high carbon ferrochrome requires high temperature, high acid concentration, and long reaction time to completely leach chromium, while medium, low, and micro carbon ferrochrome can leach more than 95% of chromium using low concentration hydrochloric acid at room temperature and in a short time. The acid solubility of carbon ferrochrome varies greatly, and the essential reason is the different molecular structures. The existing literature such as "Solid Phase Microstructure and Crushing Performance of High Carbon Ferrochrome Alloy", "Microstructure of High Carbon Ferrochrome and Its Effect on Solid Phase Decarburization", "Basic Research on Co-reduction Smelting of High Carbon Ferrochrome by High Chromium Type Vanadium Extraction Tailings and Chromite", etc., reveal that the chromium in high carbon ferrochrome mainly exists in the form of chromium carbide, which is difficult to be completely dissolved by acid; for example, "CN 106244753 B New Method for Producing Medium Carbon Ferrochrome", "Research on the Use of CO2 in Oxygen Blowing Method for Producing Medium and Low Carbon Ferrochrome", and "Exploration of Low Carbon Ferrochrome Smelting Process" reveal that medium, low, and micro carbon ferrochrome undergo decarburization during production, and it can be reasonably inferred that the chromium form should be different from chromium carbide. The chromium leaching rates of low-carbon ferrochrome and metallic chromium, as well as the highest H2 concentration during the reaction are very close. It can be reasonably inferred that the chromium in low-carbon ferrochrome is elemental chromium, and further inferred that the chromium in medium- and low-carbon ferrochrome is also elemental chromium.

[0192] (2) The H2 concentration is always high during the dissolution of carbon ferrochrome with hydrochloric acid. During the industrial process, a large amount of inert gas must be added to dilute it to below the explosion limit. The H2 safety issue is difficult to resolve.

[0193] Test Example 6

[0194] In order to avoid the H2 problem generated during the leaching of carbon ferrochrome, it is necessary to find a + Ferric chloride can react with elemental iron. After consulting the data, the physical and chemical properties of elemental chromium and elemental iron are similar. It is speculated that ferric chloride can also react with elemental iron, that is, ferric chloride can dissolve medium, low and micro carbon ferrochrome. In order to verify this speculation, carbon ferrochrome was dissolved with equivalent ferric chloride, and the test results are shown in Table 6.

[0195] Table 6 Dissolution test of equivalent ferric chloride for carbon ferrochrome

[0196] ;

[0197] According to the test data in Table 6, we can know that:

[0198] (1) As the carbon content in carbon ferrochrome decreases, the chromium dissolution rate increases, that is, the elemental chromium content in the ferrochrome increases. High-carbon ferrochrome is difficult to dissolve with ferric chloride, while the dissolution rates of other types of carbon ferrochrome with equivalent ferric chloride are all greater than 90%.

[0199] (2) A small amount of hydrogen will be produced during the dissolution of carbon ferrochrome, which is mainly caused by a small amount of free acid in ferric chloride. When medium, low and micro carbon ferrochrome are dissolved with ferric chloride of the same acid concentration, the maximum concentration of hydrogen produced during the process is close. Hydrogen is mainly produced in the first 2 minutes of the dissolution process. When the reaction continues, the hydrogen concentration is lower than 0.005%. When the acid concentration in ferric chloride decreases, the maximum concentration of hydrogen in the reaction process drops rapidly. The maximum concentration of hydrogen can be kept below the lower explosion limit by controlling the acidity in ferric chloride.

[0200] (3) When low-carbon ferrochromium was dissolved with ferric chloride having an acid concentration of 0.2% and the reaction temperature was 70°C, no Fe was found during the dissolution process. 3+ Hydrolysis, and when the reaction temperature is 100℃, a small amount of Fe 3+ Hydrolysis resulted in a decrease in the chromium dissolution rate, while when the acidity of ferric chloride was increased to 0.3%, no Fe 3+ Hydrolysis, therefore, considering the utilization rate of ferric chloride, the dissolution rate of chromium and the maximum concentration of hydrogen during the reaction, the acidity of ferric chloride should be controlled between 0.2% and 0.3%.

[0201] Electrical performance test

[0202] The electrolytes obtained in Experimental Examples 1 and 2 and electrolytes with various impurity concentrations were subjected to electrical performance tests. The charge and discharge mode was set to constant current charge and discharge, and the current was 120 mA / cm 2 , the charge cut-off voltage is 1.2V, the discharge cut-off voltage is 0.3V, the charge and discharge times are 20 times, and the obtained data are shown in Table 7. In the iron-chromium electrolyte, Fe=1.2M, Cr=1.4M, and HCl=2.5M.

[0203] Table 7 Electrical performance test data record table of various impurity concentration electrolytes

[0204] ;

[0205] It can be seen from the data in Table 7 that the level of impurity concentration directly affects the energy efficiency and attenuation rate of the electrolyte when it is used, and the attenuation rate varies greatly. It is stipulated in the industry that when the discharge amount of the electrolyte drops to 60% of the initial amount, the electrolyte needs to be regenerated. After the carbon ferrochrome is leached and impurities are not removed, the attenuation rate is as high as 3.6%. The electrolyte can only be regenerated after 11 times of charge and discharge, and it cannot be applied in engineering; the impurities in the prior art CN115832379A product are still high, and the electrolyte can only be regenerated after 17 times of charge and discharge, and it cannot be applied in engineering; the electrolyte in Example 1 of this technical solution has a purity close to that of the analytical pure reagent configuration, and the energy efficiency and attenuation rate are also close. It can run stably for 167 times before the electrolyte needs to be regenerated, which greatly reduces the number of electrolyte regenerations and greatly improves the utilization rate of the electrolyte. The electrolyte produced by this technical solution has a cost much lower than that of the analytical pure reagent, and has the advantages of low cost and high purity.

[0206] Cost Analysis

[0207] The cost of the production method of compounding the electrolyte by purchasing finished products of chromium chloride and ferrous chloride is calculated based on Fe=1.2M, Cr=1.4M, and HCl=2.5M in the ferrochromium electrolyte. The data are shown in Table 8.

[0208] Table 8 Cost accounting table for purchasing finished chromium chloride and ferrous chloride composite electrolyte raw materials

[0209] ;

[0210] It can be seen from Table 8 that the raw material cost of purchasing finished compound electrolyte is close to 7,000 yuan / ton; when carbon ferrochrome is used as raw material, the raw material cost is about 1,400 yuan / ton, and the cost of dissolution and purification process is less than 2,000 yuan / ton. Under the premise of purification to the same purity, the electrolyte cost is reduced to less than 50% of the existing technology, with significant economic benefits, promotion significance, and in line with the trend of technological development.

[0211] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. It should be clear to those skilled in the art that any improvement of the present invention, the equivalent replacement of each raw material in the method of the present invention, the addition of auxiliary components, the selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention without departing from the principle of the present invention.

Claims

1. A method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride, characterized in that: The following steps are included: S1. adding a ferric chloride solution to the carbon ferrochrome, heating the temperature to 80°C to 100°C to dissolve the carbon ferrochrome, dissolving the carbon ferrochrome, and then filtering and separating to obtain a ferrochrome solution, wherein the ferrochrome solution contains chromium chloride and ferrous chloride; S2. adding iron powder to the ferrochrome solution to generate chromium hydroxide from chromium chloride in the ferrochrome solution and precipitate to obtain a solid-liquid mixture; S3. After diluting the solid-liquid mixture, removing the iron powder in the solid-liquid mixture with an iron remover, followed by solid-liquid separation to obtain a first ferrous chloride solution and solid chromium hydroxide; The solid chromium hydroxide is washed with water, and then dissolved in hydrochloric acid to obtain a chromium chloride solution, and the chromium chloride solution is sequentially evaporated and concentrated, and cooled and crystallized to obtain chromium chloride crystals; adding elemental iron to the first ferrous chloride solution to remove impurities, followed by solid-liquid separation to obtain a second ferrous chloride solution, evaporating and concentrating the second ferrous chloride solution, cooling and crystallizing to obtain ferrous chloride crystals; S4. Mix the chromium chloride crystals, the ferrous chloride crystals, hydrochloric acid and water in proportion to prepare an iron-chromium electrolyte.

2. The method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome from ferric chloride according to claim 1, characterized in that: In step S1, the free acid in ferric chloride is 0.2% to 0.3%.

3. The method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome from ferric chloride according to claim 1, characterized in that: In step S1, after the ferric chloride solution is added to the carbon ferrochrome, the carbon ferrochrome is dissolved for 10 to 60 minutes until the Fe 3+ <0.05%.

4. The method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome from ferric chloride according to claim 1, characterized in that: In step S2, before adding the iron powder, the ferrochrome solution is diluted to a chromium concentration of 1-2%; the amount of the iron powder added is 1.1-1.3 times the theoretical amount of the iron powder added; after adding the reduced iron powder, the temperature is raised to 80-100° C. to convert the chromium chloride in the ferrochrome solution into chromium hydroxide.

5. The method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride according to claim 1, characterized in that: In step S3, before the iron remover removes iron, a diluent must be added to dilute and slurry the solid-liquid mixture described in step S2. The diluent is tap water, dilute acid water, or ferrous chloride solution. The amount of the diluent is 0.5 to 2.0 times that of the solid-liquid mixture.

6. The method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride according to claim 1, characterized in that: In step S3, the magnetic force of the iron remover is greater than 12000 Gs.

7. The method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride according to claim 1, characterized in that: In step S3, the solid chromium hydroxide is washed online with water using a filter press; the amount of hydrochloric acid used to dissolve the solid chromium hydroxide is 1.1 to 1.5 times the theoretical amount of hydrochloric acid; The chromium chloride solution is concentrated to a sum of iron and chromium concentrations of 15.5% to 16.5%, and the cooling crystallization temperature of the chromium chloride solution is 20° C. to 35° C.; The mass of the elemental iron is 2% to 10% of the mass of the first ferrous chloride solution.

8. The method for preparing an iron-chromium electrolyte for leaching carbon ferrochrome with ferric chloride according to claim 1, characterized in that: The carbon ferrochrome is any one or more of medium carbon ferrochrome, low carbon ferrochrome and micro carbon ferrochrome.

9. An electrolyte, characterized in that: The electrolyte contains an iron-chromium electrolyte, and the iron-chromium electrolyte is prepared by the method for preparing an iron-chromium electrolyte by leaching carbon ferrochrome with ferric chloride as described in any one of claims 1 to 8.

10. An iron-chromium redox flow battery, characterized in that: Containing the electrolyte according to claim 9.

Citation Information

Cited By

  • Method for preparing iron-chromium electrolyte and electronic-grade ferrous chloride from stainless steel waste liquid

    CN119976983A

  • Preparation method of iron-chromium electrolyte and electronic-grade ferrous chloride

    CN121202199A

  • Process for the preparation of ferrochrome electrolyte and electronic grade ferrous chloride