A high-entropy cerate water-based paint and coating thereof for high-temperature radiation heat dissipation

By combining high-entropy cerate aqueous coatings and boron nitride and other materials, a coating with high infrared emissivity and thermal conductivity in the 1-20μm band is prepared, which solves the problem of the performance of existing high-temperature radiation heat dissipation materials in high-temperature environments. The best problem achieves more effective radiation heat dissipation and high temperature resistance.

CN118126547BActive Publication Date: 2024-12-03LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410279397.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-12
Publication Date
2024-12-03
Estimated Expiration
2044-03-12

AI Technical Summary

Technical Problem

The existing high-temperature radiation heat dissipation materials have poor performance in environments where the temperature exceeds 1000℃, especially the band range corresponding to infrared emissivity is narrow, which cannot effectively cope with the propagation of high-temperature radiation energy.

Method used

Using high-entropy cerate aqueous coatings, a coating with excellent infrared emissivity and thermal conductivity is prepared by combining high-entropy cerate, boron nitride, zirconia and other materials. The infrared emissivity of the coating is in the 1~20μm band. More than 0.93, thermal conductivity exceeds 60 W·(m·K)-1, combined with ball mill mixing process and composite high-temperature adhesive, enhance the directional thermal conductivity and toughness of the coating.

Benefits of technology

It significantly widens the infrared emission band, improves the radiation heat dissipation performance of the material at high temperatures, enhances the coating's high temperature, thermal shock and corrosion resistance, extends the service life of the hot end components, and improves the boiler heat exchange efficiency .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118126547B_ABST
    Figure CN118126547B_ABST
Patent Text Reader

Abstract

The present invention relates to a high-entropy cerate water-based paint for high-temperature radiation heat dissipation, and the water-based paint is composed of the following raw materials in parts by weight: 10-20 parts of high-entropy cerate, 5-10 parts of boron nitride, 5-10 parts of zirconium oxide, 0-5 parts of cordierite, 3-5 parts of silicon carbide, 3-5 parts of silicon nitride, 5-10 parts of brown corundum, 3-5 parts of fumed silica, 2-5 parts of kaolin, 1-3 parts of whiskers, 1-3 parts of defoamers, 1-3 parts of leveling agents, 1-3 parts of wetting and dispersing agents, 1-3 parts of organic bentonite, 20-30 parts of composite high-temperature binders, and 15-25 parts of deionized water; the chemical formula of the high-entropy cerate is A2Ce2O7, wherein the A position is at least five elements of La, Pr, Gd, Ca, Cu, Fe, Ni, and Co, and each element is in an equal molar ratio or a nearly equal molar ratio. At the same time, the present invention also discloses a coating made by using the water-based paint. The water-based paint of the present invention has high infrared emissivity, directional heat conduction, strong toughness and a thermal expansion coefficient matching that of the substrate in the 1-20 μm band. The prepared coating can be used as a protective energy-saving material in power station boilers and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-temperature radiation heat dissipation, and in particular to a high-entropy cerate water-based paint for high-temperature radiation heat dissipation and a coating thereof. Background Art

[0002] Infrared radiation is a technology that increases the infrared emissivity of the heat source surface to enhance heat exchange capacity. Due to its versatility and adjustability, it is widely used in the field of high-temperature heat dissipation.

[0003] CN 115710459A discloses a high temperature resistant heat dissipation powder coating and its preparation method. This invention adopts polyimide resin and polyester resin, and by improving the heat dissipation efficiency (high infrared radiation efficiency) of the surface of the object, the obtained powder coating has excellent impact resistance and heat dissipation performance, and can withstand up to 360°C. According to Planck's law and Wien's displacement law, it can be known that in a high temperature environment, radiant heat is dominant. When the use temperature is greater than 1000°C, 95% of the energy of the black body is transmitted in the form of radiant heat. Therefore, this material is not suitable for a high temperature environment of more than 800°C.

[0004] CN 115724658A discloses a high-temperature and high-radiance protective coating for coal-fired boilers and a preparation method thereof. The protective coating is composed of rare earth-doped spinel, functional fillers, high-temperature binders and additives, and has a normal infrared emissivity of 0.946 in the 2-15 μm band. It can withstand a high temperature of 1200°C, and provides a protective solution for solving the problems of contamination and coking, high-temperature corrosion, and wear resistance on the heating surfaces of power plant boilers and industrial kilns facing the fire side. However, the document does not mention the influence of thermal conductivity on material properties. However, as a radiation heat dissipation material, high thermal conductivity is also an important indicator.

[0005] CN 115975453A discloses a flaky rare earth-based high radiation heat dissipation coating and its preparation method and application. The obtained flaky rare earth-based high radiation heat dissipation coating has an emissivity of 0.97 in the 8~13m atmospheric window, and has a significant heat dissipation effect. CN116676003A discloses a colored radiation heat dissipation coating and its preparation method, which has excellent photothermal performance, an emissivity of 99% in the near-infrared band, a reflectivity of 89% in the full solar band, and an emissivity of 98% in the atmospheric window band, which can effectively improve the radiation heat dissipation effect. However, the infrared emissivity in these documents corresponds to a narrow band range, which is not suitable for use in environments with temperatures greater than 1000°C (temperatures above 1000°C, the corresponding bands of radiation energy are mainly concentrated in the 1~5μm range). Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a high-entropy cerate water-based coating with good high-temperature radiation heat dissipation performance.

[0007] Another technical problem to be solved by the present invention is to provide a coating prepared by the water-based paint.

[0008] In order to solve the above problems, the present invention discloses a high-entropy cerate water-based coating for high-temperature radiation heat dissipation, characterized in that the water-based coating is composed of the following raw materials in parts by weight: 10-20 parts of high-entropy cerate, 5-10 parts of boron nitride, 5-10 parts of zirconium oxide, 0-5 parts of cordierite, 3-5 parts of silicon carbide, 3-5 parts of silicon nitride, 5-10 parts of brown corundum, 3-5 parts of fumed silica, 2-5 parts of kaolin, 1-3 parts of whiskers, 1-3 parts of defoaming agent, 1-3 parts of leveling agent, 1-3 parts of wetting dispersant, 1-3 parts of organic bentonite, 20-30 parts of composite high-temperature binder, and 15-25 parts of deionized water; the chemical formula of the high-entropy cerate is A2Ce2O7, wherein the A position is at least five elements of La, Pr, Gd, Ca, Cu, Fe, Ni, and Co, and the elements are in an equal molar ratio or a nearly equal molar ratio.

[0009] The particle size of the high entropy cerate is less than 1 μm.

[0010] The particle sizes of the zirconium oxide and brown corundum are both 300-500 nm; the particle size of the boron nitride is 100-200 nm; and the particle size of the silicon nitride is 500-800 nm.

[0011] The boron nitride is hexagonal boron nitride with a layered crystal structure, and its theoretical thermal conductivity along the a, b and c axes is 4.1 W·(m·K) respectively. -1 and 537 W·(m·K) -1 .

[0012] The whiskers are SiC w 、Si3N 4w 、Al2O 3w One or both of the following.

[0013] The defoaming agent is one or two of TEGO 901W polyether siloxane defoaming agent, TEGO 8030 silicone water-based defoaming agent, and EFKA 2720 unsaturated polyester defoaming agent; the leveling agent is one or two of TEGO Glide450 silicone leveling agent, EFKA 3777 polyurethane leveling agent, and EFKA 3034 leveling agent; the wetting and dispersing agent is one or two of TEGO 755W, TEGO 662 C, and EFKA 5065.

[0014] The composite high-temperature adhesive is a composite adhesive obtained by uniformly mixing chromium aluminum phosphate, modified aluminum dihydrogen phosphate and silica sol in a mass ratio of 1: (0.6-0.8): (0.2-0.4).

[0015] The method for preparing the high-entropy cerate water-based coating for high-temperature radiation heat dissipation as described above comprises the following steps:

[0016] (1) Add high entropy cerate to the composite high temperature binder, stir mechanically for 10 to 15 minutes, and after stirring evenly, add boron nitride, zirconium oxide, cordierite, whisker, silicon carbide, silicon nitride, brown corundum, fumed silica, and kaolin in sequence, and stir mechanically for 30 to 60 minutes to obtain a mixture A;

[0017] (2) Add defoamer, leveling agent, wetting dispersant and organic bentonite to deionized water in sequence, and stir mechanically for 5 to 10 minutes; then add to mixture A, and stir mechanically for 30 to 60 minutes to obtain mixture B;

[0018] ⑶ Transfer the mixture B to a planetary ball mill, the ball milling medium is zirconia balls, the ball-to-material mass ratio is 2:1, the ball milling speed is 200-400 r / min, and the ball milling time is 2-4 hours to obtain a high-entropy cerate water-based coating.

[0019] A coating made of the above water-based paint, characterized in that: the coating has an infrared emissivity of >0.93 in the 1-20 μm band, has directional heat conduction and toughness, and the coating has a thermal conductivity of >60 W·(m·K) -1 .

[0020] The method for preparing the coating as described above comprises the following steps:

[0021] ①Surface treatment of substrate:

[0022] The surface of the substrate is sandblasted with quartz sand having a particle size of 60-100 meshes, so that the cleanliness of the substrate surface reaches the Sa 2.5 level requirement, thereby obtaining a treated substrate;

[0023] ② Fill the water-based paint into the spray gun and spray the water-based paint on the treated substrate surface by air spraying. The spraying environment temperature is 15-30°C, the relative air humidity is less than 85%, and the spraying pressure is 0.3-0.4MPa to obtain a wet film with a thickness of 120-180μm;

[0024] ③Cure the wet film at room temperature for 12 hours, and then cure it with furnace heating. The curing temperature is 500°C, the heating rate is 5°C / min, the curing time is 2~4 hours, and the cooling method is furnace cooling to obtain a dry film with a thickness of 60~90μm.

[0025] Compared with the prior art, the present invention has the following advantages:

[0026] 1. The present invention uses high-entropy cerate as the main functional filler. Since high-entropy cerate has a defective fluorite structure, more than five rare earth elements and transition metal elements can be randomly distributed at the A position. The disorder of the elements and the differences in radius and mass cause the crystal structure of the material to present severe lattice distortion and produce a large number of oxygen vacancies. At the same time, the arrangement characteristics of the 3d orbital of the transition metal element and the 4f orbital of the rare earth element form an intermediate band near the Fermi level, effectively reducing the intrinsic band gap of the high-entropy cerate material. In addition, the change in the valence of multivalent elements can produce small polarons and promote electronic transitions. Therefore, high-entropy cerate ceramics can significantly broaden the band of infrared emission and improve the infrared radiation performance of the material at 1~20μm by enhancing electronic transitions, free carrier absorption, impurity energy level absorption and lattice vibration absorption.

[0027] 2. The water-based coating prepared by ball milling mixing in the present invention has high infrared emissivity, directional thermal conductivity, strong toughness and a thermal expansion coefficient matching the substrate in the 1-20 μm band, and has potential application prospects in the field of radiation heat management such as large energy equipment, aircraft engines, gas turbines, electronic devices, and power station boilers.

[0028] 3. The high entropy cerate coating prepared by the present invention has directional thermal conductivity and strong toughness. Since the added boron nitride is hexagonal boron nitride with a layered crystal structure, its theoretical thermal conductivity along the a, b and c axes is 4.1 W·(m·K) respectively. -1 and 537 W·(m·K) -1 , with significant directional thermal conductivity. In addition, the filler particle size also affects the thermal conductivity of the coating system. The ultra-fine micro-processing of boron nitride particles (100~200 nm) is conducive to its dispersion in the material and the mutual contact and interaction between it and the filler. Figure 1 As shown, according to the ASTM E1461-13 (2022) "Standard Test Method for Thermal Diffusivity by the Flash Method" test standard, the thermal conductivity of the high entropy cerate coating is >60 W·(m·K) -1 .

[0029] 4. The high entropy cerate coating prepared by the present invention has strong toughness. Due to the addition of high modulus and high strength whiskers (SiC w 、Si3N 4w and Al2O 3w ) can be composited with the matrix to achieve the toughening of the coating material through the extraction and bridging of whiskers or fibers and the deflection and passivation of cracks.

[0030] 5. The high entropy cerate coating prepared by the present invention has excellent radiation heat dissipation capability. Figure 2As shown, according to the GB / T4653-1984 "Coating Infrared Emissivity" test standard, the normal infrared emissivity of the coating at 1~20μm is 0.938. The coating of the present invention combines high infrared emissivity with high thermal conductivity. Under a certain range of heat flux density, the higher the emissivity of the material, the stronger the surface radiation heat dissipation capacity, thereby reducing the energy damage to the base material and extending the service life of the hot end components.

[0031] 6. The high entropy cerate coating prepared by the present invention has excellent sulfate corrosion resistance. A saturated solution of Na2SO4 and K2SO4 with a mass ratio of 1:1 was prepared, and the saturated salt solution was brushed on the surface of the sample. After drying, the salt film was weighed to make the mass of the salt film 12-14 mg cm -2 , heated to 700℃ for corrosion test, one cycle is 24 hours. Figure 3 As shown, after 10 cycles of corrosion, the coating surface is smooth and dense, without blistering or cracking.

[0032] 7. The high entropy cerate coating prepared by the present invention has excellent high temperature resistance. Since the high entropy cerate exhibits the stability of the entropy-driven structure and the high temperature resistance of the composite binder modification, such as Figure 4 As shown, according to the test standard GB / T 1735-2009 "Determination of Heat Resistance of Paints and Varnishes", a high entropy cerate water-based coating was sprayed on an alumina crucible and placed in an air atmosphere of a box furnace. After a 168-hour thermal stability test at 1500°C, the coating surface was smooth and dense, without blistering or cracking.

[0033] 8. The high entropy cerate coating prepared by the present invention has good thermal shock resistance. Figure 5 As shown in the figure, according to the GB / T7320-2018 "Coating Thermal Expansion Coefficient" test standard, the linear expansion coefficient of high entropy cerate coating is (8.9~12.2)×10 -6 / ℃, which can match a variety of substrates, so it can effectively reduce the stress caused by thermal shock during thermal cycle tests. After 40 thermal shock tests at 1000℃ (air cooling), the coating surface is smooth, dense, without blistering, cracking, etc.

[0034] 9. The high-entropy cerate coating prepared by the present invention can be used as a protective energy-saving material in power station boilers. It has high infrared radiation performance, can effectively enhance the furnace radiation heat transfer capacity, and improve the boiler heat exchange efficiency. In addition, it has high directional heat conduction, excellent resistance to molten salt corrosion, high temperature resistance, thermal shock resistance and good thermal matching with the substrate, and has potential application value in coping with the complex operating conditions of coal-fired boilers. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0036] Figure 1 The thermal conductivity of the high entropy cerate coating for high temperature radiation heat dissipation prepared in Example 2 of the present invention.

[0037] Figure 2 This is the infrared emission spectrum of the high-entropy cerate coating for high-temperature radiation heat dissipation prepared in Example 2 of the present invention.

[0038] Figure 3 This is a surface appearance diagram of the high-entropy cerate coating for high-temperature radiation heat dissipation prepared in Example 3 of the present invention after being resistant to high-temperature molten salt corrosion.

[0039] Figure 4 This is an apparent image of the coating after the high-entropy cerate coating for high-temperature radiation heat dissipation prepared in Example 3 of the present invention has been subjected to a high-temperature resistance test.

[0040] Figure 5 This is a thermal expansion coefficient diagram of a high-entropy cerate coating for high-temperature radiation heat dissipation prepared in Example 4 of the present invention. DETAILED DESCRIPTION

[0041] A high-entropy cerate water-based paint for high-temperature radiation heat dissipation, the water-based paint is composed of the following raw materials in parts by weight (g): 10-20 parts of high-entropy cerate, 5-10 parts of boron nitride, 5-10 parts of zirconium oxide, 0-5 parts of cordierite, 3-5 parts of silicon carbide, 3-5 parts of silicon nitride, 5-10 parts of brown corundum, 3-5 parts of fumed silica, 2-5 parts of kaolin, 1-3 parts of whiskers, 1-3 parts of defoaming agent, 1-3 parts of leveling agent, 1-3 parts of wetting dispersant, 1-3 parts of organic bentonite, 20-30 parts of composite high-temperature binder, and 15-25 parts of deionized water.

[0042] The particle size of high entropy cerate is less than 1 μm, and it has excellent infrared radiation performance. Its chemical formula is A2Ce2O7, where the A position is at least five elements of La, Pr, Gd, Ca, Cu, Fe, Ni, and Co, and each element is in an equal molar ratio or a nearly equal molar ratio. The high entropy cerate is prepared by the following method: AO with a metal element molar ratio of 1:1 x Powder and CeO2 powder as raw materials, AO x La2O3, Pr6O 11 、Gd2O3、CaO、CuO、Fe2O 3、At least five of NiO and CoO powders. The raw materials are ball-milled and mixed in a planetary ball mill, the ball-milling medium is zirconium oxide balls, the ball-milling speed is 200-400 r / min, the ball-milling time is 12-24 hours, and the mass ratio (g / g) of ball material to water is 3:1:2. Then, the mixture powder is obtained by drying at 80-100°C for 12-24 hours and then grinding. The mixture powder is calcined at high temperature in an air atmosphere, the calcination temperature is 1200-1500°C, the heating rate is 3-5°C / min, and the calcination time is 6-8 hours. After the calcination, the high entropy cerate with a defective fluorite structure and a particle size of less than 1 μm is obtained by cooling, grinding, and sieving.

[0043] The particle size of zirconium oxide and brown corundum is 300~500nm; the particle size of boron nitride is 100~200nm; the particle size of silicon nitride is 500~800nm. Boron nitride is hexagonal boron nitride with a layered crystal structure. Its theoretical thermal conductivity along the a, b and c axes is 4.1 W·(m·K) respectively. -1 and 537 W·(m·K) -1 , with significant directional heat conduction characteristics.

[0044] Whiskers are SiC w 、Si3N 4w 、Al2O 3w One or both of the following.

[0045] The defoaming agent is one or two of TEGO 901W polyether siloxane defoaming agent, TEGO 8030 silicone water-based defoaming agent, and EFKA 2720 unsaturated polyester defoaming agent; the leveling agent is one or two of TEGO Glide 450 silicone leveling agent, EFKA 3777 polyurethane leveling agent, and EFKA 3034 leveling agent; the wetting and dispersing agent is one or two of TEGO 755W, TEGO 662 C, and EFKA 5065.

[0046] The composite high-temperature binder is a composite binder obtained by uniformly mixing chromium aluminum phosphate, modified aluminum dihydrogen phosphate, and silica sol in a mass ratio (g / g) of 1: (0.6-0.8): (0.2-0.4).

[0047] A method for preparing a high-entropy cerate water-based coating for high-temperature radiation heat dissipation comprises the following steps:

[0048] (1) Add high entropy cerate to the composite high temperature binder, stir mechanically for 10 to 15 minutes, and after stirring evenly, add boron nitride, zirconium oxide, cordierite, whisker, silicon carbide, silicon nitride, brown corundum, fumed silica, and kaolin in sequence, and stir mechanically for 30 to 60 minutes to obtain a mixture A;

[0049] (2) Add defoamer, leveling agent, wetting dispersant and organic bentonite to deionized water in sequence, and stir mechanically for 5 to 10 minutes; then add to mixture A, and stir mechanically for 30 to 60 minutes to obtain mixture B;

[0050] ⑶ Transfer the mixture B to a planetary ball mill, the ball milling medium is zirconia balls, the ball-to-material mass ratio (g / g) is 2:1, the ball milling speed is 200-400 r / min, and the ball milling time is 2-4 hours to obtain a high-entropy cerate water-based coating.

[0051] A coating made of the above water-based paint, the coating has an infrared emissivity of >0.93 in the 1-20 μm band, has directional heat conduction and strong toughness, and the thermal conductivity of the coating is >60 W·(m·K) -1 ; and has good thermal stability at 1500℃.

[0052] The method for preparing the coating comprises the following steps:

[0053] ①Surface treatment of substrate:

[0054] The surface of the substrate is sandblasted with quartz sand having a particle size of 60-100 meshes, so that the cleanliness of the substrate surface reaches the Sa 2.5 level requirement, thereby obtaining a treated substrate;

[0055] ② Fill the water-based paint into the spray gun and spray the water-based paint on the treated substrate surface by air spraying. The spraying environment temperature is 15-30°C, the relative air humidity is less than 85%, and the spraying pressure is 0.3-0.4MPa to obtain a wet film with a thickness of 120-180μm;

[0056] ③Cure the wet film at room temperature for 12 hours, and then cure it with furnace heating. The curing temperature is 500°C, the heating rate is 5°C / min, the curing time is 2~4 hours, and the cooling method is furnace cooling to obtain a dry film with a thickness of 60~90μm.

[0057] Example 1

[0058] A method for preparing a high-entropy cerate water-based coating for high-temperature radiation heat dissipation comprises the following steps:

[0059] ⑴ 10g high entropy cerate (La 0.2 Pr 0.2 G 0.2 Cu 0.2 Co 0.2 )2Ce2O7 was added to 30g of composite high-temperature binder (15g of aluminum chromium phosphate, 12g of modified aluminum dihydrogen phosphate, 3g of silica sol), mechanically stirred for 10 minutes, and after stirring evenly, 5g of boron nitride, 5g of zirconium oxide, and 1g of SiC were added in sequence. w, 5 g of silicon carbide, 5 g of silicon nitride, 5 g of brown corundum, 3 g of fumed silica, and 2 g of kaolin, and mechanically stirred for 30 minutes to obtain a mixture A;

[0060] (2) 1 g of defoamer (TEGO 901W), 2 g of leveling agent (TEGO Glide450), 3 g of wetting and dispersing agent (TEGO 755W), and 3 g of organic bentonite were sequentially added to 25 g of deionized water and mechanically stirred for 5 minutes; then added to mixture A and mechanically stirred for 30 minutes to obtain mixture B;

[0061] ⑶ Transfer the mixture B to a planetary ball mill, the ball milling medium is zirconia balls, the ball-to-material mass ratio (g / g) is 2:1, the ball milling speed is 300 r / min, and the ball milling time is 2 hours to obtain a high-entropy cerate water-based coating.

[0062] The method for preparing the coating comprises the following steps:

[0063] ①Surface treatment of substrate:

[0064] The surface of the substrate is sandblasted with quartz sand having a particle size of 60 meshes, so that the cleanliness of the substrate surface reaches the Sa2.5 level requirement, thereby obtaining a treated substrate;

[0065] ② Fill the water-based paint into the spray gun and spray the water-based paint on the treated substrate surface by air spraying. The spraying environment temperature is 15~30℃, the relative air humidity is less than 85%, and the spraying pressure is 0.3~0.4MPa to obtain a wet film;

[0066] ③ The wet film was cured at room temperature for 12 hours, and then cured with furnace heating. The curing temperature was 500°C, the heating rate was 5°C / min, the curing time was 2 hours, and the cooling method was furnace cooling to obtain a high entropy cerate coating dry film.

[0067] Example 2

[0068] A method for preparing a high-entropy cerate water-based coating for high-temperature radiation heat dissipation comprises the following steps:

[0069] ⑴ 10g high entropy cerate (La 0.2 Pr 0.2 G 0.2 Ni 0.2 Co 0.2 )2Ce2O7 was added to 24g of composite high temperature binder (12g of aluminum chromium phosphate, 7.2g of modified aluminum dihydrogen phosphate, 4.8g of silica sol), mechanically stirred for 15 minutes, and after stirring evenly, 10g of boron nitride, 10g of zirconium oxide, 3g of cordierite, 1g of whisker (0.5g of SiC w , 0.5g Si3N 4w), 3 g of silicon carbide, 3 g of silicon nitride, 7 g of brown corundum, 3 g of fumed silica, and 2 g of kaolin, and mechanically stirred for 45 minutes to obtain a mixture A;

[0070] (2) 1 g of defoamer (0.5 g of TEGO 8030, 0.5 g of EFKA 2720), 3 g of leveling agent (EFKA 3777), 2 g of wetting and dispersing agent (1 g of TEGO 755W, 1 g of TEGO 662 C), and 1 g of organic bentonite were sequentially added into 20 g of deionized water, and mechanically stirred for 10 minutes; then added into mixture A, and mechanically stirred for 60 minutes to obtain mixture B;

[0071] ⑶ Transfer the mixture B to a planetary ball mill, the ball milling medium is zirconia balls, the ball-to-material mass ratio (g / g) is 2:1, the ball milling speed is 200 r / min, and the ball milling time is 4 hours, thereby obtaining a high-entropy cerate water-based coating.

[0072] The method for preparing the coating comprises the following steps:

[0073] ①Surface treatment of substrate:

[0074] The surface of the substrate is sandblasted with quartz sand having a particle size of 80 meshes, so that the cleanliness of the substrate surface reaches the Sa2.5 level requirement, thereby obtaining a treated substrate;

[0075] ② Fill the water-based paint into the spray gun and spray the water-based paint on the treated substrate surface by air spraying. The spraying environment temperature is 15~30℃, the relative air humidity is less than 85%, and the spraying pressure is 0.3~0.4MPa to obtain a wet film;

[0076] ③ The wet film was cured at room temperature for 12 hours, and then cured with furnace heating. The curing temperature was 500°C, the heating rate was 5°C / min, the curing time was 4 hours, and the cooling method was furnace cooling to obtain a high entropy cerate coating dry film.

[0077] Example 3

[0078] A method for preparing a high-entropy cerate water-based coating for high-temperature radiation heat dissipation comprises the following steps:

[0079] ⑴ 17g high entropy cerate (La 0.2 Pr 0.16 G 0.16 Ca 0.16 Fe 0.16 Co 0.16)2Ce2O7 was added to 20g of composite high-temperature binder (10g of aluminum chromium phosphate, 7g of modified aluminum dihydrogen phosphate, and 3g of silica sol), and mechanically stirred for 13 minutes. After stirring evenly, 8g of boron nitride, 6g of zirconium oxide, 3g of cordierite, and 1g of Si3N were added in sequence. 4w , 4 g of silicon carbide, 4 g of silicon nitride, 10 g of brown corundum, 5 g of fumed silica, and 5 g of kaolin, and mechanically stirred for 30 minutes to obtain a mixture A;

[0080] (2) 2 g of defoamer (TEGO 901W, TEGO 8030), 2 g of leveling agent (EFKA 3777, EFKA 3034), 2 g of wetting and dispersing agent (TEGO 662 C, EFKA 5065), and 1 g of organic bentonite were sequentially added to 15 g of deionized water, and mechanically stirred for 5 minutes; then added to mixture A, and mechanically stirred for 45 minutes to obtain mixture B;

[0081] ⑶ Transfer the mixture B to a planetary ball mill, the ball milling medium is zirconia balls, the ball-to-material mass ratio (g / g) is 2:1, the ball milling speed is 400 r / min, and the ball milling time is 3 hours, thereby obtaining a high-entropy cerate water-based coating.

[0082] The method for preparing the coating comprises the following steps:

[0083] ①Surface treatment of substrate:

[0084] The surface of the substrate is sandblasted with quartz sand having a particle size of 60 meshes, so that the cleanliness of the substrate surface reaches the Sa2.5 level requirement, thereby obtaining a treated substrate;

[0085] ② Fill the water-based paint into the spray gun and spray the water-based paint on the treated substrate surface by air spraying. The spraying environment temperature is 15~30℃, the relative air humidity is less than 85%, and the spraying pressure is 0.3~0.4MPa to obtain a wet film;

[0086] ③ The wet film was cured at room temperature for 12 hours, and then cured with furnace heating. The curing temperature was 500°C, the heating rate was 5°C / min, the curing time was 3 hours, and the cooling method was furnace cooling to obtain a high entropy cerate coating dry film.

[0087] Example 4

[0088] A method for preparing a high-entropy cerate water-based coating for high-temperature radiation heat dissipation comprises the following steps:

[0089] ⑴ 20g high entropy cerate (La 0.16 Pr 0.14 G 0.14 Ca 0.14 Fe0.14 Ni 0.14 Co 0.14 )2Ce2O7 was added to 25g of composite high-temperature binder (12.5g of aluminum chromium phosphate, 10g of modified aluminum dihydrogen phosphate, and 2.5g of silica sol), and mechanically stirred for 15 minutes. After stirring evenly, 5g of boron nitride, 5g of zirconium oxide, 5g of cordierite, and 2g of Al2O 3w , 3 g of silicon carbide, 3 g of silicon nitride, 5 g of brown corundum, 4 g of fumed silica, and 3 g of kaolin, and mechanically stirred for 60 minutes to obtain a mixture A;

[0090] (2) 1 g of defoamer (TEGO 8030), 1 g of leveling agent (EFKA 3034), 1 g of wetting and dispersing agent (TEGO 662 C), and 2 g of organic bentonite were sequentially added to 20 g of deionized water and mechanically stirred for 8 minutes; then added to mixture A and mechanically stirred for 30 minutes to obtain mixture B;

[0091] ⑶ Transfer the mixture B to a planetary ball mill, the ball milling medium is zirconia balls, the ball-to-material mass ratio (g / g) is 2:1, the ball milling speed is 400 r / min, and the ball milling time is 2 hours, thereby obtaining a high-entropy cerate water-based coating.

[0092] The method for preparing the coating comprises the following steps:

[0093] ①Surface treatment of substrate:

[0094] The substrate surface is sandblasted with quartz sand having a particle size of 100 meshes, so that the cleanliness of the substrate surface reaches the Sa2.5 level requirement, thereby obtaining a treated substrate;

[0095] ② Fill the water-based paint into the spray gun and spray the water-based paint on the treated substrate surface by air spraying. The spraying environment temperature is 15~30℃, the relative air humidity is less than 85%, and the spraying pressure is 0.3~0.4MPa to obtain a wet film;

[0096] ③ The wet film was cured at room temperature for 12 hours, and then cured with furnace heating. The curing temperature was 500°C, the heating rate was 5°C / min, the curing time was 3 hours, and the cooling method was furnace cooling to obtain a high entropy cerate coating dry film.

[0097] The above is only an explanation of the best embodiment of the present invention, which should not be construed as a limitation on the claims. The present invention is not limited to the above embodiments. All changes made within the scope of protection of the independent claims of the present invention are within the scope of protection of the present invention.

Claims

1. A high-entropy cerate water-based coating for high-temperature radiation heat dissipation, characterized in that: The water-based coating is composed of the following raw materials in parts by weight: 10-20 parts of high-entropy cerate, 5-10 parts of boron nitride, 5-10 parts of zirconium oxide, 0-5 parts of cordierite, 3-5 parts of silicon carbide, 3-5 parts of silicon nitride, 5-10 parts of brown corundum, 3-5 parts of fumed silica, 2-5 parts of kaolin, 1-3 parts of whiskers, 1-3 parts of defoamers, 1-3 parts of leveling agents, 1-3 parts of wetting and dispersing agents, 1-3 parts of organic bentonite, 20-30 parts of composite high-temperature binders, and 15-25 parts of deionized water; the chemical formula of the high-entropy cerate is A2Ce2O7, wherein the A position is at least five elements of La, Pr, Gd, Ca, Cu, Fe, Ni, and Co, and the elements are in an equal molar ratio or a nearly equal molar ratio; the particle size of the high-entropy cerate is less than 1 μm; the particle sizes of the zirconium oxide and brown corundum are both 300-500nm; the particle size of the boron nitride is 100-200nm; the particle size of the silicon nitride is 500-800nm; the boron nitride is hexagonal boron nitride with a layered crystal structure; the whisker is SiC w 、Si3N 4w 、Al2O 3w One or both of the following.

2. A high-entropy cerate water-based paint for high-temperature radiation heat dissipation as claimed in claim 1, characterized in that: The defoaming agent is one or two of TEGO 901W polyether siloxane defoaming agent, TEGO 8030 silicone water-based defoaming agent, and EFKA 2720 unsaturated polyester defoaming agent; the leveling agent is one or two of TEGO Glide 450 silicone leveling agent, EFKA 3777 polyurethane leveling agent, and EFKA 3034 leveling agent; the wetting and dispersing agent is one or two of TEGO 755W, TEGO 662 C, and EFKA 5065.

3. A high-entropy cerate water-based paint for high-temperature radiation heat dissipation as claimed in claim 1, characterized in that: The composite high-temperature adhesive is a composite adhesive obtained by uniformly mixing chromium aluminum phosphate, modified aluminum dihydrogen phosphate and silica sol in a mass ratio of 1: (0.6-0.8): (0.2-0.4).

4. The method for preparing a high-entropy cerate water-based coating for high-temperature radiation heat dissipation according to claim 1 comprises the following steps: (1) Add high entropy cerate to the composite high temperature binder, stir mechanically for 10 to 15 minutes, and after stirring evenly, add boron nitride, zirconium oxide, cordierite, whisker, silicon carbide, silicon nitride, brown corundum, fumed silica, and kaolin in sequence, and stir mechanically for 30 to 60 minutes to obtain a mixture A; (2) Add defoamer, leveling agent, wetting dispersant and organic bentonite to deionized water in sequence, and stir mechanically for 5 to 10 minutes; then add to mixture A, and stir mechanically for 30 to 60 minutes to obtain mixture B; ⑶ Transfer the mixture B to a planetary ball mill, the ball milling medium is zirconia balls, the ball-to-material mass ratio is 2:1, the ball milling speed is 200-400 r / min, and the ball milling time is 2-4 hours to obtain a high-entropy cerate water-based coating.

5. A coating made of the water-based paint as claimed in claim 1, characterized in that: The infrared emissivity of the coating in the 1~20μm band is greater than 0.93, and it has directional heat conduction and strong toughness. The thermal conductivity of the coating is greater than 60 W·(m·K) -1 .

6. The method for preparing the coating according to claim 5, comprising the following steps: ①Surface treatment of substrate: The surface of the substrate is sandblasted with quartz sand having a particle size of 60-100 meshes, so that the cleanliness of the substrate surface reaches the Sa2.5 level requirement, thereby obtaining a treated substrate; ② Fill the water-based paint into the spray gun and spray the water-based paint on the treated substrate surface by air spraying. The spraying environment temperature is 15-30°C, the relative air humidity is less than 85%, and the spraying pressure is 0.3-0.4MPa to obtain a wet film with a thickness of 120-180μm; ③Cure the wet film at room temperature for 12 hours, and then cure it with furnace heating. The curing temperature is 500°C, the heating rate is 5°C / min, the curing time is 2~4 hours, and the cooling method is furnace cooling to obtain a dry film with a thickness of 60~90μm.